An encapsulating film, its preparation method, and a photovoltaic module

By using different types of organic and inorganic UV blockers in the encapsulation film to control light transmittance and form a multilayer structure, the problem that the encapsulation film cannot effectively block UVA and UVB is solved, thereby improving the reliability and power generation efficiency of solar cells.

CN123063091APending Publication Date: 2026-11-10JIAXING YOUGU APPLIED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510590048.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing encapsulation films cannot effectively block UVA and UVB ultraviolet light, leading to solar cell aging and reduced power generation efficiency.

Method used

Different types of organic UV cut-off agents are used in combination, and the UVB transmittance of the encapsulation film is controlled at 1%-3% and the UVA transmittance at 60%-70%. Inorganic UV cut-off agents are combined to reflect UVB, forming a multi-layer encapsulation film.

Benefits of technology

It effectively slows down solar cell aging, improves power generation efficiency, reduces costs, and has good water vapor barrier properties and long-lasting UV cutoff effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063091A_ABST
    Figure CN123063091A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of photovoltaic technology and discloses an encapsulating film, its preparation method, and a photovoltaic module. The encapsulating film includes at least a first EVA layer, which comprises a first organic UV-blocking agent and a second organic UV-blocking agent. The first organic UV-blocking agent absorbs UVB but not UVA, while the second blocking agent absorbs both UVA and UVB. The UVB transmittance of the encapsulating film is in the range of 1%-3%, and the UVA transmittance is in the range of 60%-70%. By using different types of organic UV-blocking agents in combination and controlling the UVB transmittance of the encapsulating film within the range of 1%-3% and the UVA transmittance within the range of 60%-70%, this invention can reduce the aging of solar cells caused by ultraviolet radiation and thus decrease reliability, while also enabling the solar cells to have higher power output.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photovoltaic technology, and relates to an encapsulating film, its preparation method, and a photovoltaic module. Background Technology

[0002] The market is dominated by TOPCon battery technology for technological iteration and updates. Initially, its battery cell paste used Ag / Al composite technology. Conventional EVA encapsulation film corroded it, so POE was used for encapsulation. However, based on the LECO technology update, the paste was changed to Ag, which is an inert metal. Therefore, EVA can be used for encapsulation, which will reduce the corrosivity and reduce the cost of encapsulation materials.

[0003] According to the latest research report, solar cells (such as TOPCon cells) have a UVID problem, which is mainly reflected in the UVB band. Commercially available encapsulation films and existing publicly disclosed encapsulation films are mainly full cutoff, which not only cut off the UVB ultraviolet band, but also have a relatively high cutoff rate in the UVA ultraviolet band, which will affect the power of the module and thus affect the power generation efficiency of the module.

[0004] Therefore, providing an encapsulating film that can reduce the aging of solar cells caused by ultraviolet radiation and thus decrease their reliability, while also enabling solar cells to have high power, is a technical problem that urgently needs to be solved. Summary of the Invention

[0005] To address the aforementioned technical problems in the prior art, the present invention aims to provide an encapsulating film, its preparation method, and a photovoltaic module. By using different types of organic UV-blocking agents in combination and controlling the UVB and UVA transmittance of the encapsulating film, the present invention can reduce the aging of solar cells caused by ultraviolet radiation, thereby minimizing reliability loss, while simultaneously enabling the solar cells to achieve higher power output.

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides an encapsulating film, wherein the encapsulating film includes at least a first EVA layer, the first EVA layer including a first organic UV cutoff agent and a second organic UV cutoff agent, the first organic UV cutoff agent being able to absorb UVB but not UVA, and the second cutoff agent being able to absorb both UVA and UVB; the UVB transmittance of the encapsulating film is in the range of 1%-3% (e.g., it can be 1%, 1.2%, 1.5%, 1.7%, 2%, 2.3%, 2.5%, 2.7%, or 3%, etc.), and the UVA transmittance of the encapsulating film is in the range of 60%-70% (e.g., it can be 60%, 61%, 62%, 62.5%, 63%, 64%, 64.5%, 65%, 66%, 66.5%, 67%, 68%, 69%, or 70%, etc.).

[0008] This invention combines different types of organic UV cutoff agents and controls the UVB transmittance of the encapsulating film to be in the range of 1%-3% and the UVA transmittance of the encapsulating film to be in the range of 60%-70%. This approach can reduce the aging of solar cells caused by ultraviolet radiation and thus improve their reliability, while also enabling the solar cells to have higher power.

[0009] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. The technical objectives and beneficial effects of the present invention can be better achieved and realized through the following preferred technical solutions.

[0010] Preferably, the first organic UV cutoff agent includes at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312.

[0011] Preferably, the second organic UV cutoff agent includes at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-dimethylyl)-2-(1,3,5-triazinyl)5-octoxyphenol, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate sodium, UV-531, or UV-1164.

[0012] Preferably, the mass ratio of the first organic UV cutoff agent to the second organic UV cutoff agent is (1-5):1, for example, it can be 1:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.8:1, 3:1, 3.2:1, 3.5:1, 3.7:1, 4:1, 4.2:1, 4.4:1, 4.6:1, or 5:1, etc., preferably (1.5-2.5):1. Compared with the first organic UV cutoff agent, the second organic UV cutoff agent has a larger cutoff range for ultraviolet light and a greater impact on the transmittance of the entire ultraviolet band. When the mass ratio of the two is within the above-mentioned preferred range, the transmittance of the UVB and UVA bands can be better controlled in segments while ensuring cost.

