Bridging and sealing compositions and methods

By combining rigid porous materials with elastic deformable materials, an integral sealing layer is formed, and the small pores are filled with fibers and fine particles, which solves the problem of backflow failure in bridging and sealing technology and achieves high anti-backflow capability and stable sealing effect.

CN123063153APending Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202510583862.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing bridging and plugging technologies are prone to backflow failure during the drilling process, and their insufficient resistance to backflow leads to plugging failure.

Method used

A combination of rigid porous materials, elastic deformable materials, fiber materials, and fine particulate materials is used. Through the interaction between the rigid porous materials and the elastic deformable materials, an integral sealing layer is formed. The fiber and fine particulate materials are used to fill the small pores to improve the anti-backflow ability.

Benefits of technology

It achieves a pressure resistance of not less than 10MPa and a backflow resistance of not less than 5MPa for bridging and plugging, significantly reducing the occurrence of backflow of plugging material during tripping in and out of the drill string and improving the stability of the plugging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063153A_ABST
    Figure CN123063153A_ABST
Patent Text Reader

Abstract

This invention relates to the field of bridging and sealing technology, and discloses a bridging and sealing composition and method. The bridging and sealing composition of this invention comprises a rigid porous material, an elastic deformable material, a fiber material, and a fine particulate material; wherein the weight ratio of the rigid porous material, the elastic deformable material, the fiber material, and the fine particulate material is 1:0.1-0.8:0.2-1:1-2. The bridging and sealing composition of this invention has a pressure resistance of not less than 10 MPa and a backflow resistance of not less than 5 MPa when used for bridging and sealing, which significantly improves the backflow resistance compared to conventional bridging and sealing slurries, greatly reducing the occurrence of sealing failure accidents caused by backflow of sealing material due to the suction effect generated during drilling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of bridging and sealing technology, and more specifically to bridging and sealing compositions and methods. Background Technology

[0002] Bridging and sealing technology is widely used, accounting for over 80% of all well leakage treatment methods. This technology is convenient to use and safe to implement. Bridging and sealing materials are classified into three main categories based on their appearance: granular, flake-like, and fibrous materials. In sealing operations, these three types of materials, when used individually, have limited effectiveness and cannot effectively seal the leaking layer. They must be combined in a reasonable ratio and gradation to achieve the desired sealing effect. Based on the different physical properties of the sealing materials, the mechanisms of action in the bridging and sealing process include: bridging, blocking and embedding, filtration, "stretching" within the filter cake, expansion blocking, and choking.

[0003] Bridging and sealing utilize the physical accumulation of materials to create a sealing layer of sufficient strength within the leakage channel, isolating the wellbore from the formation and achieving the purpose of sealing the leakage. However, during the bridging process, there is little or no interaction between the materials, resulting in a sealing layer that cannot function as a unified whole and has poor resistance to backflow. Although the positive pressure resistance can meet the requirements of normal drilling operations, during processes such as tripping out of the well, the suction pressure creates a certain negative pressure at the leakage site. The poor backflow resistance of the sealing wall formed by the bridging material causes the sealing material to be backflowed, reducing the strength of the sealing wall and leading to sealing failure and re-leakage at the leakage site.

[0004] CN115873566A discloses a bridging and plugging material for drilling fluids and its preparation method. The bridging and plugging material used is composed of at least one of the following: regularly shaped polyhedra, irregularly shaped polyhedra, and irregularly shaped bodies with corners or sharp points. Materials with sharp edges are more likely to adhere and bridge in fractures, and the sharper the edges and the more irregular the shape of the particles, the more conducive it is to the retention of the plugging material in the fracture. Therefore, the mixed application of materials with different shapes is more conducive to the sealing of fractures and the retention of the material in the fracture, while increasing the material's resistance to backflow, reducing the risk of re-leakage, and improving the success rate of plugging.

