A polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips and its preparation method.

By combining composite abrasives and copper corrosion inhibitors, the problems of copper removal rate, dish-shaped depression and dielectric layer removal relationship in the polishing of copper layers in silicon through-holes of silicon carbide chips were solved, achieving efficient copper layer planarization and surface quality control.

CN123063086APending Publication Date: 2026-11-10XINGHUA TSINGKE (TIANJIN) ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611312462.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing copper chemical mechanical polishing systems struggle to balance copper removal rate, dish-shaped depressions, surface roughness, and the relationship between copper layer and dielectric layer removal when polishing copper layers in silicon through-holes of silicon carbide chips.

Method used

A combination of composite abrasives, copper corrosion inhibitors, organic acid complexing agents, and pH adjusters, including fumed silica and silica sol, 2-mercaptobenzothiazole and 8-hydroxyquinoline, malonic acid, L-aspartic acid, and glycine, is used to adjust the pH of the polishing solution to 7.8–8.3, thereby creating a synergistic effect.

Benefits of technology

While maintaining copper removal efficiency, it reduces dish-shaped depressions and surface roughness, improves the removal relationship between the copper layer and the dielectric layer, and enhances the stability and planarization quality of the polishing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention provides a polishing slurry for chemical mechanical polishing of copper layers in through-silicon vias (TSVs) of silicon carbide (SiV) chips and its preparation method, belonging to the field of semiconductor wafer-level packaging and processing technology. The polishing slurry comprises a composite abrasive, a copper corrosion inhibitor, an organic acid complexing agent, an oxidant, a surfactant, a pH adjuster, and deionized water. The composite abrasive is composed of fumed silica and silica sol, the copper corrosion inhibitor is composed of 2-mercaptobenzothiazole and 8-hydroxyquinoline, and the organic acid complexing agent is composed of malonic acid, L-aspartic acid, and glycine. The pH of the polishing slurry is 7.8–8.3. The preparation method includes premix preparation, copper corrosion inhibitor dispersion, abrasive suspension preparation, compounding and blending, and filtration. This invention can reduce the dish-shaped depressions and surface roughness of the TSV copper layer while maintaining copper layer removal efficiency, and coordinate the removal processes of the copper layer and the dielectric layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor wafer-level packaging and processing technology, and in particular to a polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips and its preparation method. Background Technology

[0002] Silicon carbide (SiC) materials possess a large bandgap, high thermal conductivity, and strong breakdown field, making them widely used in power semiconductor devices. With increasing device integration, through-silicon via (TSV) technology is being used to achieve vertical interconnects and 3D integration of chips. In TSV structures, the chemical mechanical polishing (CMP) quality of the copper layer directly affects the planarization of the copper layer and the stability of subsequent processes.

[0003] In silicon through-silicon via (TSV) structures for silicon carbide (SiC) chips, the difference in thermal expansion coefficients between the SiC substrate and the copper layer can easily lead to interfacial stress during subsequent thermal cycling. Therefore, chemical mechanical polishing (CMP) of the copper layer not only requires appropriate copper removal efficiency but also necessitates control over-polishing and the resulting surface and interfacial damage.

[0004] Furthermore, the hardness of silicon carbide differs from that of conventional silicon-based materials. Existing chemical mechanical polishing (CMP) systems, primarily designed for silicon-based copper interconnect layers, are prone to mismatch between mechanical abrasion and chemical reaction when directly applied to the copper layers of through-silicon vias (TSVs) in silicon carbide chips. Excessive mechanical removal can lead to large dish-shaped depressions in the copper layer of the TSV region, increasing surface roughness. Conversely, excessive copper corrosion inhibition can suppress dynamic copper removal, reducing polishing efficiency. Simultaneously, the removal relationship between the copper layer and the SiCN or SiCO dielectric layer must be considered in TSV structures to minimize excessive dielectric layer loss.