[0013] Preferably, based on the mass of the first EVA layer, the total mass ratio of the first organic UV cutoff agent and the second organic UV cutoff agent is a1, where a1 is 0.1%-2%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.6%, 2.8%, 3%, 3.2%, 3.3%, 3.5%, 3.6%, 3.7%, 3.8%, or 4%, preferably 0.1%-1%. The total mass of the first organic UV cutoff agent and the second organic UV cutoff agent in the first EVA layer should not be too high, otherwise it will affect the visible light transmittance.

[0014] As a preferred embodiment of the encapsulating film of the present invention, the first EVA layer further includes a first inorganic UV cutoff agent. The inorganic UV cutoff agent can reflect UVB ultraviolet light, and compared to organic UV cutoff agents, it has a price advantage, thus reducing the cost of the encapsulating film.

[0015] Preferably, the first inorganic UV blocking agent includes titanium dioxide and / or zinc oxide.

[0016] Preferably, the average particle size of the first inorganic UV cutoff agent is 15nm-200nm, for example, it can be 15nm, 17nm, 18nm, 20nm, 22nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, 180nm, 185nm, 190nm, or 200nm, preferably 15nm-100nm. If the particles of the inorganic UV cutoff agent are too large, they are difficult to disperse and have high refractive index, reducing the transmittance of visible light; if the particles are too small, the cost is high.

[0017] Preferably, based on the mass of the first EVA layer, the mass percentage of the first inorganic UV cutoff agent is a2, where a2 is 0.05%-1%, for example, it can be 0.05%, 0.06%, 0.08%, 0.1%, 0.15%, 0.18%, 0.2%, 0.22%, 0.25%, 0.27%, 0.3%, 0.32%, 0.34%, 0.38%, 0.4%, 0.43%, 0.46%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, 1%, 1.05%, or 1.1%, etc., preferably 0.05%-0.5%. The mass percentage of the first inorganic UV cutoff agent in the first EVA layer should not be too high, otherwise it will affect the visible light transmittance.

[0018] In one embodiment, the thickness of the encapsulating film is 0.1mm-0.7mm, for example, it can be 0.1mm, 0.2mm, 0.3mm, 0.4mm, 0.5mm, 0.6mm or 0.7mm, etc.

[0019] As a preferred embodiment of the encapsulating film of the present invention, the encapsulating film further includes a POE layer and a second EVA layer, wherein the first EVA layer, the POE layer, and the second EVA layer are stacked sequentially; the second EVA layer includes a third organic UV cutoff agent and a fourth organic UV cutoff agent, wherein the third organic UV cutoff agent can absorb UVB but not UVA, and the fourth cutoff agent can absorb both UVA and UVB; the POE layer includes a fifth organic UV cutoff agent and a sixth organic UV cutoff agent, wherein the fifth organic UV cutoff agent can absorb UVB but not UVA, and the sixth cutoff agent can absorb both UVA and UVB.

[0020] In this technical solution, a first EVA layer, a POE layer, and a second EVA layer are sequentially stacked to form an EPE film. The POE layer blocks moisture, and the EVA layer has good adhesion. By setting the above structure and introducing two types of organic UV-blocking agents into the first EVA layer, the POE layer, and the second EVA layer, the EPE film's UV blocking effect can be improved while maintaining high initial power, and it also provides excellent moisture blocking. Furthermore, the correlation between the organic UV-blocking agents in the first EVA layer, the POE layer, and the second EVA layer effectively reduces migration problems, enabling long-term UV blocking.

[0021] In one embodiment, the encapsulation film is composed of a first EVA layer, a POE layer, and a second EVA layer stacked sequentially. This encapsulation film is an EPE encapsulation film.

[0022] Preferably, the third organic UV cutoff agent includes at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312.

[0023] Preferably, the fourth organic UV cutoff agent includes at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-dimethylyl)-2-(1,3,5-triazinyl)5-octoxyphenol, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate sodium, UV-531, or UV-1164.

[0024] Preferably, the mass ratio of the third organic UV cutoff agent to the fourth organic UV cutoff agent is (1.5 to 2.5):1, for example, it can be 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1 or 2.5:1, etc.

[0025] Preferably, the fifth organic UV cutoff agent includes at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312.

[0026] Preferably, the sixth organic ultraviolet blocking agent comprises at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)-5-octyloxyphenol, 2-hydroxy-4-methoxybenzophenone, sodium 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate, UV-531 or UV-1164.

[0027] Preferably, the mass ratio of the fifth organic ultraviolet blocking agent to the sixth organic ultraviolet blocking agent is (1.5 to 2.5):1, for example, may be 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1 or 2.5:1, etc.

[0028] As a preferred technical solution of the encapsulating adhesive film of the present invention, the first EVA layer comprises the first organic ultraviolet blocking agent, the second organic ultraviolet blocking agent and the first inorganic ultraviolet blocking agent; the second EVA layer comprises the third organic ultraviolet blocking agent, the fourth organic ultraviolet blocking agent and the second inorganic ultraviolet blocking agent; the POE layer comprises the fifth organic ultraviolet blocking agent and the sixth organic ultraviolet blocking agent, and the PEO layer does not contain an inorganic ultraviolet blocking agent;

[0029] The inorganic ultraviolet blocking agents are added to the first EVA layer and the second EVA layer, and the reflection of ultraviolet light by the inorganic ultraviolet blocking agents can effectively reduce the risk of failure of the solar cell after UV aging. Moreover, the inorganic blocking agents have better thermal stability and are not easy to fail, so that the internal POE layer can exert its effectiveness durably. Therefore, the encapsulating adhesive film is provided with long-acting UV blocking performance and excellent damp-heat aging resistance at the same time, and after being applied to a photovoltaic module, the service life and long-term power generation power of the photovoltaic module can be effectively improved.

