A spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging and its preparation method
By synergistically designing components such as hydroxyl-terminated boron-containing polysiloxane, the problem of decreased adhesion and optical performance degradation of spacecraft heat dissipation coatings under alternating humid and hot-vacuum environments was solved, achieving stability and efficient heat dissipation performance of the coating under alternating environments.
Patent Information
- Application Number
- CN202611436581.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-10
AI Technical Summary
Existing spacecraft heat dissipation coatings are prone to decreased adhesion, blistering, peeling, and optical performance degradation in humid and hot-vacuum alternating environments, making it difficult to meet the stable and reliable thermal control performance requirements of spacecraft throughout their entire lifecycle from ground launch to on-orbit service.
The coating employs a synergistic design of components such as hydroxyl-terminated boron-containing polysiloxane, perhydropolysilazane, modified silicon hexaboride powder, modified precipitated barium sulfate, yttrium oxide-stabilized zirconium oxide fiber, and fumed silica to form a dense cross-linked network and hydrophobic interface, thereby enhancing the coating's resistance to alternating humid heat and vacuum aging.
After undergoing alternating aging in a humid heat-vacuum environment, the coating still maintains high infrared emissivity, good adhesion, and a good appearance. It also has low vacuum outgassing and moisture absorption, meeting the thermal control performance requirements of spacecraft throughout their entire lifecycle.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of spacecraft thermal control coating technology, specifically to a spacecraft heat dissipation coating resistant to alternating aging of humidity and vacuum and its preparation method. Background Technology
[0002] During spacecraft operation, the electronic equipment and payloads inside generate a significant amount of waste heat. If this heat cannot be dissipated in a timely manner, it will directly affect the operational stability and lifespan of the equipment. Thermal control coatings, as one of the core methods of passive thermal control for spacecraft, are applied to the outer surface of the spacecraft. By adjusting the surface's absorption of solar radiation and its own emission of infrared thermal radiation, effective temperature control is achieved. Among these, heat-dissipating coatings are characterized by high infrared emissivity, enabling them to rapidly dissipate internal heat to the external space through thermal radiation, making them an indispensable material in the thermal control design of various spacecraft.
[0003] For a long time, research on spacecraft heat dissipation coatings has mainly focused on two directions. The first is organic systems, using silicone resins, polyurethanes, or fluorocarbon resins as film-forming materials, combined with functional pigments with high emissivity. These coatings have good application performance and excellent coating flexibility, but they suffer from significant outgassing problems in the vacuum environment of space. The released volatiles may condense on optical components and sensitive surfaces, causing contamination. The second is inorganic systems, using silicates or phosphates as binders. Although these systems have low vacuum outgassing and excellent radiation resistance, the coatings are generally brittle and prone to hygroscopic hydrolysis under humid and hot conditions, leading to decreased adhesion and deteriorated appearance.
[0004] In terms of environmental tolerance evaluation, existing research and standard testing methods mostly treat damp heat aging and vacuum aging as independent evaluation items. Damp heat testing is usually used to evaluate the stability of coatings during ground storage and transportation, while vacuum testing is used to evaluate their outgassing characteristics and structural stability during on-orbit service. However, the actual service process of spacecraft is not a static exposure to a single environment, but rather a dynamic transition from a damp heat environment on the ground to a vacuum environment in space. Especially for space stations, manned spacecraft, and recoverable spacecraft, their outer surface coatings may be exposed to the high temperature and high humidity launch site environment for a long time before launch, and then face the extreme conditions of high vacuum after entering orbit. When the spacecraft is docked in the transition section or airlock and undergoes depressurization and repressurization operations, the damp heat environment and vacuum environment experienced by the coating are often not a simple sequential relationship, but rather multiple alternating superpositions. During this alternating process, the moisture adsorbed by the coating under humid heat is rapidly desorbed in a vacuum environment, causing the coating volume to shrink. The expansion and contraction stress generated by repeated moisture absorption and dehydration accumulates continuously, which can easily induce the initiation and expansion of microcracks inside the coating, ultimately manifesting as adhesion degradation, blistering, peeling, and deterioration of optical properties.
