A self-consolidating composite resin sealant, its preparation method and application

By using a self-consolidating composite resin sealant, a three-dimensional cross-linked network is formed through thermal polycondensation and chemical bonding. Combined with expandable graphite and fiber reinforcement, the stability and retention capacity of resin sealant materials under high temperature and high pressure conditions are solved, achieving a highly efficient sealing effect.

CN123063155APending Publication Date: 2026-11-10CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611579085.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing resin-based sealing materials lack stability under high temperature and high pressure conditions, have poor self-filling effect, poor retention capacity, and low curing strength, making it difficult to achieve effective sealing over a long period of time.

Method used

A self-consolidating composite resin sealant is used, which includes water-soluble phenolic resin, toughening resin, reinforcing filler, high-temperature stabilizing material and adaptive retention material. It forms a three-dimensional cross-linked network through thermal polycondensation and chemical bonding, and combines expandable graphite to construct a temperature-responsive retention-consolidation system. The reinforcing fibers provide compressive and shear strength, and the rheological function adjustment material improves dispersibility.

Benefits of technology

It achieves good dispersion stability under high temperature and high pressure conditions, high temperature pumpability and delayed consolidation performance, can adaptively fill and reside in large-scale cracks for a long time, and has high solidification strength, thus achieving long-term effective sealing of high temperature and high pressure leakage formations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063155A_ABST
    Figure CN123063155A_ABST
Patent Text Reader

Abstract

This invention provides a self-consolidating composite resin plugging agent, its preparation method, and its application, belonging to the field of drilling fluid leakage prevention and plugging technology. The plugging agent of this invention is prepared from the following raw materials in the indicated mass fractions: 35-50 wt% self-consolidating composite resin, 0.5-1.5 wt% high-temperature stabilizing material, 8-18 wt% reinforcing filler material, 2-8 wt% self-adaptive retention material, 2-5 wt% rheology regulating material, and the balance being water, with the total content of all components being 100%. The self-consolidating composite resin plugging agent of this invention exhibits good dispersion stability, high-temperature pumpability, and delayed consolidation performance. It can self-adaptively fill and remain in large-scale fractures for extended periods, has high curing strength, and can achieve long-term effective plugging of high-temperature, high-pressure leaking formations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a self-consolidating composite resin plugging agent, its preparation method and application, belonging to the field of drilling fluid leak prevention and plugging technology. Background Technology

[0002] Encountering fractured, porous, or highly permeable heterogeneous formations with lost circulation during drilling operations is a common technical challenge. Significant drilling fluid loss not only causes substantial economic losses and delays in the drilling cycle, but can also induce serious downhole accidents such as wellbore instability and stuck pipe, even leading to well abandonment. Therefore, efficient and reliable plugging technology is one of the key guarantees for safe and economical drilling.

[0003] Curable plugging materials are one of the commonly used and effective materials for controlling severe well leakage caused by fractures. Resin-based plugging materials, as curable plugging materials, are divided into thermosetting resins and thermoplastic resins. Thermosetting resins, under the influence of curing agents and temperature, have small-molecule monomers polymerize and cross-link to form a three-dimensional network structure, which can form a rigid plug with a certain strength and bond integrally with the formation within the leakage channel. Thermoplastic resins soften at high temperatures; under pressure, the softened resin particles further undergo molecular chain diffusion and entanglement, forming a flexible solidified body with a certain strength and viscoelasticity within the fracture.

[0004] Chinese patent document CN121064805A discloses a self-consolidating plugging agent, its preparation method, and drilling fluid. This plugging agent is prepared by coating aggregate materials, high-temperature resistant fibers, plugging supplementary materials, and water-swellable materials with a thermosetting resin (resin physically mixed with a curing agent) at low temperatures, and then compounding the coated materials according to a certain ratio. Chinese patent document CN121064810A discloses a self-consolidating plugging material, its preparation method, and its application. The raw materials for preparing the self-consolidating plugging material include: fatty acid esters, sulfur, resin, curing agent, organic solvent, rigid aggregate, fiber, water-absorbing and swelling material, plugging supplementary material, and dispersant. The plugging agents involved in the above patents exhibit poor long-term thermal stability and mechanical property retention under ultra-high temperature (>200℃) conditions; their self-adaptive filling ability relies on a single water-swellable or water-absorbing and swelling material, lacking particle size distribution design for different crack sizes, making it difficult to achieve a "synergistic sealing effect of expansion filling and resin consolidation" for large-scale cracks.