[0030] As a preferred technical solution of the encapsulating adhesive film of the present invention, based on the mass of the second EVA layer, the total mass proportion of the third organic ultraviolet blocking agent and the fourth organic ultraviolet blocking agent is b1, b1>a1, the mass proportion of the second inorganic ultraviolet blocking agent is b2, b2<a2; based on the mass of the POE layer, the total mass proportion of the fifth organic ultraviolet blocking agent and the sixth organic ultraviolet blocking agent is c1, c1>b1.

[0031] In this preferred technical solution, the content gradient of the organic UV cutoff agent increases along the direction from the first EVA layer to the POE layer to the second EVA layer. Furthermore, the content of the inorganic UV cutoff agent in the first EVA layer is greater than that in the second EVA layer. The purpose of this arrangement is: ① To prevent the surface energy of the second EVA layer from becoming too low, ensuring sufficient adhesion for protecting the solar cell. Moreover, the highest content of the organic UV cutoff agent in the second EVA layer further blocks UVB light that the inorganic UV cutoff agent has not reflected. ② The higher content of the inorganic UV cutoff agent in the first EVA layer not only initially reflects some UVB light but also relatively protects the organic UV cutoff agent, preventing its decomposition and failure upon exposure to light.

[0032] Preferably, the second inorganic UV blocking agent comprises titanium dioxide and / or zinc oxide.

[0033] Preferably, the average particle size of the second inorganic UV cutoff agent is 15nm-200nm, for example, it can be 15nm, 17nm, 18nm, 20nm, 22nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 150nm, 155nm, 160nm, 165nm, 170nm, 175nm, 180nm, 185nm, 190nm, or 200nm, preferably 15nm-100nm. If the particles of the inorganic UV cutoff agent are too large, they are difficult to disperse and have high refractive index, reducing the transmittance of visible light; if the particles are too small, the cost is high.

[0034] Preferably, the thickness of the first EVA layer is 100μm-200μm, for example, it can be 100μm, 120μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm or 200μm.

[0035] Preferably, the thickness of the POE layer is 100μm-250μm, for example, it can be 100μm, 120μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm, 200μm, 210μm, 220μm, 230μm, 240μm or 250μm, etc.

[0036] Preferably, the thickness of the second EVA layer is 100μm-200μm, for example, it can be 100μm, 120μm, 140μm, 150μm, 160μm, 170μm, 180μm, 190μm or 200μm.

[0037] As a preferred embodiment of the encapsulating film of the present invention, the first EVA layer comprises the following components:

[0038]

[0039] The second EVA layer comprises the following components:

[0040]

[0041]

[0042] The POE layer comprises the following components:

[0043]

[0044] In this preferred embodiment, the content of each component in the first EVA layer is calculated as 100% of the total mass of the first EVA layer. The content of each component in the second EVA layer is calculated as 100% of the total mass of the second EVA layer. The content of each component in the POE layer is calculated as 100% of the total mass of the POE layer.

[0045] For example, the content of EVA material in the first EVA layer is 85%-95%, such as 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or 95%; the content of crosslinking agent in the first EVA layer is 0.1%-5%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%; the content of acrylate in the first EVA layer is 0.1%-4%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, or 4%; the content of silane coupling agent in the first EVA layer is 0.3%-3%, for example... The content of antioxidant in the first EVA layer can be 0.3%, 0.5%, 1%, 1.5%, 2%, 2.5%, or 3%, etc.; the content of antioxidant in the first EVA layer is 0.1%-0.3%, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, or 0.3%, etc.; the total content of the first organic UV cutoff agent and the second organic UV cutoff agent in the first EVA layer is 0.1%-0.8%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, or 0.8%, etc.; the content of the first inorganic UV cutoff agent is 0.1%-0.8%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, or 0.8%, etc.

[0046] For example, the content of EVA material in the second EVA layer is 85%-95%, such as 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or 95%; the content of crosslinking agent in the second EVA layer is 0.1%-5%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or 5%; the content of acrylate in the second EVA layer is 0.1%-4%, such as 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, or 4%; the content of silane coupling agent in the second EVA layer is 0.3%-3%, such as 0.3%-3%. The content of antioxidants in the second EVA layer is 0.1%-0.3%, such as 0.1%, 0.15%, 0.2%, 0.25%, or 0.3%. The total content of the third and fourth organic UV cutoff agents in the second EVA layer is 0.1%-1%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%. The content of the second inorganic UV cutoff agent is 0.05%-0.3%, such as 0.05%, 0.08%, 0.1%, 0.15%, 0.2%, 0.25%, or 0.3%.

[0047] For example, the POE material content in the POE layer is 85%-95%, such as 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, or 95%; the crosslinking agent content in the POE layer is 0.8%-3%, such as 0.8%, 1.5%, 2%, 2.5%, or 3%; and the silane coupling agent content in the POE layer is 0.3%-2%, such as 0.3%, 0.5%, etc. The content of antioxidants in the POE layer is 0.1%-0.3%, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, or 0.3%, etc.; the total content of the fifth and sixth organic UV cut-off agents in the POE layer is 0.1%-1%, for example, it can be 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, or 1%, etc.