[0005] Currently, numerous existing technologies have reported spacecraft coatings with resistance to damp heat or thermal control coatings with low-vacuum venting performance. However, these studies only address formulation design and performance optimization for single environmental factors. Systematic reports on failure mechanisms and targeted material design under the coupled environmental conditions of damp heat and vacuum are lacking, and standardized experimental evaluation methods are also absent. The performance evolution patterns of existing coating products under this alternating aging mode are unclear, making it difficult to meet the application requirements of new spacecraft for long-life and high-reliability thermal control coatings.
[0006] Therefore, there is an urgent need for a spacecraft heat dissipation coating that can withstand the alternating effects of humid heat and vacuum environments. After undergoing alternating aging cycles of humid heat and vacuum, it should still maintain a high infrared emissivity, good adhesion, and intact coating appearance, thereby ensuring the stable and reliable thermal control performance of the spacecraft before launch, during launch, and throughout its entire on-orbit service life. Summary of the Invention
[0007] This invention addresses the problems existing in the prior art by providing a spacecraft heat dissipation coating resistant to alternating humid heat and vacuum aging and its preparation method. It aims to solve the problems that existing spacecraft heat dissipation coatings are prone to decreased adhesion, blistering and peeling, and optical performance degradation under alternating humid heat and vacuum environments. This invention provides a heat dissipation coating that can maintain high infrared emissivity and good adhesion even after undergoing alternating humid heat and vacuum aging cycles, so as to meet the practical application requirements of stable and reliable thermal control coating performance throughout the entire life cycle of spacecraft from ground launch site storage, launch to on-orbit service.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is as follows: The first aspect of this invention provides a spacecraft heat dissipation coating resistant to alternating aging of damp heat and vacuum. The raw materials for its preparation include, by weight, 40-60 parts of hydroxyl-terminated boron-containing polysiloxane, 10-20 parts of perhydropolysilazane, 20-30 parts of modified silicon hexaboride powder, 10-20 parts of modified precipitated barium sulfate, 3-6 parts of yttrium oxide-stabilized zirconium oxide fiber, 1-3 parts of fumed silica, 2-5 parts of dimethyldimethoxysilane, 0.5-1.5 parts of tetraisopropyl titanate, and 20-40 parts of solvent.
[0009] Furthermore, the hydroxyl-terminated boron-containing polysiloxane is prepared by a method comprising the following steps: Dimethyldichlorosilane was mixed with phenylboronic acid, and concentrated sulfuric acid was added as a catalyst. The mixture was stirred and reacted under nitrogen protection. Then, deionized water was added to carry out hydrolysis. The mixture was allowed to stand and separated. The organic phase was washed with water until neutral, and the volatile components were removed by vacuum distillation to obtain boron-containing polysiloxane with terminal hydroxyl groups.
[0010] Furthermore, the molar ratio of dimethyldichlorosilane to phenylboronic acid is 1:(0.1 to 0.3).
[0011] Furthermore, the mass of the concentrated sulfuric acid is 0.5% to 2% of the mass of dimethyldichlorosilane.
[0012] Furthermore, the temperature of the stirring reaction is 60–100°C, and the time is 4–8 hours.
[0013] Furthermore, the modified silicon hexaboride powder is prepared by a method comprising the following steps: Silicon hexaboride powder was dispersed in anhydrous ethanol to prepare a suspension with a solid content of 10% to 20%. Deionized water was added and the pH was adjusted to 4 to 5 with acetic acid. Then, γ-glycidoxypropyltrimethoxysilane (KH-560) and perfluorodecyltrimethoxysilane were added and stirred to react. After the reaction was completed, the mixture was filtered, the filter cake was washed with anhydrous ethanol, dried and ground to obtain modified silicon hexaboride powder.
[0014] Furthermore, the amount of KH-560 added is 1% to 3% of the mass of silicon hexaboride powder, and the amount of perfluorodecyltrimethoxysilane added is 2% to 5% of the mass of silicon hexaboride powder.