[0005] CN116064009A discloses a bridging plugging slurry and its preparation method. The bridging plugging slurry utilizes a shape memory alloy with a two-way effect, whose shape changes with temperature, to form a novel plugging slurry with good backflow capability. This slurry is used for reservoir plugging operations. At reservoir temperatures, it expands to form a sealing layer. Later, when the near-wellbore reservoir temperature is lowered using clean water circulation, the plugging material shrinks, the sealing layer is destroyed, and the plugging material in the oil and gas permeation channel is backflowed, freeing up the oil and gas permeation channel without affecting subsequent oil and gas production, thus improving production and development efficiency.

[0006] CN115806808A discloses a bridging and sealing method and its application. The method uses a bridging and sealing formula containing slag to form a primary sealing layer in the leakage channel, and then injects an alkaline solution to activate the slag in the sealing layer, thereby solidifying the entire sealing layer into a whole and improving the anti-backflow ability.

[0007] Although existing technologies utilize the interaction of irregular shapes, the expansion and contraction of shape memory metals, and chemical reactions to form a monolithic sealing layer, which improves the anti-backflow capability to some extent, there are still problems such as poor individual effects, the need to rely on external factors and chemical reactions, and the tendency to fail backflow during bridging and sealing processes. Summary of the Invention

[0008] The purpose of this invention is to overcome the problem of backflow failure that easily occurs in existing bridging and sealing processes, and to provide a bridging and sealing composition and a bridging and sealing method. The bridging and sealing composition of this invention can significantly improve the backflow resistance when used for bridging and sealing, so that the backflow resistance of the sealing layer is not less than 5MPa.

[0009] To achieve the above objectives, a first aspect of the present invention provides a bridging and sealing composition comprising a rigid porous material, an elastic deformable material, a fiber material, and a fine particulate material; wherein the weight ratio of the rigid porous material, the elastic deformable material, the fiber material, and the fine particulate material is 1:0.1-0.8:0.2-1:1-2; and the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:15-100.

[0010] A second aspect of the present invention provides a bridging and sealing grout, the bridging and sealing grout comprising a base grout and the bridging and sealing composition described in the first aspect above.

[0011] A third aspect of the present invention provides a method for bridging and plugging leaks, the method comprising pumping the bridging and plugging slurry described in the second aspect into the lost well section.

[0012] The fourth aspect of this invention relates to the application of the bridging and plugging composition described in the first aspect, the bridging and plugging slurry described in the second aspect, or the bridging and plugging method described in the third aspect in oil and gas well plugging.

[0013] The beneficial technical effects achieved by the present invention through the above technical solution are as follows:

[0014] (1) This invention utilizes the mechanism of the interaction between porous rigid materials and elastic materials with good deformation capacity. The elastic material can enter the pores of the porous rigid material through deformation to form a whole. They interact within the leakage channel to form a primary sealing layer. Other small particulate materials, fibers and other filling materials are used to seal the small pores left after bridging, and finally an effective sealing layer is formed.

[0015] (2) The bridging and sealing composition of the present invention has a pressure resistance of not less than 10 MPa and a backflow resistance of not less than 5 MPa when used for bridging and sealing. It has a significantly improved backflow resistance compared with conventional bridging and sealing slurry, which can greatly reduce the occurrence of sealing failure accidents caused by the backflow of sealing material due to the suction effect generated during the drilling process. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of a structure in which an elastically deformable material is embedded in the pores of a rigid porous material, according to one embodiment of the present invention. Detailed Implementation

[0017] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0018] The first aspect of the present invention provides a bridging and sealing composition, the bridging and sealing composition comprising a rigid porous material, an elastic deformable material, a fiber material, and a fine particulate material; wherein the weight ratio of the rigid porous material, the elastic deformable material, the fiber material, and the fine particulate material is 1:0.1-0.8:0.2-1:1-2; and the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:15-100.

[0019] The bridging and sealing composition of the present invention utilizes the interaction between different materials to form an effective physical sealing layer, thereby improving the anti-backflow capability.