[0048] By defining the components and content of the first EVA layer, POE layer, and second EVA layer, the bonding strength between the layers can be improved, the adhesion to the glass can be increased, and the service life of the encapsulating film can be extended. Specifically, the crosslinking agent promotes the formation of a polymer network structure; the acrylate acts as a co-crosslinking agent to further promote the formation of the polymer network structure; the silane coupling agent acts as a co-crosslinking agent to promote the formation of the polymer network structure and enhance the adhesion strength between the layers and between the EVA layer and the glass; and the antioxidant blocks the oxidation chain reaction and mitigates the aging of the polymer.

[0049] This invention does not specifically limit the type of acrylate in the first and second EVA layers, but includes, but is not limited to, at least one of ethoxytrimethylolpropane triacrylate, propoxytrimethylolpropane triacrylate, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, polyethylene glycol diacrylate, tricyclodecanedimethylol diacrylate, or ditrimethylolpropane tetraacrylate. It should be noted that the acrylates in both the first and second EVA layers can be selected from the above range, and the selection is independent; the specific types selected can be the same or different.

[0050] This invention does not specifically limit the types of crosslinking agents in the first EVA layer, the second EVA layer, and the POE layer, but includes, but is not limited to, at least one of tert-butyl peroxide-2-ethylhexyl carbonate, tert-amyl peroxy-2-ethylhexyl carbonate, triallyl isocyanurate, triallyl cyanurate, dicumyl peroxide, benzoyl peroxide, di-tert-butyl peroxide, or dicumyl hydroperoxide. It should be noted that the crosslinking agents in the first EVA layer, the second EVA layer, and the POE layer can all be selected from the above range, and the selection is independent; the specific types selected can be the same or different.

[0051] This invention does not specifically limit the types of silane coupling agents in the first EVA layer, the second EVA layer, and the POE layer, but includes, but is not limited to, at least one of propyltrioxyethyl isocyanate, vinyltriacetoxysilane, methacryloxypropyltrimethoxysilane derivatives, small molecule polysiloxanes, mercaptosilane derivatives, or hybrid functional silanes. It should be noted that the silane coupling agents in the first EVA layer, the second EVA layer, and the POE layer can all be selected from the above range, and the selection is independent; the specific types selected can be the same or different.

[0052] This invention does not specifically limit the types of antioxidants in the first EVA layer, the second EVA layer, and the POE layer, but includes, but is not limited to, at least one of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], or tris[2,4-di-tert-butylphenyl]phosphite. It should be noted that the antioxidants in the first EVA layer, the second EVA layer, and the POE layer can all be selected from the above range, and the selection is independent; the specific types selected can be the same or different.

[0053] In one embodiment, the first organic UV-blocking agent in the first EVA layer and the third organic UV-blocking agent in the second EVA layer are of the same type, and the second organic UV-blocking agent in the first EVA layer and the fourth organic UV-blocking agent in the second EVA layer are of the same type. This configuration helps to mitigate the performance degradation of the encapsulating film caused by material migration after prolonged use.

[0054] In a second aspect, the present invention provides a method for preparing an encapsulating film as described in the first aspect, the method comprising the following steps:

[0055] The raw materials are mixed according to the formula, and then cast to obtain the first EVA layer.

[0056] Preferably, the preparation method further includes:

[0057] The raw materials are mixed according to the formula, and then cast to obtain the second EVA layer.

[0058] The raw materials are mixed according to the formula and then cast to obtain the POE layer.

[0059] The first EVA layer, the second EVA layer, and the POE layer are laminated together by thermal bonding to obtain the encapsulating film.

[0060] In the preparation method of the present invention, the raw materials of EVA material are not specifically limited. For example, they can be EVA particles with a melt index of (10-30) g / 10min at 125°C and 2.16 kg (e.g., 10 g / 10min, 12 g / 10min, 15 g / 10min, 18 g / 10min, 20 g / 10min, 22 g / 10min, 25 g / 10min, 28 g / 10min or 30 g / 10min, etc.) and a VA mass content of 2%-30% (e.g., 2%, 4%, 5%, 8%, 10%, 12%, 15%, 17%, 20%, 22%, 25%, 27% or 30%, etc.). They can be one or more of the above-mentioned EVA particles.

[0061] In the preparation method of the present invention, the raw materials for POE material are not specifically limited, and can be POE particles, such as one or more of Dow 8669, Dow8660, LG-LF57, LG-LF657, and Mitsui Chemicals 620.

[0062] Thirdly, the present invention provides a photovoltaic module, the photovoltaic module comprising photovoltaic glass, an encapsulating film and a battery cell stacked sequentially, wherein the encapsulating film is the encapsulating film described in the first aspect, and the first EVA layer is in contact with the battery cell.

[0063] In this invention, UVT-1, UV 2908, UV-1600, UV-531 and UV-1164 are all commercially available trademarks.

[0064] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0065] Compared with existing technologies, the present invention has the following beneficial effects:

[0066] (1) By using different types of organic UV cut-off agents in combination and controlling the UVB transmittance of the encapsulating film to be in the range of 1%-3% and the UVA transmittance of the encapsulating film to be in the range of 60%-70%, the present invention can reduce the aging of solar cells caused by ultraviolet rays and reduce their reliability, while also enabling the solar cells to have higher power.