[0005] In existing copper chemical mechanical polishing slurries, the abrasive system typically uses a single silica sol or other silica abrasives; copper corrosion inhibitors usually use benzotriazole and its derivatives; and complexing agents are mostly single amino acids, organic acids, or other complexing components. When these systems are applied to the chemical mechanical polishing of copper layers in silicon carbide chip through-holes, it is difficult to simultaneously coordinate the mechanical removal of copper layers, surface corrosion inhibition, and copper ion complexation processes. Under certain process conditions, problems easily arise regarding the copper removal rate, dish-shaped depressions, surface roughness, and the relationship between copper layer and dielectric layer removal, which are difficult to balance.

[0006] To this end, a polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips and its preparation method are proposed. Summary of the Invention

[0007] The purpose of this invention is to provide a polishing slurry and its preparation method for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips, in order to solve the problems that existing copper chemical mechanical polishing systems are difficult to balance when applied to copper layers in silicon through-holes of silicon carbide chips, such as copper removal rate, dish-shaped depression, surface roughness, and the relationship between copper layer and dielectric layer removal.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: A polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips comprises the following components by mass percentage: 12-18% composite abrasive, 0.05-0.4% copper corrosion inhibitor, 0.2-1.5% organic acid complexing agent, 0.5-2.5% oxidant, 0.005-0.08% surfactant, 0.01-0.3% pH adjuster, and the balance being deionized water.

[0009] The composite abrasive is composed of fumed silica and silica sol, with a mass ratio of fumed silica to silica sol of 1:0.3 to 1:0.8.

[0010] The copper corrosion inhibitor is composed of 2-mercaptobenzothiazole and 8-hydroxyquinoline, with a mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline of 1:3 to 1:5.

[0011] The organic acid complexing agent is composed of malonic acid, L-aspartic acid and glycine, with a mass ratio of malonic acid, L-aspartic acid and glycine of 1:1 to 3:0.3 to 0.8.

[0012] The pH adjuster is one or both of tetramethylammonium hydroxide and monoethanolamine, and the pH of the polishing solution is 7.8 to 8.3.

[0013] Furthermore, the particle size of fumed silica is 120–180 nm, and the specific surface area is 220–280 m². 2 / g.

[0014] Furthermore, the particle size of the silica sol is 30–60 nm, and the absolute value of the particle size distribution deviation does not exceed 4%.

[0015] Furthermore, the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:4.

[0016] Furthermore, the mass ratio of malonic acid, L-aspartic acid, and glycine is 1:2:0.5.

[0017] Furthermore, the oxidant is one or both of urea peroxide and potassium persulfate.

[0018] Furthermore, the surfactant is composed of fluorocarbon surfactant and polyether-modified siloxane, with a mass ratio of fluorocarbon surfactant to polyether-modified siloxane of 1:5 to 1:10.

[0019] This invention also provides a method for preparing a polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips, comprising the following steps: S1. Add one or both of tetramethylammonium hydroxide and monoethanolamine to deionized water as pH adjusters to adjust the pH to 7.5-8.3. Then add malonic acid, L-aspartic acid and glycine, and stir until dissolved to obtain a premixed solution. S2. Dissolve 2-mercaptobenzothiazole and 8-hydroxyquinoline in ethanol, disperse them by ultrasonication, and then add them to the premixed solution obtained in step S1. The amount of ethanol used is 0.5-2% of the total mass of the polishing solution. Ethanol is used as a co-solvent and is not included in the total mass of the polishing solution formulation. S3. Fumed silica and silica sol are mixed in a high-speed shear disperser at a speed of 3000-5000 rpm for 20 min to obtain an abrasive suspension. S4. Add the abrasive suspension obtained in step S3 to the system obtained in step S2, then add surfactant and oxidant, and add deionized water to make up the volume. S5. The mixture obtained in step S4 is filtered sequentially through polyethersulfone filter cartridges with pore sizes of 1.2 μm and 0.45 μm to obtain a polishing solution with a pH of 7.8 to 8.3.

[0020] Furthermore, in step S2, the ultrasonic dispersion frequency is 40 kHz and the time is 15 min.