[0015] Furthermore, the temperature of the stirring reaction is 50–80°C, and the time is 2–6 hours.
[0016] Furthermore, the modified precipitated barium sulfate can be commercially available precipitated barium sulfate powder coated with organosilane, or it can be prepared by organosilane surface coating treatment of precipitated barium sulfate using methods known in the art.
[0017] Furthermore, the yttrium oxide-stabilized zirconia fiber (YSZ) has a yttrium oxide molar fraction of 3% to 10%, a fiber diameter of 1 to 10 μm, and a fiber length of 50 to 500 μm.
[0018] Furthermore, the solvent is selected from one or more of xylene, butyl acetate, and butanone.
[0019] The most direct damage to coatings caused by alternating humid heat and vacuum environments lies in the fact that the coating first absorbs moisture and swells under humid heat conditions, and then shrinks due to moisture desorption upon entering a vacuum. This repeated expansion and contraction causes stress to accumulate within the coating, eventually leading to microcracks, blistering, and even peeling. This invention selects hydroxyl-terminated boron-containing polysiloxane as the main film-forming resin. Due to the introduction of boron, the density of the cured film is improved compared to ordinary polysiloxanes, resulting in significantly less water absorption. It also reduces volatile substances under vacuum conditions. Combined with all-hydrogen polysilazane, it forms a stronger overall film layer that is less prone to internal stress accumulation under alternating water absorption and expansion, and dehydration and contraction, thus reducing the likelihood of microcracks. Modified silicon hexaboride powder plays a major role in heat dissipation. After silane modification, the filler and resin are more firmly bonded, and the filler surface is hydrophobic, preventing moisture accumulation at the contact points between the filler and resin, reducing coating defects caused by interfacial delamination under alternating conditions. Modified precipitated barium sulfate is used to adjust the solar absorptivity of the coating. Combined with silicon hexaboride, it enables the coating to possess both low solar absorptivity and high infrared emissivity. Fumed silica primarily improves the coating's storage condition, preventing the sedimentation of dense powders and fibers, and also helps reduce moisture penetration into the coating. Yttrium oxide-stabilized zirconia fibers are mixed into the coating; when the coating is under alternating stress and about to crack, they can delay crack propagation, preventing rapid crack expansion and coating damage. Dimethyldimethoxysilane enhances the coating's adhesion to the metal substrate, reducing moisture intrusion at the coating-substrate interface and preventing film peeling and blistering. Tetraisopropyl titanate promotes the curing and crosslinking of the resin and perhydropolysilazane. The solvent is used to adjust the coating's application viscosity for easy film formation. After the components are combined, the coating maintains stable adhesion and is not prone to blistering or peeling under repeated environmental changes, including humid and hot storage on the ground and subsequent vacuum in-orbit operation. Its heat dissipation-related optical properties also remain at a good level.
[0020] The second aspect of this invention provides a method for preparing the above-mentioned spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging, comprising the following steps: (1) Add hydroxyl-terminated boron-containing polysiloxane to the mixing tank, add 30% to 50% of the formula amount of solvent, add dimethyl dimethoxysilane and fumed silica under stirring, and stir for 15 to 30 minutes; then add modified silicon hexaboride powder and modified precipitated barium sulfate, and continue stirring for 30 to 50 minutes; grind the resulting mixed slurry to a fineness ≤30μm, add yttrium oxide stabilized zirconium oxide fiber, stir for 15 to 20 minutes, and discharge to obtain component A; (2) Under nitrogen protection, add the remaining solvent into the container, add perhydropolysilazane, and stir until dissolved; then add tetraisopropyl titanate and stir for 10-15 minutes to obtain component B; (3) Mix component A and component B before construction and stir to obtain the final product.