[0067] (2) By further introducing an inorganic UV cutoff agent into the encapsulation film, it can reflect UVB ultraviolet light. Moreover, the inorganic UV cutoff agent has a price advantage over the organic UV cutoff agent, which can reduce the cost of the encapsulation film.

[0068] (3) An EPE film is constructed by sequentially layering a first EVA layer, a POE layer, and a second EVA layer. Two types of organic UV cutoff agents are introduced into the first EVA layer, the POE layer, and the second EVA layer, respectively. This improves the UV cutoff effect of the EPE film while maintaining high initial power, and also gives the EPE film a good moisture barrier effect. Moreover, this EPE film can achieve long-term UV cutoff.

[0069] (4) This invention uses different types of organic UV-blocking agents in combination and controls the UVB transmittance of the encapsulating film to be within the range of 1%-3%, and the UVA transmittance of the encapsulating film to be above 50%, preferably within the range of 60%-70%. This reduces the aging of solar cells caused by ultraviolet radiation and thus lowers their reliability, while also enabling the solar cells to have higher power. The visible light transmittance of the encapsulating film of this invention is above 89%, preferably above 90%; the yellowing in the UV aging test is below 0.5, the UV power decay is below 3.25%; and the DH power decay in the damp heat aging test is below 3.8%. Attached Figure Description

[0070] Figure 1 This is a schematic diagram of the structure of an encapsulating film provided in one embodiment of the present invention, wherein 1 is a first EVA layer; 2 is a POE layer; and 3 is a second EVA layer. Detailed Implementation

[0071] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0072] The specific embodiments described herein are for illustrative purposes only and are not intended to limit the scope of the invention.

[0073] Example 1

[0074] This embodiment provides an encapsulating film, such as Figure 1 As shown, the encapsulating film includes a first EVA layer 1 (180 μm thick), a POE layer 2 (100 μm thick), and a second EVA layer 3 (150 μm thick) stacked sequentially.

[0075] The composition of the first EVA layer 1 is shown in Table 1-1, the composition of the POE layer 2 is shown in Table 1-2, and the composition of the second EVA layer 3 is shown in Table 1-3. The content of each component in the first EVA layer 1 is calculated as 100% of the total mass of the first EVA layer 1; the content of each component in the POE layer 2 is calculated as 100% of the total mass of the POE layer 2; and the content of each component in the second EVA layer 3 is calculated as 100% of the total mass of the second EVA layer 3.

[0076] Table 1-1 Composition of the first EVA layer

[0077]

[0078]

[0079] Table 1-2 Composition of POE layer

[0080]

[0081] Table 1-3 Composition of the second EVA layer

[0082]

[0083] The method for preparing the encapsulating film in this embodiment includes the following steps:

[0084] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, first organic UV cutoff agent, first inorganic UV cutoff agent and second organic UV cutoff agent are mixed and cast to obtain the first EVA layer.

[0085] POE particles, crosslinking agent, silane coupling agent, antioxidant, fifth organic UV cutoff agent and sixth organic UV cutoff agent are mixed and cast to obtain POE layer;

[0086] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, third organic UV cutoff agent, first inorganic UV cutoff agent and fourth organic UV cutoff agent are mixed and cast to obtain the second EVA layer.

[0087] The first EVA layer, the POE layer, and the second EVA layer are laminated together by a thermal lamination method to obtain the encapsulating film.

[0088] Example 2

[0089] This embodiment provides an encapsulating film comprising a first EVA layer (100 μm thick), a POE layer (150 μm thick), and a second EVA layer (200 μm thick) stacked sequentially.

[0090] The composition of the first EVA layer is shown in Table 2-1, the composition of the POE layer is shown in Table 2-2, and the composition of the second EVA layer is shown in Table 2-3. The content of each component in the first EVA layer is calculated based on the total mass of the first EVA layer being 100%; the content of each component in the POE layer is calculated based on the total mass of the POE layer being 100%; and the content of each component in the second EVA layer is calculated based on the total mass of the second EVA layer being 100%.

[0091] Table 2-1 Composition of the first EVA layer

[0092]

[0093] Table 2-2 Composition of POE layer

[0094]

[0095] Table 2-3 Composition of the second EVA layer

[0096]

[0097] The method for preparing the encapsulating film in this embodiment includes the following steps:

[0098] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, first organic UV cutoff agent, first inorganic UV cutoff agent and second organic UV cutoff agent are mixed and cast to obtain the first EVA layer.

[0099] POE particles, crosslinking agent, silane coupling agent, antioxidant, fifth organic UV cutoff agent and sixth organic UV cutoff agent are mixed and cast to obtain POE layer;

[0100] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, third organic UV cutoff agent, first inorganic UV cutoff agent and fourth organic UV cutoff agent are mixed and cast to obtain the second EVA layer.

[0101] The first EVA layer, the POE layer, and the second EVA layer are laminated together by a thermal lamination method to obtain the encapsulating film.

[0102] Example 3

[0103] This embodiment provides an encapsulating film comprising a first EVA layer (150 μm thick), a POE layer (220 μm thick), and a second EVA layer (100 μm thick) stacked sequentially.