[0005] Currently, commonly used resin-based plugging materials suffer from poor dispersion stability due to particle agglomeration, failing to form a dense and uniform sealing layer after curing in leakage channels. When a single resin plugging material enters a leakage channel with a large crack width, it quickly settles to the bottom of the crack due to gravity, failing to fully fill laterally and remain firmly within the leakage channel. Furthermore, single resin plugging materials lack sufficient thermal stability in high-temperature and high-pressure formations, and their curing strength decreases with prolonged sealing time, making it difficult to achieve long-term effective sealing of high-temperature and high-pressure leakage formations.

[0006] Therefore, it is necessary to develop a new type of resin plugging material with strong dispersion stability, good high temperature stability, strong retention ability, and high curing strength. Summary of the Invention

[0007] To address the shortcomings of existing technologies, particularly the insufficient high-temperature stability, poor self-filling effect, poor retention capacity, and low sealing strength of conventionally used single-resin plugging materials, this invention provides a self-consolidating composite resin plugging agent, its preparation method, and its application. The self-consolidating composite resin plugging agent of this invention exhibits good dispersion stability, high-temperature pumpability, and delayed consolidation properties. It can self-fill and remain in large-scale cracks for extended periods, and possesses high curing strength, enabling long-term effective sealing of high-temperature, high-pressure leaking formations.

[0008] The technical solution of the present invention is as follows:

[0009] A self-consolidating composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 35-50 wt% self-consolidating composite resin, 0.5-1.5 wt% high-temperature stable material, 8-18 wt% reinforcing filler material, 2-8 wt% adaptive retention material, 2-5 wt% rheology modifier material, and the balance being water, with the total content of all components being 100%.

[0010] The preparation method of the self-consolidating composite resin includes the following steps: fully dissolving water-soluble phenolic resin and toughening resin in a solvent, evaporating the solvent, degassing, pulverizing, and sieving to obtain the self-consolidating composite resin; the toughening resin is selected from one or two of polyamide, liquid nitrile rubber, liquid carboxylated nitrile rubber, or tetrafunctional epoxy resin.

[0011] According to the present invention, a preferred method for preparing water-soluble phenolic resin includes the following steps: in the presence of an alkali, an antioxidant, and a modifier, phenol and an aqueous formaldehyde solution undergo an addition and condensation reaction to obtain a water-soluble methyl phenolic resin solution; then, the solution is neutralized, stabilized, filtered, and dried to obtain the water-soluble phenolic resin.

[0012] Preferably, the alkali is one of ammonia, triethylamine, or hexamethylenetetramine with a mass concentration of 5%-25%; the pH of the system is controlled to be 8.5-10.0 by adding the alkali.

[0013] Preferably, the antioxidant is sodium bisulfite, and the mass of the antioxidant is 0.1wt%-0.3wt% of the mass of phenol.

[0014] Preferably, the modifier is urea, and the mass of the modifier is 10wt%-25wt% of the mass of phenol.

[0015] Preferably, the mass concentration of the formaldehyde aqueous solution is 37%-40%; the molar ratio of phenol to formaldehyde is 1:1.8-2.2.

[0016] Preferably, the addition reaction temperature is 55-65℃ and the addition reaction time is 30-60 min; the polycondensation reaction temperature is 75-85℃ and the polycondensation reaction time is 40-80 min.

[0017] Preferably, the water-soluble methyl phenolic resin solution has a viscosity of 15-30 s at 25°C in a Forck-4 cup, and can be dispersed in water at 25-60°C at a mass ratio of 1:3 to obtain a clear, oil-free system.

[0018] Preferably, neutralization is performed using an aqueous solution of formic acid, acetic acid, or phosphoric acid to neutralize the system to a pH of 7.0-8.0.

[0019] Preferred stabilization method is as follows: add sodium bisulfite or ascorbic acid to the system and mix thoroughly; the mass of sodium bisulfite or ascorbic acid is 0.05%-0.2% of the mass of the water-soluble methyl phenolic resin solution.