[0021] Furthermore, in step S4, the stirring speed is 200–250 r / min, and the ambient temperature is 18–22 ℃.

[0022] Compared with the prior art, the present invention has the following beneficial effects: I. This invention uses fumed silica and silica sol to form a composite abrasive, so that the mechanical grinding action of fumed silica and the surface finishing action of silica sol complement each other, thereby reducing the dish-shaped depressions and surface roughness of the TSV copper layer while maintaining the copper layer removal efficiency.

[0023] II. This invention uses 2-mercaptobenzothiazole and 8-hydroxyquinoline to form a copper corrosion inhibitor. By combining the two, the corrosion inhibition and dynamic removal process of the copper surface is regulated. While controlling the dish-shaped depression and surface roughness of the TSV copper layer, the copper corrosion inhibition effect is not too strong, which would cause a significant decrease in the copper removal rate.

[0024] Third, the present invention uses malonic acid, L-aspartic acid and glycine to form an organic acid complexing agent, which is beneficial to complexing copper ions generated during the polishing process, reducing the impact of copper ion redeposition on the copper layer surface, thereby improving the copper layer removal process and surface planarization quality.

[0025] Fourth, this invention uses tetramethylammonium hydroxide or monoethanolamine as a pH adjuster and controls the final pH of the polishing solution to 7.8-8.3, so that the effects of composite abrasive, copper corrosion inhibitor, organic acid complexing agent and oxidant are coordinated and the problem of imbalance in the removal relationship between copper layer and dielectric layer is improved. Detailed Implementation

[0026] This invention provides a polishing slurry for chemical mechanical polishing of the copper layer in silicon through-holes of silicon carbide chips. The polishing slurry includes composite abrasive, copper corrosion inhibitor, organic acid complexing agent, oxidant, surfactant, pH adjuster and deionized water.

[0027] The composite abrasive consists of fumed silica and silica sol. Fumed silica provides the mechanical abrasive action during the chemical mechanical polishing (CMP) process of the copper layer, while silica sol works in conjunction with fumed silica to finish the copper surface. By controlling the ratio of fumed silica to silica sol, the copper layer removal process and the surface planarization process are coordinated.

[0028] The copper corrosion inhibitor is composed of 2-mercaptobenzothiazole and 8-hydroxyquinoline. 2-mercaptobenzothiazole can interact with the copper surface to form a protective layer; 8-hydroxyquinoline participates in the regulation of chemical reactions on the copper surface through adsorption and complexation. The two work together to control localized corrosion and excessive removal of the copper layer.

[0029] The organic acid complexing agent is composed of malonic acid, L-aspartic acid, and glycine. Malonic acid, L-aspartic acid, and glycine can all participate in the complexation of copper ions. Through the cooperation of the three, the copper ions generated during the polishing process are promoted to enter the liquid phase, thereby reducing the redeposition of copper ions on the polished surface.

[0030] Oxidizing agents are used to participate in the oxidation process of copper surfaces; surfactants are used to help disperse the various components in the polishing solution; and tetramethylammonium hydroxide or monoethanolamine is used as a pH adjuster to adjust the pH of the polishing solution.

[0031] In this embodiment of the invention, the composite abrasive has a mass percentage of 12-18%, the copper corrosion inhibitor has a mass percentage of 0.05-0.4%, the organic acid complexing agent has a mass percentage of 0.2-1.5%, the oxidant has a mass percentage of 0.5-2.5%, the surfactant has a mass percentage of 0.005-0.08%, the pH adjuster has a mass percentage of 0.01-0.3%, and the balance is deionized water.

[0032] In the composite abrasive, the mass ratio of fumed silica to silica sol is 1:0.3 to 1:0.8; in the copper corrosion inhibitor, the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:3 to 1:5; and in the organic acid complexing agent, the mass ratio of malonic acid, L-aspartic acid, and glycine is 1:1 to 3:0.3 to 0.8. The final pH of the resulting polishing solution is 7.8 to 8.3.