[0104] The composition of the first EVA layer is shown in Table 3-1, the composition of the POE layer is shown in Table 3-2, and the composition of the second EVA layer is shown in Table 3-3. The content of each component in the first EVA layer is calculated as 100% of the total mass of the first EVA layer; the content of each component in the POE layer is calculated as 100% of the total mass of the POE layer; and the content of each component in the second EVA layer is calculated as 100% of the total mass of the second EVA layer.

[0105] Table 3-1 Composition of the first EVA layer

[0106]

[0107] Table 3-2 Composition of POE layer

[0108]

[0109] Table 3-3 Composition of the second EVA layer

[0110]

[0111] The method for preparing the encapsulating film in this embodiment includes the following steps:

[0112] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, first organic UV cutoff agent, first inorganic UV cutoff agent and second organic UV cutoff agent are mixed and cast to obtain the first EVA layer.

[0113] POE particles, crosslinking agent, silane coupling agent, antioxidant, fifth organic UV cutoff agent and sixth organic UV cutoff agent are mixed and cast to obtain POE layer;

[0114] EVA particles, crosslinking agent, acrylate, silane coupling agent, antioxidant, third organic UV cutoff agent, first inorganic UV cutoff agent and fourth organic UV cutoff agent are mixed and cast to obtain the second EVA layer.

[0115] The first EVA layer, the POE layer, and the second EVA layer are laminated together by a thermal lamination method to obtain the encapsulating film.

[0116] Example 4

[0117] This embodiment provides an encapsulating film, which differs from Embodiment 1 in the composition of the first EVA layer, as shown in Table 4. The content of each component in the first EVA layer is calculated based on the total mass of the first EVA layer being 100%.

[0118] Table 4 Composition of the first EVA layer

[0119]

[0120] Example 5

[0121] This embodiment provides an encapsulating film, which differs from Embodiment 1 in the composition of the second EVA layer, as shown in Table 5. The content of each component in the second EVA layer is calculated based on the total mass of the second EVA layer being 100%.

[0122] Table 5 Composition of the second EVA layer

[0123]

[0124] Example 6

[0125] This embodiment provides an encapsulating film, which differs from Embodiment 1 in the composition of the first EVA layer, as shown in Table 6. The content of each component in the first EVA layer is calculated based on the total mass of the first EVA layer being 100%.

[0126] Table 6 Composition of the first EVA layer

[0127]

[0128] Example 7

[0129] This embodiment provides an encapsulating film, which differs from Embodiment 1 in the composition of the second EVA layer, as shown in Table 7. The content of each component in the second EVA layer is calculated based on the total mass of the second EVA layer being 100%.

[0130] Table 7 Composition of the second EVA layer

[0131]

[0132] Example 8

[0133] This embodiment provides an encapsulating film, which differs from Embodiment 1 in that it includes a first EVA layer and a second EVA layer, as shown in Tables 8 and 9. The content of each component in the first EVA layer is calculated based on the total mass of the first EVA layer being 100%; the content of each component in the second EVA layer is calculated based on the total mass of the second EVA layer being 100%.

[0134] Table 8 Composition of the first EVA layer

[0135]

[0136] Table 9 Composition of the Second EVA Layer

[0137]

[0138] Comparative Example 1

[0139] This comparative example provides an encapsulating film that does not contain a UV cutoff agent. The encapsulating film includes a first EVA layer (150 μm thick), a POE layer (100 μm thick), and a second EVA layer (150 μm thick) stacked sequentially.

[0140] The composition of the first EVA layer is shown in Table 10, the composition of the POE layer is shown in Table 11, and the composition of the second EVA layer is shown in Table 12.

[0141] Table 10 Composition of the first EVA layer

[0142] Specific components Number of portions by weight Hanwha 282PV 95 2-Ethylhexyl tert-butyl peroxide 0.9 Triallyl isocyanurate 0.7 Triallyl cyanurate 0.5 propyltrioxoethylsilane 0.8 Epoxysilane oligomers 0.8 Ethylene oxide trimethylolpropane triacrylate 1.1 β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol ester 0.2

[0143] Table 11 Composition of POE layer

[0144]

[0145] Table 12 Composition of the Second EVA Layer

[0146] Specific components Number of portions by weight Hanwha 282PV 95 2-Ethylhexyl tert-butyl peroxide 0.9 Triallyl isocyanurate 0.7 Triallyl cyanurate 0.5 Propyltrioxoethylsilane isocyanate 0.8 Epoxysilane oligomers 0.8 Ethylene oxide trimethylolpropane triacrylate 1.1 β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate n-octadecyl alcohol ester 0.2

[0147] The preparation method of the encapsulating film in this comparative example includes the following steps:

[0148] The raw materials are mixed and cast to obtain the first EVA layer;

[0149] The raw materials are mixed and then cast to obtain the POE layer;

[0150] The raw materials are mixed and cast to obtain the second EVA layer;

[0151] The first EVA layer, the POE layer, and the second EVA layer are laminated together by a thermal lamination method to obtain the encapsulating film.

[0152] Comparative Example 2

[0153] This comparative example provides an encapsulating film, which differs from Example 1 in that the composition of the first EVA layer and the second EVA layer is shown in Tables 13 and 14. The content of each component in the first EVA layer is calculated as 100% of the total mass of the first EVA layer; the content of each component in the second EVA layer is calculated as 100% of the total mass of the second EVA layer.