[0020] Preferably, the drying is spray drying or vacuum drying; the spray drying conditions are: inlet air temperature 120-150℃, outlet air temperature 65-85℃, atomization method is pressure atomization or centrifugal atomization, and the particle size of the resulting water-soluble phenolic resin is 20-80μm; the vacuum drying method is: first concentrate to a solid content of 80wt%-85wt% at 50-65℃ and -0.08-(-0.09)MPa, then dry at 45-60℃ and vacuum degree ≤-0.095MPa, cool and pulverize, and pass through an 80-200 mesh sieve to obtain water-soluble phenolic resin.

[0021] According to the present invention, the water-soluble phenolic resin is a white powder, soluble in cold water at 25°C, with a solid content ≥95wt% and a moisture content of 1.5wt%-3.0wt%.

[0022] According to the present invention, preferably, the mass ratio of water-soluble phenolic resin to toughening resin is 4-20:1-3.

[0023] According to the present invention, preferably, the polyamide is a tough, angular, translucent or milky white solid particle with a weight-average molecular weight of 10,000-20,000.

[0024] According to the present invention, preferably, the liquid nitrile rubber is a slightly yellow, transparent, viscous liquid, free of mechanical impurities, with a number average molecular weight of 1,000-10,000 and an acrylonitrile content of 18wt%-40wt%.

[0025] According to the present invention, preferably, the liquid carboxylated nitrile rubber is a pale yellow to amber transparent viscous liquid; the carboxyl content is 0.5wt%-3.0wt%; and the number average molecular weight is 5,000-15,000.

[0026] According to the present invention, preferably, the tetrafunctional epoxy resin is a yellow to amber transparent liquid; the epoxy equivalent is 100-200 g / eq; and the viscosity (125°C) is 0.5-2.0 Pa·s.

[0027] According to the present invention, preferably, the solvent is anhydrous ethanol; the mass of the solvent is 1-5 times the total mass of the water-soluble phenolic resin and the toughening resin.

[0028] According to the present invention, the preferred conditions for evaporating the solvent are as follows: stirring at 40-80°C for 1-6 hours.

[0029] According to the present invention, preferably, the sieving is performed through a 100-mesh sieve.

[0030] According to the present invention, preferably, the high-temperature stable material is one or a combination of two of ultrafine alumina, water-soluble nano-silica, or boron carbide; the ultrafine alumina has a purity ≥99.9%, a particle size of 20-50 nm, a crystal form of α-Al₂O₃ or γ-Al₂O₃, and a specific surface area of ​​15-40 m². 2 / g; the particle size of water-soluble nano-silica is 10-50nm; the particle size of boron carbide is 20-50nm. Preferably, the high-temperature stable material is a combination of ultrafine alumina and water-soluble nano-silica, with a mass ratio of ultrafine alumina to water-soluble nano-silica of 1:1-10; or a combination of ultrafine alumina and boron carbide, with a mass ratio of ultrafine alumina to boron carbide of 1:3-15; or a combination of water-soluble nano-silica and boron carbide, with a mass ratio of water-soluble nano-silica to boron carbide of 1:0.5-5.

[0031] According to the present invention, preferably, the reinforcing filler material is one or a combination of two of E-glass fiber, S-glass fiber, or graphite fiber. Preferably, the E-glass fiber has a single filament diameter of 5-20 μm, a length of 3-15 mm, a tensile strength of 2200-2800 MPa, and an elastic modulus of 72-80 GPa. The S-glass fiber has a single filament diameter of 7-15 μm, a length of 5-10 mm, a tensile strength of 3000-4000 MPa, and an elastic modulus of 86-95 GPa. The graphite fiber has a single filament diameter of 5-8 μm, a length of 4-6 mm, a tensile strength of 3000-3500 MPa, an elastic modulus of 250-300 GPa, and a carbon content ≥95%, preferably ≥98%.

[0032] Preferably, the reinforcing filler material is a combination of E-glass fiber and S-glass fiber, with a mass ratio of E-glass fiber to S-glass fiber of 1:0.5-2; or a combination of E-glass fiber and graphite fiber, with a mass ratio of E-glass fiber to graphite fiber of 1:0.3-1.5; or a combination of S-glass fiber and graphite fiber, with a mass ratio of S-glass fiber to graphite fiber of 1:0.5-2.

[0033] According to the present invention, preferably, the adaptive retention material is expandable graphite. Preferably, the initial expansion temperature of expandable graphite is 160-220°C.