[0020] According to the present invention, the weight ratio of the rigid porous material to the elastically deformable material is 1:0.1-0.8, for example, 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, or any value within the range of any two values; the weight ratio of the rigid porous material to the fiber material is 1:0.2-1, for example, 1:0.2, 1:0.3, 1:0.4, 1:0. 5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, and any value within the range of any two values; the weight ratio of the rigid porous material to the fine particulate material is 1:1-2, for example, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, and any value within the range of any two values.

[0021] According to this invention, the cross-sectional diameter of an elastically deformable material refers to the maximum distance between any two points within the cross-section of the material. It is the distance between the two points furthest apart. For example, the diameter of a circular cross-section is the diameter of the circle; the diameter of a rectangular cross-section is the length of its diagonal; and the diameter of an irregular cross-section needs to be determined by calculating or measuring the distances between all possible pairs of points.

[0022] According to the present invention, the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:15-100, for example, 1:15, 1:20, 1:30, 1:40, 1:50, 1:60, 1:70, 1:80, 1:90, 1:100, and any value within the range of any two values.

[0023] The bridging and sealing composition of the present invention utilizes the interaction between different materials, especially a specific ratio of rigid porous materials and elastic deformable materials, to form an effective physical sealing layer and improve the anti-backflow capability.

[0024] According to some preferred embodiments of the present invention, the weight ratio of the rigid porous material, the elastic deformable material, the fiber material, and the fine particulate material is 1:0.2-0.5:0.4-0.8:1-1.6, for example, 1:0.3:0.5:1.2, 1:0.4:0.6:1.3, 1:0.5:0.8:1.5, 1:0.3:0.6:1.6, 1:0.5:0.5:1.5, 1:0.4:0.7:1.3, and any value within the range of any two values.

[0025] According to some preferred embodiments of the present invention, the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:50-80.

[0026] According to the present invention, the bridging and sealing composition using the above-mentioned proportions has better anti-backflow capability when used for bridging and sealing.

[0027] According to some embodiments of the present invention, at least a portion of the elastic deformable material is embedded in the pores of the rigid porous material.

[0028] According to the present invention, the elastic material has a low density and occupies a larger volume in the composition than the fiber and fine particulate materials. During the mixing process, it can be ensured that a certain proportion of the elastic material can be embedded in the pores of the rigid porous material.

[0029] According to some preferred embodiments of the present invention, based on the total number of pores of the rigid porous material, the percentage of the number of pores embedded with the elastic deformable material is not less than 30%, for example, 30%, 40%, 50%, 60%, and any value in the range of any two values, preferably 30-50%.

[0030] According to some embodiments of the present invention, the fibrous material and fine particulate material fill the voids formed by the combination of the rigid porous material and the elastic deformable material.

[0031] This invention does not specifically limit the embedding method; any method that allows the elastically deformable material to be embedded into the pores of the rigid porous material, thus connecting the two materials into one, is acceptable. For example... Figure 1 The diagram shows a structure in which an elastic deformable material is embedded in the pores of a rigid porous material. In this structure, 1 is a rigid porous material and 2 is an elastic deformable material. The elastic deformable material 2 is embedded in the pores of the rigid porous material 1, thus connecting the two materials into one.

[0032] According to this invention, the mechanism of the interaction between porous rigid material and elastic material with good deformation capacity is utilized. The elastic material enters the pores of the porous rigid material through deformation to form a whole. They interact within the leakage channel to form a primary sealing layer. Other small particulate materials, fibers and other filling materials are used to seal the small pores left after bridging, and finally an effective sealing layer is formed.

[0033] According to some embodiments of the present invention, the rigid porous material is circular or nearly circular in shape, with a number of pores not less than 50, for example, 50, 60, 70, 80, 90, 100, 120, 150, or any value within the range of any two values, preferably 60-120; the pore diameter is 10-30 μm, for example, 10 μm, 12 μm, 15 μm, 18 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, or any value within the range of any two values.