[0154] Table 13 Composition of the first EVA layer

[0155]

[0156] Table 14 Composition of the Second EVA Layer

[0157]

[0158]

[0159] The light transmittance of the encapsulating films provided in Examples 1-8 and Comparative Examples 1-2 was tested using the following methods:

[0160] The light transmittance of the encapsulating films provided in the above examples and comparative examples was tested in accordance with GB / T 2410-2008 "Determination of transmittance and haze of plastic films and sheets".

[0161] The encapsulating films provided in Examples 1-8 and Comparative Examples 1-2 are used in photovoltaic modules. The preparation method of the photovoltaic module includes: front glass (Xinyi Glass, length × width × height = 2272mm × 1128mm × 2mm), encapsulating film, solar cell (Canadian Solar, CC10MB-HJT), conventional EVA film (composition is the same as the first EVA layer in Comparative Example 1, thickness is 550μm) and back glass (length × width × height = 2272mm × 1128mm × 2mm) are stacked in sequence, wherein the third EVA layer of the encapsulating film is in contact with the solar cell, and after lamination, a double-glass TOPCon module is obtained, that is, the photovoltaic module is obtained.

[0162] The photovoltaic modules were subjected to UV aging tests with an irradiation intensity of 200W / m. 2 The cumulative irradiance is 200 kWh / m². 2 The measurement of yellowing and power decay of photovoltaic modules before and after UV aging is performed. The value of yellowing is the absolute value of the difference before and after aging. Power decay refers to the rate of change of photovoltaic module power after UV aging relative to before UV aging. The rate of change of power is calculated as (initial power - power after aging) / initial power × 100%.

[0163] The photovoltaic modules were subjected to a DH damp heat aging test under the following conditions: 85% RH, 85℃, for 2000 hours. The power degradation due to damp heat aging is calculated as: (Power before damp heat test - Power after damp heat test) / Power before damp heat test.

[0164] The test results are shown in Table 13.

[0165] Table 13

[0166]

[0167] This invention combines different types of organic UV cutoff agents and controls the UVB transmittance of the encapsulating film to be in the range of 1%-3%, and the UVA transmittance of the encapsulating film to be above 50%, preferably in the range of 60%-70%. This approach can reduce the aging of solar cells caused by ultraviolet radiation and thus reduce their reliability, while also enabling the solar cells to have higher power.

[0168] The visible light transmittance of the encapsulating film of the present invention is above 89%, preferably above 90%; the yellowing in the UV aging test is below 0.5, the UV power attenuation is below 3.5%; and the DH power attenuation in the damp heat aging test is below 3.8%.

[0169] The encapsulating film of Comparative Example 1 does not contain a UV cutoff agent, and its UVB and UVA transmittance are both high, resulting in a UV power attenuation of up to 5.5%. Moreover, since no inorganic UV cutoff agent was added, it lost its ability to absorb some moisture, resulting in a higher degree of DH power attenuation.

[0170] The cutoff agents in Comparative Example 2 are all full-band cutoff agents, which significantly reduces UVA transmittance and causes DH power attenuation of up to 4.4%.

[0171] A comparison of Examples 1 and 4-5 shows that an excessive amount of inorganic UV cutoff agent in the first or second EVA layer will reduce the transmittance of visible light and the initial power. At the same time, the increased content of inorganic UV cutoff agent increases the damp heat stability of the photovoltaic module and reduces DH power decay. Moreover, due to its own reflection of ultraviolet and visible light, it can further reduce the impact of ultraviolet light on organic UV absorbers and encapsulants, reduce the yellowing value after UV aging, and reduce UV power decay.

[0172] A comparison of Examples 1 and 6-7 shows that when both a UVB cutoff agent and a full-band UV cutoff agent are present, if the content of the full-band UV cutoff agent exceeds 50%, the UVA transmittance will decrease. This is not conducive to maintaining high initial power of the photovoltaic module while reducing its UV power decay, and thus is not conducive to improving the reliability of the module.

[0173] A comparison of Examples 1 and 8 shows that the content gradient of the organic UV cut-off agent increases along the direction of the first EVA layer → POE layer → second EVA layer. Moreover, it is a preferred setting that the content of the inorganic UV cut-off agent in the first EVA layer is greater than that in the second EVA layer. This is beneficial for ensuring high UVA transmittance, low yellowing, high initial power, low UV power attenuation, and low DH power attenuation, thereby improving the reliability of the component.

[0174] In summary, the encapsulating film prepared by this invention ensures both low transmittance in the UVB band and high transmittance in the UVA band, guaranteeing high initial power of the module, while also improving the module's UV resistance and resistance to damp heat. Furthermore, by layering inorganic UV absorbers, the overall cost of the UV absorbers can be reduced, which is beneficial for their subsequent industrialization and promotion.

[0175] The applicant declares that the detailed method of the present invention is illustrated by the above embodiments, but the present invention is not limited to the above detailed method, that is, it does not mean that the present invention must rely on the above detailed method to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An encapsulating film, characterized in that, The encapsulating film includes at least a first EVA layer, which includes a first organic UV cutoff agent and a second organic UV cutoff agent. The first organic UV cutoff agent can absorb UVB but not UVA, and the second cutoff agent can absorb both UVA and UVB. The UVB transmittance of the encapsulating film is in the range of 1%-3%, and the UVA transmittance of the encapsulating film is in the range of 60%-70%.