[0034] Preferably, the expandable graphite has a particle size of 30 mesh, 50 mesh and 80 mesh expandable graphite, and the mass ratio of 30 mesh, 50 mesh and 80 mesh expandable graphite is 1:(0.5-0.6):(0.5-0.6).

[0035] Preferably, the expansion ratio of the 30-mesh expandable graphite is 250-400 mL / g, the expansion ratio of the 50-mesh expandable graphite is 220-300 mL / g, and the expansion ratio of the 80-mesh expandable graphite is 180-250 mL / g.

[0036] According to the present invention, preferably, the rheological function regulating material is a mixture of polyvinyl alcohol and lithium-based bentonite, wherein the mass ratio of polyvinyl alcohol to lithium-based bentonite is 2-4:1.

[0037] Preferably, the particle size D of the lithium-based bentonite is... 50 It is 30-50nm.

[0038] The preparation method of the above-mentioned self-consolidating composite resin sealant includes the following steps:

[0039] The rheological function regulating material is fully dispersed in water; a high-temperature stabilizing material is added and fully dispersed; a self-consolidating composite resin is added and fully dispersed; then an adaptive retention material and a reinforcing filler are added and fully dispersed to obtain a self-consolidating composite resin sealant.

[0040] The above-mentioned self-consolidating composite resin plugging agent is used in drilling fluid plugging.

[0041] The technical features and beneficial effects of this invention are as follows:

[0042] 1. The main principle of self-consolidation in this invention lies in the following: The water-soluble thermosetting phenolic resin used is a thermosetting phenolic resin containing active hydroxymethyl groups. Under conditions of 160–220°C, the hydroxymethyl groups in the resin molecules can undergo further condensation reactions, gradually forming a three-dimensional cross-linked network with methylene bridges and methylene ether bridges as the main connecting structures. This allows the system to achieve thermal consolidation without the need for additional conventional phenolic resin curing agents. Simultaneously, the toughening resin can participate in the curing and toughening process of the phenolic resin through chemical reactions or intermolecular interactions. The self-consolidation process of this invention is mainly driven by the thermosetting phenolic resin's own thermal condensation reaction, supplemented by chemical bonding, interfacial interactions, and molecular chain entanglement of different reactive or flexible modified components. This allows flexible segments or flexible rubber phases to be distributed within the rigid phenolic cross-linked network, reducing the brittleness of a single highly cross-linked phenolic resin while ensuring consolidation strength and high-temperature stability. This balances the self-consolidation performance, toughness, and high-temperature stability of the sealing material.

[0043] 2. This invention introduces a high-temperature stable material, which is uniformly dispersed in the resin matrix at the nanoscale, significantly improving the high-temperature aging resistance of the sealant. A nano- to micro-level reinforcing network is formed between the high-temperature stable material and the self-consolidating composite resin, effectively inhibiting the thermal motion and degradation of the resin molecular chains at high temperatures, enabling the sealant to maintain high mechanical strength and structural integrity even above 220°C.

[0044] 3. This invention constructs a temperature-responsive retention-consolidation system using expandable graphite and a self-consolidating composite resin with thermal consolidation properties. The plugging agent maintains good dispersibility and flowability during preparation, surface delivery, and wellbore pumping, without significant volume expansion or rapid consolidation, thus meeting the requirements for plugging slurry preparation and pumping. As the plugging agent enters the high-temperature lost circulation zone and continues to be heated, the expandable graphite gradually expands in volume, improving the material's filling degree and retention capacity in cracks and pores. Simultaneously, the self-consolidating composite resin gradually undergoes further polycondensation and cross-linking reactions under high-temperature conditions, transforming the dispersed plugging material into a consolidated sealing body with a certain overall strength.

[0045] 4. This invention constructs a fiber-reinforced skeleton-resin matrix composite structure by combining reinforcing filler materials with self-consolidating composite resin. The reinforcing fibers provide compressive and shear strength, while the resin matrix provides bonding and sealing properties. The combined effect enables the sealant to achieve a compressive strength of 20-30 MPa.

[0046] 5. The self-consolidating composite resin sealant prepared by this invention is a water-based dispersion slurry. The product can be pre-made and used directly on site. The construction process is simple, avoiding complex procedures and significantly reducing the operational difficulty and risk of high-temperature sealant operations.