[0021] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a spacecraft heat dissipation coating capable of withstanding alternating humid and hot environments and vacuum conditions through the synergistic design of film-forming resin, functional fillers, and toughening components. The boron-containing polysiloxane, due to the introduction of boron, results in a denser cross-linking network. When co-cured with perhydropolysilazane, the resulting cross-linked structure contains both the organic network of the boron-containing polysiloxane and inorganic components derived from perhydropolysilazane. This cross-linking method minimizes stress concentration during repeated moisture absorption and dehydration, resulting in superior structural stability compared to conventional single-component cross-linking systems. Silicon hexaboride, modified with composite silane, establishes a chemical bond with the resin while possessing hydrophobic properties, preventing moisture accumulation at the filler-resin interface and resolving the issue of conventional fillers easily detaching in alternating environments. The introduction of YSZ fibers effectively inhibits the propagation of microcracks, compensating for the coating's insufficient toughness. Simultaneously, the use of modified barium sulfate ensures that the coating, while maintaining high emissivity, does not excessively absorb sunlight, thus fully realizing its heat dissipation function. The above design enables the coating to maintain its integrity, stable adhesion, and no significant decrease in emissivity after undergoing alternating aging in a humid heat-vacuum environment. Furthermore, the vacuum outgassing and moisture absorption rates are both at low levels, which can meet the requirements for thermal control coatings used in spacecraft throughout their entire lifecycle, from storage at the ground launch site to on-orbit service. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise specified, the raw materials used in the embodiments are all commercially available products.
[0023] Example 1 This embodiment provides a spacecraft heat dissipation coating resistant to alternating aging of damp heat and vacuum. The raw materials for its preparation include, by weight, 50 parts of hydroxyl-terminated boron-containing polysiloxane, 15 parts of perhydropolysilazane, 25 parts of modified silicon hexaboride powder, 15 parts of modified precipitated barium sulfate, 4 parts of yttrium oxide-stabilized zirconium oxide fiber, 2 parts of fumed silica, 3 parts of dimethyldimethoxysilane, 1 part of tetraisopropyl titanate, and 30 parts of xylene.
[0024] In this embodiment, the hydroxyl-terminated boron-containing polysiloxane was prepared by the following method: dimethyldichlorosilane and phenylboronic acid were mixed in a molar ratio of 1:0.2, and concentrated sulfuric acid (1% by mass of dimethyldichlorosilane) was added as a catalyst. The mixture was stirred at 80°C for 6 hours under nitrogen protection. Then, deionized water was added to carry out a hydrolysis reaction. The mixture was allowed to stand and separated. The organic phase was washed with water until neutral, and the volatile components were removed by vacuum distillation to obtain the hydroxyl-terminated boron-containing polysiloxane.
[0025] In this embodiment, the modified silicon hexaboride powder was prepared by the following method: silicon hexaboride powder was dispersed in anhydrous ethanol to prepare a suspension with a solid content of 15%. Deionized water was added and the pH was adjusted to 4.5 with acetic acid. Then, KH-560 and perfluorodecyltrimethoxysilane were added. The amount of KH-560 added was 2% of the mass of silicon hexaboride powder, and the amount of perfluorodecyltrimethoxysilane added was 3% of the mass of silicon hexaboride powder. The mixture was stirred and reacted at 65°C for 4 hours. After the reaction was completed, the mixture was filtered, the filter cake was washed with anhydrous ethanol, dried, and ground to obtain the modified silicon hexaboride powder.
[0026] In this embodiment, the modified precipitated barium sulfate is a commercially available product (Yunfu Hongzhi New Materials Co., Ltd., model AB-600). The yttrium oxide stabilized zirconia fiber is a commercially available product (Forsmann Technology (Beijing) Co., Ltd.), wherein the yttrium oxide molar fraction is 8%, the fiber diameter is 6-10 μm, and the fiber length is 200 μm.
[0027] The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging in this embodiment is prepared by the following method: (1) Add hydroxyl-terminated boron-containing polysiloxane to the mixing tank, add 12 parts of xylene, add dimethyldimethoxysilane and fumed silica under stirring, and stir for 20 minutes; then add modified silicon hexaboride powder and modified precipitated barium sulfate, and continue stirring for 40 minutes; transfer the resulting mixed slurry to a three-roll mill and grind it 3 times until the fineness is ≤30μm; finally add yttrium oxide stabilized zirconium oxide fiber, stir for 18 minutes, and discharge to obtain component A.