[0033] The fumed silica used in this embodiment of the invention has a particle size of 150 nm and a specific surface area of ​​250 m². 2 / g; the particle size of the silica sol is 40 nm. The surfactant consists of a fluorocarbon surfactant and a polyether-modified siloxane in a mass ratio of 1:8; the oxidant is urea peroxide.

[0034] The polishing slurries in Examples 1-5 were prepared according to the following steps.

[0035] S1. Preparation of premixed solution: Take 60% of the total amount of deionized water required, add tetramethylammonium hydroxide or monoethanolamine as pH adjuster as specified in the corresponding embodiment; then add malonic acid, L-aspartic acid and glycine according to the ratio of the corresponding embodiment, stir until dissolved, and obtain premixed solution.

[0036] S2. Copper corrosion inhibitor dispersion: Weigh 2-mercaptobenzothiazole and 8-hydroxyquinoline according to the proportions of the corresponding examples, dissolve them in ethanol, and use ethanol at 1.0% of the total mass of the polishing solution as a co-solvent, which is not included in the total mass of the polishing solution formulation; ultrasonically disperse the resulting system at 40 kHz for 15 min, and then add it to the premixed solution obtained in step S1.

[0037] S3. Preparation of abrasive suspension: Weigh fumed silica and silica sol according to the total amount of composite abrasive and the mass ratio of fumed silica to silica sol in the corresponding embodiment. Place the two in a high-speed shear disperser and mix at 4000 rpm for 20 min to obtain abrasive suspension.

[0038] S4. Compounding and blending: Add the abrasive suspension obtained in step S3 to the system obtained in step S2, and then add a surfactant composed of fluorocarbon surfactant and polyether modified siloxane and urea peroxide according to the formula of the corresponding embodiment. Compounding and blending are carried out at 225 r / min and 20 ℃, and the remaining deionized water is added to make the total mass of all formula components except ethanol 100%.

[0039] S5. Filtration: The mixture obtained in step S4 is filtered sequentially through polyethersulfone filter elements with pore sizes of 1.2 μm and 0.45 μm to obtain a polishing slurry for chemical mechanical polishing of the copper layer in the silicon through-hole of a silicon carbide chip.

[0040] Example 1 The polishing fluid in this embodiment includes 15% composite abrasive, 0.10% copper corrosion inhibitor, 0.8% organic acid complexing agent, 1.2% urea peroxide, 0.030% surfactant, 0.08% tetramethylammonium hydroxide, and the balance deionized water.

[0041] The composite abrasive consists of fumed silica and silica sol, with a mass ratio of fumed silica to silica sol of 1:0.5; the copper corrosion inhibitor consists of 2-mercaptobenzothiazole and 8-hydroxyquinoline, with a mass ratio of 1:3; the organic acid complexing agent consists of malonic acid, L-aspartic acid and glycine, with a mass ratio of 1:2:0.5; and the surfactant has a mass ratio of fluorocarbon surfactant to polyether-modified siloxane of 1:8.

[0042] The polishing solution was prepared according to the above method, wherein the amount of ethanol used was 1.0% of the total mass of the polishing solution, the high-speed shearing speed was 4000 rpm, the stirring speed for compounding was 225 r / min, and the ambient temperature was 20 ℃. The final pH of the resulting polishing solution was 8.0.

[0043] Example 2 The polishing fluid in this embodiment includes 18% composite abrasive, 0.20% copper corrosion inhibitor, 1.0% organic acid complexing agent, 1.4% urea peroxide, 0.040% surfactant, 0.10% tetramethylammonium hydroxide, and the balance deionized water.

[0044] The mass ratio of fumed silica to silica sol is 1:0.3; the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:4; the mass ratio of malonic acid, L-aspartic acid and glycine is 1:3:0.5; and the mass ratio of fluorocarbon surfactant to polyether-modified siloxane is 1:8.