[0047] 6. This invention employs rheologically modulating materials to improve the suspension stability and dispersion performance of the plugging system. Polyvinyl alcohol (PVA), when dissolved in water, increases the viscosity of the continuous phase and forms interfacial interactions such as hydrogen bonds with the resin and inorganic material surfaces through the hydroxyl groups on its molecular chains. Lithium-based bentonite undergoes hydration and interlayer expansion in water, forming a dispersion system with a certain spatial network structure, thereby improving the suspension stability of the plugging material and slowing down the sedimentation of larger particles and fibers. The interaction between PVA and lithium-based bentonite improves the dispersion uniformity of self-consolidating composite resins, reinforcing fillers, and self-retaining materials in the aqueous phase.

[0048] 7. The plugging agent of this invention is prepared by combining specific types of raw materials in specific proportions to obtain the specific composition and structure of this invention. The components of the plugging agent of this invention play complex roles, resulting in good dispersion stability, high-temperature pumpability and delayed consolidation performance. It can adaptively fill and remain in large-scale cracks for a long time, has high curing strength, and can achieve long-term effective sealing of high-temperature and high-pressure leaking formations. Attached Figure Description

[0049] Figure 1 The infrared spectrum of the water-soluble phenolic resin prepared by the method in Example 1 is shown. Detailed Implementation

[0050] The present invention will be further described below through specific embodiments, but is not limited thereto.

[0051] All raw materials used in the embodiments are conventional and commercially available; unless otherwise specified, the methods described are existing technologies.

[0052] Example 1

[0053] A self-curing composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 42 wt% self-curing composite resin, 1.0 wt% high-temperature stable material, 12 wt% reinforcing filler material, 5 wt% self-adaptive retention material, 3.5 wt% rheology modifier material, and the balance being water. The total content of all components is 100%.

[0054] The preparation method of the self-consolidating composite resin includes the following steps:

[0055] (1) Dissolve water-soluble phenolic resin and polyamide resin separately in anhydrous ethanol (the amount of anhydrous ethanol is 3 times the mass of the resin), to obtain solutions A1 and A2. The mass ratio of water-soluble phenolic resin to polyamide resin is 12:2. The polyamide resin is a tough, angular, translucent solid particle with a weight-average molecular weight of 15,000 and a density of 1.1 g / cm³. 3 It has a melting point of 205℃ and a water absorption rate (23℃, 50%RH) of 2.0wt%.

[0056] (2) Mix solutions A1 and A2 and stir at a stirring speed of 500 r / min to make the resin blend completely and evenly mixed to obtain mixture B.

[0057] (3) Mixture B is stirred at 60°C and 500r / min for 3 hours to evaporate most of the anhydrous ethanol (ethanol residue ≤5wt%). At this time, the system changes from liquid to semi-solid. Then it is transferred to a vacuum oven and degassed at 50°C and vacuum degree -0.08 to -0.09MPa for 30 minutes. The trapped bubbles are removed by ultrasonic treatment for 20 minutes.

[0058] (4) After cooling, crush it in a universal crusher and pass it through a 100-mesh sieve to obtain self-consolidated composite resin powder.

[0059] The preparation method of the water-soluble phenolic resin includes the following steps:

[0060] (1) Sodium bisulfite (0.2 wt% of phenol), urea (18 wt% of phenol), phenol and formaldehyde aqueous solution with a mass concentration of 37% (molar ratio of phenol to formaldehyde of 1:2.0) were thoroughly mixed. Ammonia water with a mass concentration of 10% was added to adjust the pH of the reaction system to 9.0. The reaction was first carried out at 60℃ for 45 min, and then heated to 80℃ for 60 min to obtain water-soluble methyl phenolic resin solution. The viscosity of the resin solution at 25℃ was 22s in a 4-cup container, and it could be dispersed in water at 40℃ in a clear, oil-free system with a mass ratio of water-soluble methyl phenolic resin solution to water of 1:3.

[0061] (2) Neutralize to pH 7.5 with acetic acid at a mass concentration of 10% and the neutralization temperature is not higher than 50℃. After treatment, cool rapidly to not higher than 35℃, add sodium bisulfite stabilizer at a mass of 0.1% of the water-soluble phenolic resin liquid, stir at 30℃ and 300r / min for 20 min, and filter to obtain a light-colored drier resin liquid.