[0028] (2) Under nitrogen protection, 18 parts of xylene were added to a container, and then perhydropolysilazane was added and stirred until dissolved; then tetraisopropyl titanate was added and stirred for 12 minutes to obtain component B; the relative humidity of the environment was controlled at ≤40% when preparing component B.
[0029] (3) Before construction, mix component A and component B and stir for 12 minutes to obtain the spacecraft heat dissipation coating that is resistant to damp heat-vacuum alternating aging.
[0030] Example 2 This embodiment provides a spacecraft heat dissipation coating resistant to alternating aging of damp heat and vacuum. The raw materials for its preparation include, by weight, 55 parts of hydroxyl-terminated boron-containing polysiloxane, 12 parts of perhydropolysilazane, 22 parts of modified silicon hexaboride powder, 18 parts of modified precipitated barium sulfate, 5 parts of yttrium oxide-stabilized zirconium oxide fiber, 2.5 parts of fumed silica, 2.5 parts of dimethyldimethoxysilane, 0.8 parts of tetraisopropyl titanate, and 35 parts of xylene.
[0031] In this embodiment, the hydroxyl-terminated boron-containing polysiloxane and the modified silicon hexaboride powder were prepared according to the method described in Example 1.
[0032] The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging in this embodiment is prepared by the following method: (1) Add hydroxyl-terminated boron-containing polysiloxane to the mixing tank, add 15 parts of xylene, add dimethyldimethoxysilane and fumed silica under stirring, and stir for 25 minutes; then add modified silicon hexaboride powder and modified precipitated barium sulfate, and continue stirring for 35 minutes; transfer the resulting mixed slurry to a three-roll mill and grind it twice until the fineness is ≤30μm; finally add yttrium oxide stabilized zirconia fiber, stir for 15 minutes, and discharge to obtain component A.
[0033] (2) Under nitrogen protection, 20 parts of xylene were added to a container, and then perhydropolysilazane was added and stirred until dissolved; then tetraisopropyl titanate was added and stirred for 10 minutes to obtain component B; the relative humidity of the environment was controlled at ≤35% when preparing component B.
[0034] (3) Before construction, mix component A and component B and stir for 10 minutes to obtain the spacecraft heat dissipation coating that is resistant to damp heat-vacuum alternating aging.
[0035] Example 3 This embodiment provides a spacecraft heat dissipation coating resistant to alternating aging of damp heat and vacuum. The raw materials for its preparation include, by weight, 45 parts of hydroxyl-terminated boron-containing polysiloxane, 18 parts of perhydropolysilazane, 28 parts of modified silicon hexaboride powder, 12 parts of modified precipitated barium sulfate, 3.5 parts of yttrium oxide-stabilized zirconium oxide fiber, 1.5 parts of fumed silica, 4.5 parts of dimethyldimethoxysilane, 1.2 parts of tetraisopropyl titanate, and 25 parts of xylene.
[0036] In this embodiment, the hydroxyl-terminated boron-containing polysiloxane and the modified silicon hexaboride powder were prepared according to the method described in Example 1.
[0037] The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging in this embodiment is prepared by the following method: (1) Add hydroxyl-terminated boron-containing polysiloxane to the mixing tank, add 11 parts of xylene, add dimethyldimethoxysilane and fumed silica under stirring, and stir for 15 minutes; then add modified silicon hexaboride powder and modified precipitated barium sulfate, and continue stirring for 45 minutes; transfer the resulting mixed slurry to a three-roll mill and grind it 4 times until the fineness is ≤30μm; finally add yttrium oxide stabilized zirconia fiber, stir for 20 minutes, and discharge to obtain component A.
[0038] (2) Under nitrogen protection, 14 parts of xylene were added to a container, and then perhydropolysilazane was added and stirred until dissolved; then tetraisopropyl titanate was added and stirred for 15 minutes to obtain component B; the relative humidity of the environment was controlled at ≤30% when preparing component B.