[0034] According to some embodiments of the present invention, the length of the elastic deformable material is 2-10 mm, and the cross-sectional diameter is 0.5-1 mm, for example, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1 mm, or any value within the range of any two values. According to some embodiments of the present invention, the length of the fiber material is 3-12 mm, for example, 3 mm, 5 mm, 8 mm, 10 mm, 11 mm, 12 mm, or any value within the range of any two values.

[0035] According to some embodiments of the present invention, the particle size of the fine particulate material is 30-50 μm, for example, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, and any value within the range of any two values.

[0036] According to some embodiments of the present invention, the rigid porous material has a hardness of 6.5-7 and a porosity of 50-80%, for example, 50%, 55%, 60%, 65%, 70%, 75%, 80%, and any value within a range of any two values.

[0037] According to some embodiments of the present invention, the rigid porous material is selected from one or more of granular ceramics, honeycomb ceramics, and foam ceramics.

[0038] According to some embodiments of the present invention, the deformation rate of the elastic deformable material is 15-30%, for example 15%, 18%, 20%, 22%, 25%, 28%, 30%, and any value within the range of any two values.

[0039] According to some embodiments of the present invention, the elastic deformable material is selected from one or more of EPDM rubber, silicone rubber, nitrile rubber and tire granules.

[0040] According to some embodiments of the present invention, the fiber material is selected from one or more of polyester fiber, polypropylene fiber, sepiolite fiber and brucite fiber.

[0041] According to some embodiments of the present invention, the fine particulate material is selected from one or more of calcium carbonate powder, silica powder, and mica powder.

[0042] According to some embodiments of the present invention, the backflow index F of the bridging and sealing composition is 0.6-1.8; for example, 0.6, 0.7, 0.8, 1, 1.2, 1.5, 1.7, 1.8, and any value within the range of any two values.

[0043] The return index F is calculated using equation (1).

[0044]

[0045] In formula (1):

[0046] F – Rebate Index, dimensionless;

[0047] T – The weight of elastically deformable material in grams, dimensionless;

[0048] X — Weight of fiber material in grams, dimensionless;

[0049] G – The weight of rigid porous material in grams, dimensionless.

[0050] Φ—Porosity, dimensionless;

[0051] K – The weight of fine particulate material in grams, dimensionless.

[0052] According to this invention, if there are multiple materials, the values ​​need to be calculated separately and then added together. For example, if there are two elastic deformation materials with different elastic deformation rates, the values ​​are calculated separately and then added together, i.e., T×10=T1××10+T2×10.

[0053] According to some embodiments of the present invention, the anti-backflow capability of the bridging and sealing composition is not less than 5 MPa. For example, 5 MPa, 5.1 MPa, 5.2 MPa, 5.3 MPa, 5.4 MPa, 5.5 MPa, 5.6 MPa, 5.7 MPa, 5.8 MPa, 5.9 MPa, 6 MPa, and any value within a range of any two values.

[0054] According to the present invention, the anti-backflow capability of the bridging and sealing composition is the ability to withstand reverse pressure.

[0055] The inventors of this invention have discovered that when the backflow index F of the bridging and sealing composition is between 0.6 and 1.8, its reverse pressure resistance is not less than 5 MPa.

[0056] A second aspect of the present invention provides a bridging and sealing grout, the bridging and sealing grout comprising a base grout and the bridging and sealing composition described in the first aspect above.

[0057] According to the present invention, the bridging and sealing composition can be mixed with the base slurry in the aforementioned proportion to obtain the bridging and sealing slurry. It is only necessary to ensure that a portion of the elastic deformable material is embedded in the pores of the rigid porous material to meet the usage requirements. For example, if the percentage of the number of pores embedded with the elastic deformable material is not less than 30%, it will produce better anti-backflow ability, preferably 30-50%.

[0058] According to some embodiments of the present invention, the base slurry comprises: water, bentonite, and sodium carbonate.