[0062] (3) The drier resin liquid is spray-dried (inlet air temperature 135℃, outlet air temperature 75℃, atomization method is centrifugal atomization) to obtain a white powder of water-soluble thermosetting phenolic resin with a particle size of 50 μm. Solid content ≥95wt%, moisture 1.8wt%.

[0063] Fourier transform infrared spectroscopy analysis was performed on the prepared water-soluble phenolic resin, and the results are as follows: Figure 1 As shown in the figure. It can be seen from the figure that at approximately 3380cm... -1 A broad, strong absorption peak appears at approximately 2925 cm⁻¹, mainly attributed to the stretching vibrations of the OH groups in the phenolic hydroxyl and hydroxymethyl groups, and possibly superimposed by the stretching vibrations of the NH groups in the system; -1 The absorption peak at approximately 1605 cm⁻¹ mainly corresponds to the CH stretching vibration of aliphatic -CH₂-. -1 The presence of a characteristic peak for the C=C stretching vibration of the benzene ring skeleton at approximately 1455 cm⁻¹ indicates that the resin retains the aromatic ring skeleton of the phenolic structure; -1 The absorption peak at approximately 1235 cm⁻¹ is mainly related to the bending vibration of -CH₂- and the methylene bridge structure; -1 The absorption peak at approximately 10¹⁰ cm⁻¹ can be attributed to the stretching vibration of the phenolic hydroxyl group (CO); while the peak at approximately 10¹⁰ cm⁻¹... -1 The characteristic absorption peak at the specified location mainly corresponds to the CO stretching vibration in hydroxymethyl-CH2OH. These characteristic peaks indicate that phenol and formaldehyde underwent hydroxymethylation and a certain degree of condensation polymerization under alkaline conditions. The resulting product exhibits the typical structural characteristics of methyl phenolic resins and retains a significant amount of hydroxymethyl groups with subsequent reactivity, providing a structural basis for further condensation polymerization, crosslinking, and the formation of a three-dimensional solidified network under high-temperature conditions.

[0064] The high-temperature stable material is a combination of high-purity ultrafine alumina and water-soluble nano-silica, with a mass ratio of 1:5. The high-purity ultrafine alumina has a purity ≥99.9%, a particle size of 30 nm, a crystal form of α-Al₂O₃, and a specific surface area of ​​20 m² / g; the water-soluble nano-silica has a particle size of 30 nm.

[0065] The reinforcing filler material is a combination of E-glass fiber and S-glass fiber in a mass ratio of 1:1. The E-glass fiber has a single filament diameter of 12μm, a length of 8mm, a tensile strength of 2500MPa, and an elastic modulus of 75GPa; the S-glass fiber has a single filament diameter of 10μm, a length of 8mm, a tensile strength of 3600MPa, and an elastic modulus of 90GPa.

[0066] The adaptive retention material is expandable graphite with an initial expansion temperature of 160℃ and a sulfur content ≤0.03%. The expandable graphite has a particle size distribution of 30 mesh, 50 mesh, and 80 mesh, in a mass ratio of 1:0.55:0.55. The expansion ratio of 30 mesh expandable graphite is 300 mL / g, that of 50 mesh expandable graphite is 280 mL / g, and that of 80 mesh expandable graphite is 200 mL / g.

[0067] The rheological function modifier is polyvinyl alcohol (weight average molecular weight 15000) and lithium-based bentonite (montmorillonite content ≥90wt%). 50 A mixture of particles with a density of 30 nm (in 2:1 mass ratio) was prepared.

[0068] The preparation method of the above-mentioned self-consolidating composite resin sealant includes the following steps:

[0069] (1) Lithium-based bentonite was added to water and dispersed at 1000 rpm for 15 minutes at room temperature to ensure full hydration; then polyvinyl alcohol was added and dispersion was continued for 5 minutes to obtain dispersion A;

[0070] (2) The high-temperature stable material was slowly added to the dispersion A and dispersed at 40°C and 1500 rpm for 15 minutes; the self-consolidating composite resin was added and mixed at 1000 rpm for 10 minutes; the rotation speed was reduced to 500 rpm, and the adaptive retention material and reinforcing filler material were added in sequence and mixed for another 15 minutes to obtain the self-consolidating composite resin plugging agent sample B1.