[0045] The polishing solution was prepared according to the above method, with ethanol accounting for 1.0% of the total mass of the polishing solution, a high-speed shearing speed of 4000 rpm, a stirring speed of 225 r / min for compounding, and an ambient temperature of 20 ℃. The final pH of the resulting polishing solution was 7.9.

[0046] Example 3 The polishing fluid in this embodiment includes 12% composite abrasive, 0.05% copper corrosion inhibitor, 0.4% organic acid complexing agent, 1.0% urea peroxide, 0.020% surfactant, 0.06% tetramethylammonium hydroxide, and the balance deionized water.

[0047] The mass ratio of fumed silica to silica sol is 1:0.8; the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:5; the mass ratio of malonic acid, L-aspartic acid and glycine is 1:1:0.3; and the mass ratio of fluorocarbon surfactant to polyether-modified siloxane is 1:8.

[0048] The polishing solution was prepared according to the above method, with ethanol accounting for 1.0% of the total mass of the polishing solution, a high-speed shearing speed of 4000 rpm, a stirring speed of 225 r / min for compounding, and an ambient temperature of 20 ℃. The final pH of the resulting polishing solution was 8.2.

[0049] Example 4 The polishing fluid in this embodiment includes 14% composite abrasive, 0.15% copper corrosion inhibitor, 1.2% organic acid complexing agent, 1.3% urea peroxide, 0.035% surfactant, 0.12% monoethanolamine, and the balance deionized water.

[0050] The mass ratio of fumed silica to silica sol is 1:0.6; the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:4; the mass ratio of malonic acid, L-aspartic acid and glycine is 1:2.5:0.6; and the mass ratio of fluorocarbon surfactant to polyether-modified siloxane is 1:8.

[0051] Prepared according to the above method, this embodiment uses monoethanolamine as a pH adjuster, with ethanol accounting for 1.0% of the total mass of the polishing solution. The high-speed shearing speed is 4000 rpm, the stirring speed for compounding is 225 r / min, and the ambient temperature is 20 ℃. The final pH of the resulting polishing solution is 8.1.

[0052] Example 5 The polishing fluid in this embodiment includes 16% composite abrasive, 0.30% copper corrosion inhibitor, 0.6% organic acid complexing agent, 1.5% urea peroxide, 0.038% surfactant, 0.09% tetramethylammonium hydroxide, and the balance deionized water.

[0053] The mass ratio of fumed silica to silica sol is 1:0.4; the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:4; the mass ratio of malonic acid, L-aspartic acid and glycine is 1:2:0.4; and the mass ratio of fluorocarbon surfactant to polyether-modified siloxane is 1:8.

[0054] The polishing solution was prepared according to the above method, with ethanol accounting for 1.0% of the total mass of the polishing solution, a high-speed shearing speed of 4000 rpm, a stirring speed of 225 r / min for compounding, and an ambient temperature of 20 ℃. The final pH of the resulting polishing solution was 7.8.

[0055] Comparative Example 1 This comparative example is used to investigate the effect of composite abrasive composition on polishing performance.

[0056] The abrasive was prepared according to the formulation and specific preparation conditions of Example 1, with the only difference being that only fumed silica was used as the abrasive, without the addition of silica sol, and the content of fumed silica was 15%.

[0057] The copper corrosion inhibitor content is 0.10%, of which the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:3; the organic acid complexing agent content is 0.8%, of which the mass ratio of malonic acid, L-aspartic acid and glycine is 1:2:0.5; the urea peroxide content is 1.2%; the surfactant content is 0.030%, of which the mass ratio of fluorocarbon surfactant to polyether-modified siloxane is 1:8; the tetramethylammonium hydroxide content is 0.08%; the ethanol content is 1.0% of the total mass of the polishing solution, and the remainder is deionized water.

[0058] During the preparation process, the high-speed shearing speed was 4000 rpm, the stirring speed for compounding was 225 r / min, the ambient temperature was 20 ℃, and the remaining operations were the same as in Example 1. The final pH of the resulting polishing solution was 8.0.

[0059] Comparative Example 2 This comparative example is used to investigate the effect of the composition of copper corrosion inhibitor on polishing performance.