[0059] According to some embodiments of the present invention, based on 100 parts by weight of water, 4-8 parts by weight of bentonite and 0.1-0.5 parts by weight of sodium carbonate, more preferably 0.16-0.48 parts by weight.

[0060] A third aspect of the present invention provides a method for bridging and plugging leaks, the method comprising pumping the bridging and plugging slurry described in the second aspect into the lost well section.

[0061] According to the present invention, after the bridging slurry is pumped into the lost well section, pressure is applied at the wellhead to force the slurry into the lost channel. The rigid porous material and the elastic material interact within the lost channel to generate an effective sealing layer, which isolates the wellbore and the formation, preventing further leakage.

[0062] The fourth aspect of this invention relates to the application of the bridging and plugging composition described in the first aspect, the bridging and plugging slurry described in the second aspect, or the bridging and plugging method described in the third aspect in oil and gas well plugging.

[0063] The bridging and sealing composition of the present invention has a pressure resistance of not less than 10 MPa and a backflow resistance of not less than 5 MPa when used for bridging and sealing. It has a significantly improved backflow resistance compared with conventional bridging and sealing slurries, which can greatly reduce the occurrence of sealing failure accidents caused by the backflow of sealing material due to the suction effect generated during the drilling process.

[0064] According to the present invention, unless otherwise specified, the content of each component is expressed in parts by weight.

[0065] The present invention will be described in detail below through embodiments. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit the present invention.

[0066] Unless otherwise specified in the following examples and comparative examples, all conditions were performed under standard conditions or conditions recommended by the manufacturer. Reagents or instruments used, unless otherwise specified, are all commercially available products.

[0067] The base slurry formulation is as follows: 100 parts by weight of water; 6 parts by weight of bentonite; and 0.25 parts by weight of sodium carbonate (Na2CO3). During preparation, first add sodium carbonate to water and stir at high speed for 5 minutes to ensure complete dissolution; then add bentonite, stir at high speed for 30 minutes, and let stand for 24 hours to allow the bentonite to fully hydrate.

[0068] The experimental apparatus used in the following comparative examples is a DL-2 type leak-stopping simulation device (see CN2866805Y for specific structure). A leak-stopping wall is formed by slow pressurization. After the pressure stabilizes and the leak is successfully plugged, the pressure gauge displays the forward pressure-bearing capacity. Then, the pressure is released, the artificial rock core is removed, and it is inserted back into the working cylinder. Water is slowly applied in the reverse direction to test the reverse pressure-bearing capacity of the leak-stopping wall, i.e., its resistance to backflow. The artificial rock core has a diameter of 100mm and a length of 600mm, and different particle sizes of crushed stone are used to simulate leakage channels. The fabrication process of the artificial rock core is described in CN2900782Y.

[0069] Example 1

[0070] Base paste: 100g;

[0071] Elastic deformation material (EPDM rubber: particle size 2mm, elastic deformation rate 15%): 2g;

[0072] Rigid porous material (honeycomb ceramic: particle size 2mm, hardness 6.5, porosity 50%, pore size 10-30μm): 5g;

[0073] Fiber material (polyester fiber: 3mm in length): 2g;

[0074] Fine particulate material (calcium carbonate powder: particle size 30-50μm): 5g;

[0075] The above materials were added to the base slurry sequentially, and after stirring for 10 minutes, the mixture was added to the DL-2 plugging simulation device. A medium-fine particle core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. Then, the pressure was released, the core cylinder was removed, and it was reversed and loaded into the working cylinder of the plugging simulation device. The base slurry was used to slowly increase the pressure to 5.8 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 5.8 MPa.

[0076] Example 2

[0077] Base paste: 100g;

[0078] Elastic deformable material (nitrile rubber: particle size 3mm, elastic deformation rate 20%): 1g;

[0079] Rigid porous material (honeycomb ceramic: particle size 3mm, hardness 6.5, porosity 60%, pore size 10-30μm): 4g;

[0080] Fiber material (polypropylene fiber: 5mm in length): 2g;

[0081] Fine particulate material (silica powder: particle size 30-50μm): 6g;

[0082] The above materials were added to the base slurry sequentially and stirred for 10 minutes. Then, the mixture was added to the DL-2 plugging simulation device. A medium-fine particle core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. After depressurization, the core cylinder was removed and placed in reverse into the working cylinder of the plugging simulation device. The base slurry was then used to slowly increase the pressure to 5.6 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 5.6 MPa.