[0071] Example 2

[0072] A self-curing composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 35 wt% self-curing composite resin, 1.5 wt% high-temperature stable material, 15 wt% reinforcing filler material, 8 wt% self-adaptive retention material, 2 wt% rheology modifier material, and the balance being water, with the total content of all components being 100%.

[0073] The preparation method of the self-consolidating composite resin is the same as in Example 1, except that: in step (1), the polyamide resin is replaced with liquid nitrile rubber, which is a slightly yellow, transparent, viscous liquid with no mechanical impurities, a number-average molecular weight of 5000, an acrylonitrile content of 28wt%, and a viscosity (25℃) of 5 Pa·s; the mass ratio of water-soluble phenolic resin to liquid nitrile rubber is 5:1; and the amount of anhydrous ethanol used is 1 times the mass of the resin. Step (2) is the same as in Example 1, and in step (3), the stirring temperature of the volatile solvent is 80℃ and the stirring time is 1 hour.

[0074] The preparation method of the water-soluble phenolic resin is the same as in Example 1.

[0075] The high-temperature stable material is a combination of high-purity ultrafine alumina and boron carbide, with a mass ratio of 1:10. The high-purity ultrafine alumina has a purity ≥99.9%, a particle size of 20 nm, a crystal form of γ-Al₂O₃, and a specific surface area of ​​40 m² / g; the boron carbide has a particle size of 50 nm.

[0076] The reinforcing filler material is a combination of E-glass fiber and graphite fiber, with a mass ratio of 1:0.5. The E-glass fiber has a single filament diameter of 20 μm, a length of 15 mm, a tensile strength of 2200 MPa, and an elastic modulus of 72 GPa; the graphite fiber has a single filament diameter of 8 μm, a length of 6 mm, a tensile strength of 3000 MPa, an elastic modulus of 250 GPa, and a carbon content of 98%.

[0077] The adaptive retention material is expandable graphite with an initial expansion temperature of 160℃. The expandable graphite has a particle size distribution of 30 mesh, 50 mesh, and 80 mesh, in a mass ratio of 1:0.5:0.6. The expansion ratio of 30 mesh expandable graphite is 400 mL / g, that of 50 mesh expandable graphite is 350 mL / g, and that of 80 mesh expandable graphite is 250 mL / g.

[0078] The rheological function modifier is polyvinyl alcohol (weight average molecular weight 15000) and lithium-based bentonite (montmorillonite content ≥90wt%). 50 A mixture of two materials (35nm and 35nm) with a mass ratio of 2.5:1.

[0079] The preparation method of the above-mentioned self-consolidating composite resin sealant is the same as that in Example 1, and the self-consolidating composite resin sealant sample B2 is obtained.

[0080] Example 3

[0081] A self-curing composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 50 wt% self-curing composite resin, 0.5 wt% high-temperature stable material, 8 wt% reinforcing filler material, 2 wt% self-adaptive retention material, 5 wt% rheology modifier material, and the balance being water, with the total content of all components being 100%.

[0082] The preparation method of the self-consolidating composite resin is the same as in Example 1, except that: in step (1), the polyamide resin is replaced with a tetrafunctional epoxy resin, which is a yellow to amber transparent liquid with an epoxy equivalent of 150 g / eq, a viscosity (125℃) of 1.2 Pa·s, and a functionality of 3.9; the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin is 20:3; the amount of anhydrous ethanol used is 5 times the mass of the resin; and in step (3), the stirring temperature of the volatile solvent is 40℃ and the stirring time is 6 hours.

[0083] The preparation method of the water-soluble phenolic resin is the same as in Example 1.

[0084] The high-temperature stable material is a combination of water-soluble nano-silica and boron carbide, with a mass ratio of 1:1. The particle size of the water-soluble nano-silica is 10 nm; the particle size of the boron carbide is 20 nm.

[0085] The reinforcing filler material is a combination of S-glass fiber and graphite fiber in a mass ratio of 1:2. The S-glass fiber has a single filament diameter of 7 μm, a length of 5 mm, a tensile strength of 4000 MPa, and an elastic modulus of 95 GPa; the graphite fiber has a single filament diameter of 5 μm, a length of 4 mm, a tensile strength of 3500 MPa, an elastic modulus of 300 GPa, and a carbon content of 99%.