[0060] The preparation was carried out according to the formulation and specific preparation conditions of Example 1, with the only difference being that benzotriazole was used as a copper corrosion inhibitor at a content of 0.4%, and 2-mercaptobenzothiazole and 8-hydroxyquinoline were not added.

[0061] The composite abrasive content is 15%, the mass ratio of fumed silica to silica sol is 1:0.5; the organic acid complexing agent content is 0.8%, the mass ratio of malonic acid, L-aspartic acid and glycine is 1:2:0.5; the urea peroxide content is 1.2%; the surfactant content is 0.030%, the mass ratio of fluorocarbon surfactant to polyether modified siloxane is 1:8; the tetramethylammonium hydroxide content is 0.08%; the amount of ethanol is 1.0% of the total mass of the polishing solution, and the balance is deionized water.

[0062] During the preparation process, the high-speed shearing speed was 4000 rpm, the stirring speed for compounding was 225 r / min, the ambient temperature was 20 ℃, and the remaining operations were the same as in Example 1. The final pH of the resulting polishing solution was 8.0.

[0063] Comparative Example 3 This comparative example is used to investigate the effect of the composition of the organic acid complexing agent on polishing performance.

[0064] The preparation was carried out according to the formulation and specific preparation conditions of Example 1, except that citric acid was used as a complexing agent, and malonic acid, L-aspartic acid and glycine were not added, and the content of citric acid was 1.2%.

[0065] The composite abrasive content is 15%, the mass ratio of fumed silica to silica sol is 1:0.5; the copper corrosion inhibitor content is 0.10%, the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:3; the urea peroxide content is 1.2%; the surfactant content is 0.030%, the mass ratio of fluorocarbon surfactant to polyether modified siloxane is 1:8; the tetramethylammonium hydroxide content is 0.08%; the amount of ethanol is 1.0% of the total mass of the polishing fluid, and the balance is deionized water.

[0066] During the preparation process, the high-speed shearing speed was 4000 rpm, the stirring speed for compounding was 225 r / min, the ambient temperature was 20 ℃, and the remaining operations were the same as in Example 1. The final pH of the resulting polishing solution was 8.0.

[0067] Comparative Example 4 This comparative example is used to investigate the effect of the final pH of the polishing slurry on the polishing performance.

[0068] The preparation was carried out according to the basic formula and specific preparation conditions of Example 1, with the only difference being that the content of tetramethylammonium hydroxide was adjusted to 0.15%, so that the final pH after mixing all components was 10.0.

[0069] The composition includes: 15% composite abrasive; a mass ratio of fumed silica to silica sol of 1:0.5; 0.10% copper corrosion inhibitor; a mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline of 1:3; 0.8% organic acid complexing agent; a mass ratio of malonic acid, L-aspartic acid, and glycine of 1:2:0.5; 1.2% urea peroxide; 0.030% surfactant; a mass ratio of fluorocarbon surfactant to polyether-modified siloxane of 1:8; 1.0% ethanol by mass of the polishing solution; and the remainder being deionized water.

[0070] During the preparation process, the high-speed shearing speed was 4000 rpm, the stirring speed for compounding was 225 r / min, the ambient temperature was 20 ℃, and the remaining operations were the same as in Example 1. The final pH of the resulting polishing solution was 10.0.

[0071] Test case To evaluate the performance of the polishing slurries prepared in Examples 1-5 and Comparative Examples 1-4 in chemical mechanical polishing of the copper layer in silicon through-holes of silicon carbide chips, the copper removal rate, dish-shaped depression, surface roughness, and the selectivity ratio of Cu to dielectric layer removal rates were tested under the same polishing conditions.

[0072] 1. Testing equipment and samples Chemical mechanical polishing tests were conducted using a Universal-300 series polishing machine, with IC1010 polishing pads used as the polishing pads.

[0073] The test wafer is a 6-inch 4H-SiC wafer with a 1 μm thick Cu layer and a 50 nm thick TaN barrier layer deposited on its surface, and has a TSV array with an aspect ratio of 1:1.