[0083] Example 3

[0084] Base paste: 100g;

[0085] Elastic deformable material (silicone rubber: particle size 5mm, elastic deformation rate 25%): 2g;

[0086] Rigid porous material (foam ceramic: particle size 5mm, hardness 7.0, porosity 80%, pore size 10-30μm): 4g;

[0087] Fiber material (sepiolite fiber: 8mm in length): 3g;

[0088] Fine particulate material (mica powder: particle size 30-50μm): 7g;

[0089] The above materials were added to the base slurry sequentially, and after stirring for 10 minutes, the mixture was added to the DL-2 plugging simulation device. A medium-coarse particle core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. Then, the pressure was released, the core cylinder was removed, and it was repositioned into the working cylinder of the plugging simulation device. The base slurry was used to slowly increase the pressure to 5.5 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 5.5 MPa.

[0090] Example 4

[0091] Base paste: 100g;

[0092] Elastic deformable material (tire particles: particle size 8mm, elastic deformation rate 30%): 2g;

[0093] Rigid porous material (granular ceramic: particle size 8mm, hardness 7.0, porosity 60%, pore size 10-30μm): 5g;

[0094] Fiber material (polyester fiber: 10mm in length): 3g;

[0095] Fine particulate material (calcium carbonate powder: particle size 30-50μm): 8g;

[0096] The above materials were added to the base slurry sequentially and stirred for 10 minutes. Then, the mixture was added to the DL-2 plugging simulation device. A medium-coarse particle core was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. After depressurization, the core was removed and placed in reverse into the working cylinder of the plugging simulation device. The base slurry was then used to slowly increase the pressure to 5.6 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 5.6 MPa.

[0097] Example 5

[0098] Base paste: 100g;

[0099] Elastic material (nitrile rubber: particle size 10mm, elastic deformation rate 20%): 3g;

[0100] Rigid porous material (foam ceramic: particle size 10mm, hardness 7.0, porosity 70%, pore size 10-30μm): 3g;

[0101] Fiber material (brucite fiber: 12mm in length): 3g;

[0102] Fine particulate material (calcium carbonate powder: particle size 30-50μm): 8g;

[0103] The above materials were added to the base slurry sequentially, and after stirring for 10 minutes, the mixture was added to the DL-2 plugging simulation device. A coarse-grained core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. Then, the pressure was released, the core cylinder was removed, and it was reversed and placed into the working cylinder of the plugging simulation device. The base slurry was used to slowly increase the pressure to 5.7 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 5.7 MPa.

[0104] Comparative Example 1

[0105] Base paste: 100g;

[0106] Elastic deformation material (EPDM rubber: particle size 2mm, elastic deformation rate 15%): 2g;

[0107] Rigid material (walnut shells: particle size 2mm, hardness 3.5): 5g;

[0108] Fiber material (polyester fiber: 3mm in length): 2g;

[0109] Fine particulate material (calcium carbonate powder: particle size 30-50μm): 5g;

[0110] The above materials were added to the base slurry sequentially and stirred for 10 minutes. Then, the mixture was added to the DL-2 plugging simulation device. A medium-fine particle core cylinder was used as the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. After depressurization, the core cylinder was removed and placed in reverse into the working cylinder of the plugging simulation device. The base slurry was then used to slowly increase the pressure to 1.1 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 1.1 MPa.