[0039] (3) Before construction, mix component A and component B and stir for 15 minutes to obtain the spacecraft heat dissipation coating that is resistant to damp heat-vacuum alternating aging.
[0040] Comparative Example 1 The difference between this comparative example and Example 1 is that the hydroxyl-terminated boron-containing polysiloxane is replaced with an equal amount of methylphenyl silicone resin; all other aspects are the same as in Example 1.
[0041] Comparative Example 2 The difference between this comparative example and Example 1 is that the hydroxyl-terminated boron-containing polysiloxane is replaced with an equal amount of polyborosilazane; all other aspects are the same as in Example 1.
[0042] Comparative Example 3 The difference between this comparative example and Example 1 is that the all-hydrogen polysilazane is replaced with an equal amount of hydrogen-containing silicone oil; all other aspects are the same as in Example 1.
[0043] Comparative Example 4 The difference between this comparative example and Example 1 is that the modified silicon hexaboride powder is replaced with an equal amount of KH-560 single-modified silicon hexaboride powder; all other aspects are the same as in Example 1.
[0044] KH-560-modified silicon hexaboride powder was prepared as follows: silicon hexaboride powder was dispersed in anhydrous ethanol to prepare a suspension with a solid content of 15%. Deionized water was added and the pH was adjusted to 4.5 with acetic acid. Then, KH-560 was added at a rate of 2% of the mass of silicon hexaboride powder. The mixture was stirred at 65°C for 4 hours. After the reaction was completed, the powder was filtered, washed, dried, and ground to obtain the final product.
[0045] Comparative Example 5 The difference between this comparative example and Example 1 is that the modified precipitated barium sulfate is replaced with an equal amount of rutile titanium dioxide; all other aspects are the same as in Example 1.
[0046] Comparative Example 6 The difference between this comparative example and Example 1 is that the yttrium oxide stabilized zirconium oxide fiber is replaced with an equal amount of alumina fiber (Al2O3 to SiO2 mass ratio of 72:28, fiber diameter of 9-12 μm, which is shortened to 200 μm before use), and all other aspects are the same as in Example 1.
[0047] Performance testing Test samples were prepared for the coatings obtained in Examples 1-3 and Comparative Examples 1-6.
[0048] Coating sample preparation: The coatings prepared in each example and comparative example were applied by air spraying to the surface of an LY12 aluminum alloy substrate (50mm × 50mm × 1mm) that had been sanded and cleaned with acetone. The dry film thickness of the coating was controlled to be approximately 50μm. After spraying, the coating was allowed to dry at room temperature for 60 minutes, followed by holding at 80℃ for 2 hours, 120℃ for 2 hours, and 150℃ for 1 hour, and then naturally cooled to room temperature to obtain the coating samples. Multiple sets of parallel samples were prepared. The emissivity test and solar absorptivity test before and after the damp heat-vacuum alternating aging test used the same set of samples, while the adhesion test and vacuum degassing performance test each used a separate set of samples.
[0049] Preparation of test samples for moisture absorption rate test: Using the same coating and the same spraying process, the coating was applied to a polytetrafluoroethylene (PTFE) plate. After curing according to the same curing regime described above, the coating was peeled off and cut into 20mm × 20mm sheet samples. Before testing, the peeled coating film was dried at 120℃ to constant weight, cooled, and weighed as the mass before moisture absorption. This sample was used for the moisture absorption rate test.
[0050] Test method: 1. Alternating damp heat-vacuum aging test The coating sample was placed in a humidity test chamber and kept at 60℃ and 95%RH for 48 hours. After removal, it was transferred to a vacuum test chamber within 5 minutes and kept at ≤1×10⁻⁶. -3 The sample was kept at 125°C and 125 Pa for 48 hours, which constituted one cycle. After the vacuum stage, dry nitrogen gas was introduced into the vacuum test chamber to repressurize it to atmospheric pressure. After the sample cooled naturally to room temperature, the next cycle of the damp heat stage was carried out, for a total of 10 cycles. After aging was completed, the sample was removed, and the appearance of the coating was visually observed. The presence of defects such as blistering, cracking, or peeling was recorded.