[0074] Examples 1-3 and Comparative Examples 1-4 used SiCN dielectric layers for removal rate selectivity tests, while Examples 4 and 5 used SiCO dielectric layers for corresponding tests.

[0075] 2. Polishing process conditions All embodiments and comparative examples used the same polishing conditions: polishing pressure of 2.0 psi, turntable speed of 90 rpm, star disk speed of 100 rpm, polishing fluid flow rate of 250 mL / min, and polishing time of 60 s.

[0076] 3. Copper removal rate The copper layer thickness was measured using a four-point probe method. Nine measurement points were selected at the wafer center, half the wafer radius, and the wafer edge. The copper layer thickness before and after polishing was measured at the corresponding locations. The copper removal rate was calculated based on the change in copper layer thickness, and the average value of the results from each measurement point was taken as the copper removal rate test result.

[0077] 4. Disc-shaped depression The TSV structure region was scanned using an atomic force microscope with a scanning range of 20 μm × 20 μm. Five TSV units were selected from the central and edge regions of each wafer for testing, and the maximum depression depth was used as the result of the dish-shaped depression test.

[0078] 5. Surface roughness Atomic force microscopy was used to inspect the flat area of ​​the copper layer away from the TSV opening, with a scanning range of 5 μm × 5 μm. Three locations were selected for measurement on each wafer, and the average Ra value at the three locations was used as the surface roughness test result of the copper layer.

[0079] 6. Selectivity ratio of Cu to dielectric layer removal rate The thickness change of the SiCN or SiCO dielectric layer before and after polishing was measured using a profilometer. The dielectric layer removal rate was calculated based on the change in dielectric layer thickness. The ratio of the copper removal rate to the corresponding dielectric layer removal rate was used as the Cu: dielectric layer removal rate selection ratio.

[0080] The test results of Examples 1-5 and Comparative Examples 1-4 are shown in Table 1.

[0081] Table 1 Performance test results of the examples and comparative examples

[0082] Test Result Analysis: The test results of Example 1 and Comparative Example 1 show that when only fumed silica is used as the abrasive, although the copper removal rate is increased, the dish-shaped depression and surface roughness are significantly increased. When a composite abrasive composed of fumed silica and silica sol is used, the flatness and surface quality of the TSV copper layer can be improved while maintaining the copper removal efficiency, indicating that the two abrasives have a good synergistic dressing effect.

[0083] The test results of Example 1 and Comparative Example 2 show that when benzotriazole is used as a copper corrosion inhibitor, the copper removal rate is significantly reduced. When a copper corrosion inhibitor composed of 2-mercaptobenzothiazole and 8-hydroxyquinoline is used, a high copper removal rate can be maintained while controlling the dish-shaped depression and surface roughness, which is beneficial to coordinating the inhibitory effect on the copper surface and the dynamic removal process.

[0084] The test results of Example 1 and Comparative Example 3 show that when citric acid was used to replace the organic acid complexing agent composed of malonic acid, L-aspartic acid and glycine, the copper removal rate decreased, and the dish-shaped depression and surface roughness increased. This indicates that the organic acid complexing agent composed of malonic acid, L-aspartic acid and glycine is beneficial to improving the complexation and migration process of copper ions, thereby improving the stability of the copper layer polishing process.

[0085] The test results from Example 1 and Comparative Example 4 show that when the final pH of the polishing solution is increased to 10.0, although the copper removal rate increases, the Cu:SiCN removal rate selectivity decreases, and the dish-shaped depressions and surface roughness increase significantly. This indicates that controlling the final pH of the polishing solution between 7.8 and 8.3 is beneficial for coordinating the copper layer removal, dielectric layer removal, and TSV copper layer surface planarization processes.