2. The encapsulating film according to claim 1, characterized in that, The first organic UV cutoff agent includes at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312; Preferably, the second organic UV cutoff agent comprises at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-dimethylyl)-2-(1,3,5-triazinyl)5-octoxyphenol, 2-hydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate sodium salt, UV-531 or UV-1164; Preferably, the mass ratio of the first organic UV cutoff agent to the second organic UV cutoff agent is (1-5):1, more preferably (1.5-2.5):1; Preferably, based on the mass of the first EVA layer, the total mass ratio of the first organic UV cutoff agent and the second organic UV cutoff agent is a1, where a1 is 0.1%-2%, preferably 0.1%-1%.

3. The encapsulating film according to claim 1 or 2, characterized in that, The first EVA layer also includes a first inorganic ultraviolet blocking agent; Preferably, the first inorganic UV blocking agent includes at least one of titanium dioxide and / or zinc oxide; Preferably, the average particle size of the first inorganic UV cutoff agent is 15nm-200nm, and more preferably 15nm-100nm; Preferably, based on the mass of the first EVA layer, the mass percentage of the first inorganic UV cutoff agent is a2, where a2 is 0.05%-1%, preferably 0.05%-0.5%.

4. The encapsulating film according to any one of claims 1-3, characterized in that, The encapsulating film also includes a POE layer and a second EVA layer, wherein the first EVA layer, the POE layer and the second EVA layer are stacked sequentially. The second EVA layer includes a third organic UV cutoff agent and a fourth organic UV cutoff agent. The third organic UV cutoff agent can absorb UVB but cannot absorb UVA, and the fourth cutoff agent can absorb both UVA and UVB. The POE layer includes a fifth organic UV cutoff agent and a sixth organic UV cutoff agent. The fifth organic UV cutoff agent can absorb UVB but not UVA, and the sixth cutoff agent can absorb both UVA and UVB.

5. The encapsulating film according to claim 4, characterized in that, The third organic UV cutoff agent includes at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoate, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312. Preferably, the fourth organic ultraviolet blocking agent comprises at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)-5-octyloxyphenol, 2-hydroxy-4-methoxybenzophenone, sodium 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate, UV-531 or UV-1164; Preferably, the mass ratio of the third organic ultraviolet blocking agent to the fourth organic ultraviolet blocking agent is (1.5~2.5):1; Preferably, the fifth organic ultraviolet blocking agent comprises at least one of 3,5-bis(1,1-dimethylethyl)-4-hydroxybenzoic acid hexadecyl ester, 2-hydroxyphenyl-s-triazine derivative, UV-120, UVT-1, UV-2908, UV-1600 or UV-312; Preferably, the sixth organic ultraviolet blocking agent comprises at least one of 2,4-dihydroxybenzophenone, 2-[4,6-bis(2,4-xylyl)-2-(1,3,5-triazinyl)-5-octyloxyphenol, 2-hydroxy-4-methoxybenzophenone, sodium 2,2'-dihydroxy-4,4'-dimethoxybenzophenone-5,5'-disulfonate, UV-531 or UV-1164; Preferably, the mass ratio of the fifth organic ultraviolet blocking agent to the sixth organic ultraviolet blocking agent is (1.5~2.5):

1.

6. The encapsulating film according to claim 4 or 5, characterized in that, The first EVA layer comprises the first organic ultraviolet blocking agent, the second organic ultraviolet blocking agent and the first inorganic ultraviolet blocking agent; The second EVA layer comprises the third organic ultraviolet blocking agent, the fourth organic ultraviolet blocking agent and the second inorganic ultraviolet blocking agent; The POE layer comprises the fifth organic ultraviolet blocking agent and the sixth organic ultraviolet blocking agent, and the POE layer contains no inorganic ultraviolet blocking agent; Preferably, based on the mass of the second EVA layer, the total mass proportion of the third organic ultraviolet blocking agent and the fourth organic ultraviolet blocking agent is b1, b1>a1, the mass proportion of the second inorganic ultraviolet blocking agent is b2, b2<a2; based on the mass of the POE layer, the total mass proportion of the fifth organic ultraviolet blocking agent and the sixth organic ultraviolet blocking agent is c1, c1>b1; Preferably, the second inorganic ultraviolet blocking agent comprises titanium dioxide and / or zinc oxide; Preferably, the average particle size of the second inorganic ultraviolet blocking agent is 15nm-200nm, preferably 15nm-100nm.

7. The encapsulating film according to any one of claims 4-6, characterized in that, The thickness of the first EVA layer is 100μm-200μm; Preferably, the thickness of the POE layer is 100μm-250μm; Preferably, the thickness of the second EVA layer is 100μm-200μm.

8. The encapsulating film according to any one of claims 4-7, characterized in that, The first EVA layer comprises the following components: The second EVA layer comprises the following components: The POE layer comprises the following components:

9. A method for preparing an encapsulating film as described in any one of claims 1-8, characterized in that, The preparation method comprises the following steps: Mix the raw materials according to the formula amount, and perform casting to obtain the first EVA layer; Preferably, the preparation method further comprises: The raw materials are mixed according to the formula, and then cast to obtain the second EVA layer. The raw materials are mixed according to the formula and then cast to obtain the POE layer. The first EVA layer, the second EVA layer, and the POE layer are laminated together by thermal bonding to obtain the encapsulating film.

10. A photovoltaic module, characterized in that, The photovoltaic module includes photovoltaic glass, encapsulating film and solar cells stacked in sequence, wherein the encapsulating film is the encapsulating film according to any one of claims 1-8.