[0051] 2. Adhesion Cross-cut aging tests were conducted according to GB / T 9286. Tests were performed before the alternating damp heat-vacuum aging test (hereinafter referred to as "before aging") and after the alternating damp heat-vacuum aging test (hereinafter referred to as "after aging"). The rating criteria are as follows: Level 0: The cut edges are completely smooth, with no chips missing. Level 1: Minor coating peeling at the cutting intersections, affected area ≤ 5%. Level 2: Coating peeling occurs along cut edges or intersections, affecting 5%–15% of the area. Level 3: The coating peels off partially or entirely along the cut edge, affecting an area of 15%–35%. Level 4: Large sections of the coating peel off along the cut edge, affecting an area of 35%–65%. Level 5: Peeling area > 65% 3. Infrared emissivity According to GJB 2502.3-2006, the normal infrared emissivity of the coating in the 5–20 μm band was measured using an infrared radiometer. Measurements were taken once before aging and once after aging.
[0052] 4. Solar absorptivity According to GJB 2502.4-2006, the spectral reflectance of the coating in the 250–2500 nm wavelength range was measured using a spectrophotometer, and the solar absorptivity α was calculated. s Measure once before aging and once after aging.
[0053] 5. Vacuum venting performance Perform the procedure according to ASTM E595, placing the coated sample in a vacuum chamber at 125°C and ≤1×10⁻⁶. -3 Under Pa conditions, the total mass loss (TML) and condensable volatile matter (CVCM) were measured after 24 hours.
[0054] 6. Moisture absorption rate The moisture absorption test sample was placed at 60℃ and 95%RH for 48 hours, and then weighed after moisture absorption. Moisture absorption rate = (mass after moisture absorption) (mass before moisture absorption) / mass before moisture absorption × 100%.
[0055] The test results are shown in Table 1.
[0056] Table 1 Performance Test Results
[0057] As can be seen from Table 1, after 10 cycles of alternating wet heat and vacuum aging, the coatings in Examples 1 to 3 remained intact, the adhesion did not decrease, and the changes in infrared emissivity and solar absorptivity were very small. This indicates that the present invention effectively suppressed the accumulation of expansion and contraction stress during repeated moisture absorption and desiccation, and the film structure had good stability. At the same time, the vacuum degassing and moisture absorption rate were also at a low level.
[0058] In Comparative Example 1, after replacing boron-containing polysiloxane with ordinary methylphenyl silicone resin, severe blistering and peeling occurred after aging, adhesion decreased significantly, and moisture absorption increased significantly. This was because ordinary silicone resin does not contain boron, resulting in insufficient cross-linking network density, making it easy for moisture to penetrate under humid and hot conditions, and low molecular weight segments to escape more easily under vacuum. In Comparative Example 2, microcracks appeared after replacing hydroxyl-terminated boron-containing polysiloxane with polyborosilazane. This is because although polyborosilazane contains boron, its main chain structure is different from that of the present invention, resulting in poor compatibility with perhydropolysilazane and uneven distribution of internal stress after cross-linking. In Comparative Example 3, cracking and blistering occurred after replacing perhydropolysilazane with hydrogen-containing silicone oil. After cross-linking, hydrogen-containing silicone oil lacks inorganic rigid nodes to share expansion and contraction stress. In Comparative Example 4, silicon hexaboride was modified only with KH-560 without hydrophobic treatment with fluorosilane, resulting in blistering after aging. This is because the filler surface lacks hydrophobic segments, making it easy for moisture to accumulate at the interface. In Comparative Example 5, bubbling also occurred after titanium dioxide was used to replace modified barium sulfate. Titanium dioxide has a hydrophilic surface and photocatalytic activity, and its interfacial stability under alternating humid heat and vacuum conditions is not as good as that of modified barium sulfate. In Comparative Example 6, microcracks appeared after YSZ fibers were replaced with alumina fibers. Alumina fibers have a stronger hydrophilic surface, and the fiber-resin interfacial bonding strength decreased under humid heat conditions, weakening the toughening effect.