[0111] Comparative Example 2

[0112] Base paste: 100g;

[0113] Rigid porous material (honeycomb ceramic: particle size 2mm, hardness 6.5, porosity 50%, pore size 10-30μm): 5g;

[0114] Fiber material (polyester fiber: 3mm in length): 2g;

[0115] Fine particulate material (calcium carbonate powder: particle size 30-50μm): 5g;

[0116] The above materials were added to the base slurry sequentially and stirred for 10 minutes. Then, the mixture was added to the DL-2 plugging simulation device. A medium-fine particle core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. After depressurization, the core cylinder was removed and placed in reverse into the working cylinder of the plugging simulation device. The base slurry was then used to slowly increase the pressure to 0.4 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 0.4 MPa.

[0117] Comparative Example 3

[0118] Base paste: 100g;

[0119] Elastic deformable material (nitrile rubber: particle size 3mm, elastic deformation rate 20%): 1g;

[0120] Rigid material (walnut shells: particle size 3mm, hardness 3.5): 4g;

[0121] Fiber material (polypropylene fiber: 8mm in length): 2g;

[0122] Fine particulate material (silica powder: particle size 30-50μm): 6g;

[0123] The above materials were added to the base slurry sequentially, and after stirring for 10 minutes, the mixture was added to the DL-2 plugging simulation device. A medium-coarse particle core cylinder was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. Then, the pressure was released, the core cylinder was removed, and it was reversed and placed into the working cylinder of the plugging simulation device. The base slurry was used to slowly increase the pressure to 1.0 MPa. The pressure suddenly dropped to 0, and the anti-backflow capability was 1.0 MPa.

[0124] Comparative Example 4

[0125] Base paste: 100g;

[0126] Rigid material (walnut shells: particle size 5mm, hardness 3.5): 2g;

[0127] Rigid material (walnut shells: particle size 3mm, hardness 3.5): 3g;

[0128] Rigid material (walnut shells: particle size 1mm, hardness 3.5): 5g;

[0129] Fiber material (polyester fiber: 8mm in length): 2g;

[0130] Fine particulate material (mica powder: particle size 30-50μm: 5g);

[0131] The above materials were added to the base slurry sequentially and stirred for 10 minutes. Then, the mixture was added to the DL-2 plugging simulation device. A medium-coarse particle core was used for the artificial core. The pressure was slowly increased to 10 MPa and maintained for 10 minutes without dropping. After depressurization, the core was removed and placed in reverse into the working cylinder of the plugging simulation device. The base slurry was then used to slowly increase the pressure to 0.7 MPa. The pressure suddenly dropped to 0, indicating an anti-backflow capability of 0.7 MPa.

[0132] The detection results of Examples 1-5 and Comparative Examples 1-4 are shown in Table 1.

[0133] The backflow index F of Examples 1-5 and Comparative Examples 1-4 above was calculated according to formula (1). (In the comparative examples, the hardness of the walnut shell is only 3.5. It has relatively more micropores and mesopores and fewer macropores. The average pore size is about 10-20 nm. It is difficult for elastic materials to enter such small pores. Therefore, the porosity of the walnut shell is taken as 0% when calculating the backflow index F.) as shown in Table 1.

[0134] Table 1

[0135]

[0136]

[0137] As can be seen from the results in Table 1, under the same forward pressure of 10 MPa, the reverse pressure of the bridging and sealing compositions obtained in Examples 1-5 of the present invention is greater than 5 MPa, while the reverse pressure of the bridging and sealing compositions obtained in Comparative Examples 1-4 is not greater than 1.1 MPa.

[0138] As can be seen from the above, the backflow index of the bridging and sealing compositions obtained in Examples 1-5 of the present invention is in the range of 0.6-1.8, and their reverse pressure resistance is greater than 5 MPa; while the backflow index of the bridging and sealing compositions obtained in Comparative Examples 1-4 is not in the range of 0.6-1.8, and their reverse pressure resistance is not greater than 1.1 MPa. Therefore, the bridging and sealing compositions of the present invention have significantly better backflow resistance.