[0086] The test results of Examples 1-5 show that the copper removal rate of the polishing solution of the present invention is 3560-4720. The Cu:dielectric layer removal rate selectivity ratio was 1.04–1.12 / min, the dish-shaped depression was 16–21 nm, and the surface roughness Ra was 0.23–0.31 nm. This demonstrates that by combining composite abrasives, copper corrosion inhibitors, organic acid complexing agents, and a final pH of 7.8–8.3, it is possible to maintain copper layer removal efficiency while reducing the dish-shaped depression and surface roughness of the copper layer in the silicon through-hole of the silicon carbide chip, and controlling the removal relationship between the copper layer and the dielectric layer.

[0087] The above are merely specific embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various variations or substitutions within the technical scope disclosed in the present invention, and these should all be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips, characterized in that, It comprises the following components by weight percentage: 12-18% composite abrasive, 0.05-0.4% copper corrosion inhibitor, 0.2-1.5% organic acid complexing agent, 0.5-2.5% oxidant, 0.005-0.08% surfactant, 0.01-0.3% pH adjuster, and the balance being deionized water; The composite abrasive is composed of fumed silica and silica sol, wherein the mass ratio of fumed silica to silica sol is 1:0.3 to 1:0.

8. The copper corrosion inhibitor is composed of 2-mercaptobenzothiazole and 8-hydroxyquinoline, wherein the mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:3 to 1:

5. The organic acid complexing agent is composed of malonic acid, L-aspartic acid and glycine, wherein the mass ratio of malonic acid, L-aspartic acid and glycine is 1:1 to 3:0.3 to 0.

8. The pH adjuster is one or both of tetramethylammonium hydroxide and monoethanolamine, and the pH of the polishing solution is 7.8 to 8.

3.

2. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The fumed silica has a particle size of 120–180 nm and a specific surface area of ​​220–280 m². 2 / g.

3. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The silica sol has a particle size of 30–60 nm, and the absolute value of the particle size distribution deviation does not exceed 4%.

4. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The mass ratio of 2-mercaptobenzothiazole to 8-hydroxyquinoline is 1:

4.

5. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The mass ratio of malonic acid, L-aspartic acid and glycine is 1:2:0.

5.

6. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The oxidant is one or both of urea peroxide and potassium persulfate.

7. The polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 1, characterized in that, The surfactant is composed of a fluorocarbon surfactant and a polyether-modified siloxane, wherein the mass ratio of the fluorocarbon surfactant to the polyether-modified siloxane is 1:5 to 1:

10.

8. A method for preparing a polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips, characterized in that, Includes the following steps: S1. Add one or both of tetramethylammonium hydroxide and monoethanolamine to deionized water as pH adjusters to adjust the pH to 7.5-8.

3. Then add malonic acid, L-aspartic acid and glycine, and stir until dissolved to obtain a premixed solution. S2. Dissolve 2-mercaptobenzothiazole and 8-hydroxyquinoline in ethanol, disperse them by ultrasonication, and then add them to the premixed solution obtained in step S1. The amount of ethanol used is 0.5-2% of the total mass of the polishing solution. The ethanol is used as a co-solvent and is not included in the total mass of the polishing solution formulation. S3. Fumed silica and silica sol are mixed in a high-speed shear disperser at a speed of 3000-5000 rpm for 20 minutes to obtain an abrasive suspension. S4. Add the abrasive suspension obtained in step S3 to the system obtained in step S2, then add surfactant and oxidant, and add deionized water to make up the volume. S5. The mixture obtained in step S4 is filtered sequentially through polyethersulfone filter cartridges with pore sizes of 1.2 μm and 0.45 μm to obtain a polishing solution with a pH of 7.8 to 8.

3.

9. The method for preparing the polishing slurry for chemical mechanical polishing of copper layers in silicon through-holes of silicon carbide chips according to claim 8, characterized in that, In step S2, the ultrasonic dispersion frequency is 40 kHz and the time is 15 min.

10. The method for preparing the polishing slurry for chemical mechanical polishing of the copper layer in silicon through-holes of silicon carbide chips according to claim 8, characterized in that, In step S4, the stirring speed is 200-250 r / min and the ambient temperature is 18-22 ℃.