[0059] Finally, it should be noted that the above content is only used to illustrate the technical solution of the present invention, and is not intended to limit the scope of protection of the present invention. Simple modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention do not depart from the essence and scope of the technical solution of the present invention.
Claims
1. A spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging, characterized in that, The raw materials for its preparation include, by weight: 40-60 parts of hydroxyl-terminated boron-containing polysiloxane, 10-20 parts of perhydropolysilazane, 20-30 parts of modified silicon hexaboride powder, 10-20 parts of modified precipitated barium sulfate, 3-6 parts of yttrium oxide-stabilized zirconium oxide fiber, 1-3 parts of fumed silica, 2-5 parts of dimethyldimethoxysilane, 0.5-1.5 parts of tetraisopropyl titanate, and 20-40 parts of solvent.
2. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 1, characterized in that, The hydroxyl-terminated boron-containing polysiloxane is prepared by a method comprising the following steps: mixing dimethyldichlorosilane with phenylboronic acid, adding concentrated sulfuric acid as a catalyst, and stirring the reaction under nitrogen protection; then adding deionized water to carry out a hydrolysis reaction, allowing the mixture to stand and separate, washing the organic phase with water until neutral, and removing the volatile components by vacuum distillation to obtain the hydroxyl-terminated boron-containing polysiloxane.
3. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 2, characterized in that, The molar ratio of dimethyldichlorosilane to phenylboronic acid is 1: (0.1 to 0.3).
4. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 2, characterized in that, The mass of the concentrated sulfuric acid is 0.5% to 2% of the mass of dimethyldichlorosilane.
5. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 2, characterized in that, The stirring reaction is carried out at a temperature of 60–100°C for 4–8 hours.
6. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 1, characterized in that, The modified silicon hexaboride powder is prepared by a method comprising the following steps: dispersing silicon hexaboride powder in anhydrous ethanol to prepare a suspension with a solid content of 10% to 20%, adding deionized water and adjusting the pH to 4 to 5 with acetic acid, then adding KH-560 and perfluorodecyltrimethoxysilane, stirring and reacting, filtering after the reaction is completed, washing the filter cake with anhydrous ethanol, drying and grinding to obtain the modified silicon hexaboride powder.
7. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 6, characterized in that, The amount of KH-560 added is 1% to 3% of the mass of silicon hexaboride powder, and the amount of perfluorodecyltrimethoxysilane added is 2% to 5% of the mass of silicon hexaboride powder.
8. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 6, characterized in that, The stirring reaction is carried out at a temperature of 50–80°C for 2–6 hours.
9. The spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to claim 1, characterized in that, The yttrium oxide stabilized zirconia fiber has a yttrium oxide molar fraction of 3% to 10%, a fiber diameter of 1 to 10 μm, and a fiber length of 50 to 500 μm; the solvent is selected from one or more of xylene, butyl acetate, and methyl ethyl ketone.
10. The method for preparing a spacecraft heat dissipation coating resistant to alternating damp heat and vacuum aging according to any one of claims 1 to 9, characterized in that, Includes the following steps: (1) Add hydroxyl-terminated boron-containing polysiloxane to the mixing tank, add 30% to 50% of the formula amount of solvent, add dimethyl dimethoxysilane and fumed silica under stirring, and stir for 15 to 30 minutes; then add modified silicon hexaboride powder and modified precipitated barium sulfate, and continue stirring for 30 to 50 minutes; grind the resulting mixed slurry to a fineness ≤30μm, add yttrium oxide stabilized zirconium oxide fiber, stir for 15 to 20 minutes, and discharge to obtain component A; (2) Under nitrogen protection, add the remaining solvent into the container, add perhydropolysilazane, and stir until dissolved; then add tetraisopropyl titanate and stir for 10-15 minutes to obtain component B; (3) Mix component A and component B before construction and stir to obtain the final product.