[0139] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A bridging and sealing composition, characterized in that, The bridging and sealing composition comprises a rigid porous material, an elastic deformable material, a fiber material, and a fine particulate material; wherein the weight ratio of the rigid porous material, the elastic deformable material, the fiber material, and the fine particulate material is 1:0.1-0.8:0.2-1:1-2; and the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:15-100.

2. The bridging and sealing composition according to claim 1, wherein, The weight ratio of the rigid porous material, elastic deformable material, fiber material, and fine particulate material is 1:0.2-0.5:0.4-0.8:1-1.6; And / or, the ratio of the pore size of the rigid porous material to the cross-sectional diameter of the elastic deformable material is 1:50-80.

3. The bridging and sealing composition according to claim 1 or 2, wherein, At least a portion of the elastically deformable material is embedded in the pores of the rigid porous material; Preferably, based on the total number of pores in the rigid porous material, the percentage of pores embedded with the elastic deformable material is not less than 30%, and more preferably 30-50%. Preferably, the fibrous material and fine particulate material fill the voids formed by the combination of the rigid porous material and the elastic deformable material.

4. The bridging and sealing composition according to any one of claims 1-3, wherein, The rigid porous material is circular or near-circular in shape, with no less than 50 pores and a pore diameter of 10-30 μm. And / or, the length of the elastic deformable material is 2-10 mm, and the cross-sectional diameter is 0.5-1 mm; And / or, the length of the fiber material is 3-12 mm; And / or, the particle size of the fine particulate material is 30-50 μm.

5. The bridging and sealing composition according to any one of claims 1-4, wherein, The rigid porous material has a hardness of 6.5-7 and a porosity of 50-80%. Preferably, the rigid porous material is selected from one or more of granular ceramics, honeycomb ceramics, and foam ceramics.

6. The bridging and sealing composition according to any one of claims 1-5, wherein, The deformation rate of the elastic deformable material is 15-30%; Preferably, the elastic deformable material is selected from one or more of EPDM rubber, silicone rubber, nitrile rubber, and tire granules.

7. The bridging and sealing composition according to any one of claims 1-6, wherein, The fiber material is selected from one or more of polyester fiber, polypropylene fiber, sepiolite fiber and brucite fiber.

8. The bridging and sealing composition according to any one of claims 1-7, wherein, The fine particulate material is selected from one or more of calcium carbonate powder, silica powder, and mica powder.

9. The bridging and sealing composition according to any one of claims 1-8, wherein, The backflow index F of the bridging and sealing composition is 0.6-1.8; The return index F is calculated using equation (1). In formula (1): F – Rebate Index, dimensionless; T – Weight fraction of elastically deformable material, dimensionless; X — weight fraction of fiber material, dimensionless; G – Parts by weight of rigid porous material, dimensionless; Φ—Porosity, %; K – Parts by weight of fine-particle material, dimensionless.

10. The bridging and sealing composition according to any one of claims 1-9, wherein, The reverse pressure withstand capability of the bridging and sealing composition is not less than 5 MPa.

11. A bridging and sealing grout, characterized in that, The bridging and sealing grout comprises a base grout and the bridging and sealing composition according to any one of claims 1-10.

12. The bridging and sealing grout according to claim 11, wherein, The base slurry comprises: water, bentonite, and sodium carbonate; Preferably, based on 100 parts by weight of water, the bentonite is 4-8 parts by weight and the sodium carbonate is 0.1-0.5 parts by weight.

13. A method for bridging and sealing leaks, characterized in that, The method includes pumping the bridging plugging slurry of claim 11 or 12 into the lost well section.

14. The application of the bridging and plugging composition according to any one of claims 1-10, the bridging and plugging slurry according to claim 11 or 12, or the bridging and plugging method according to claim 13 in oil and gas well plugging.

Citation Information

Patent Citations

  • Bridging plugging method and application thereof

    CN115806808A

  • Drilling well leakage plugging simulating experimental instrument

    CN2866805Y

  • Device for producing large size artificial rock core for analogue drilling block

    CN2900782Y