[0086] The adaptive retention material is expandable graphite with an initial expansion temperature of 160℃. The expandable graphite has a particle size distribution of 30 mesh, 50 mesh, and 80 mesh, in a mass ratio of 1:0.6:0.5. The expansion ratio of 30 mesh expandable graphite is 350 mL / g, that of 50 mesh expandable graphite is 300 mL / g, and that of 80 mesh expandable graphite is 200 mL / g.

[0087] The rheological function modifier is polyvinyl alcohol (weight average molecular weight of 15000) and lithium-based bentonite (montmorillonite content ≥90wt%). 50 A mixture of two materials (40 nm and 40 nm) in a mass ratio of 3:1.

[0088] The preparation method of the above-mentioned self-consolidating composite resin sealant is the same as that in Example 1, and the self-consolidating composite resin sealant sample B3 is obtained.

[0089] Example 4

[0090] A self-curing composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 45 wt% self-curing composite resin, 0.8 wt% high-temperature stable material, 10 wt% reinforcing filler material, 6 wt% self-adaptive retention material, 4 wt% rheology modifier material, and the balance being water. The total content of all components is 100%.

[0091] The preparation method of the self-consolidating composite resin is the same as in Example 1, except that: in step (1), the polyamide resin is replaced with liquid carboxylated nitrile rubber. The liquid carboxylated nitrile rubber is a light yellow to amber transparent viscous liquid with a carboxyl content of 2.0 wt%, a number average molecular weight of 10,000, an acid value of 20 mg KOH / g, and a viscosity (25℃) of 3.0 Pa·s; the mass ratio of water-soluble phenolic resin to liquid carboxylated nitrile rubber is 15:2.5.

[0092] The preparation method of the water-soluble phenolic resin is the same as in Example 1.

[0093] The high-temperature stable material is high-purity ultrafine alumina. The high-purity ultrafine alumina has a purity ≥99.9%, a particle size of 50 nm, a crystal form of α-Al₂O₃, and a specific surface area of ​​15 m². 2 / g.

[0094] The reinforcing filler material is E-glass fiber. The E-glass fiber has a single filament diameter of 5μm, a length of 3mm, a tensile strength of 2800MPa, and an elastic modulus of 80GPa.

[0095] The adaptive retention material is expandable graphite. The initial expansion temperature is 160℃, and the particle size of the expandable graphite is a combination of 30 mesh, 50 mesh, and 80 mesh in a mass ratio of 1:0.55:0.55. The expansion ratio of 30 mesh expandable graphite is 250 mL / g, that of 50 mesh expandable graphite is 220 mL / g, and that of 80 mesh expandable graphite is 180 mL / g.

[0096] The rheological function modifier is polyvinyl alcohol (weight average molecular weight of 15000) and lithium-based bentonite (montmorillonite content ≥90wt%). 50 A mixture of two materials (45 nm and 45 nm) with a mass ratio of 3.5:1.

[0097] The preparation method of the above-mentioned self-consolidating composite resin sealant is the same as that in Example 1, and the self-consolidating composite resin sealant sample B4 is obtained.

[0098] Example 5

[0099] A self-curing composite resin sealant is prepared from the following raw materials in the indicated mass fractions: 38 wt% self-curing composite resin, 1.2 wt% high-temperature stable material, 18 wt% reinforcing filler material, 4 wt% adaptive retention material, 3 wt% rheology modifier material, and the balance being water. The total content of all components is 100%.

[0100] The preparation method of the self-consolidating composite resin is as described in Example 1, except that:

[0101] (1) Dissolve water-soluble phenolic resin, polyamide resin, and liquid nitrile rubber in anhydrous ethanol (the amount of anhydrous ethanol used is 3 times the mass of the resin), respectively, to obtain solutions A1, A2, and A3. The mass ratio of water-soluble phenolic resin, polyamide resin, and liquid nitrile rubber is 10:1:1.5. The parameters of the polyamide resin are the same as in Example 1, and the parameters of the liquid nitrile rubber are the same as in Example 2.

[0102] (2) Mix solutions A1, A2 and A3 and stir at a stirring speed of 500 r / min to make the resin blend completely and evenly mixed to obtain mixture B.

[0103] Steps (3) and (4) are the same as in Example 1.

[0104] The preparation method of the water-soluble phenolic resin is the same as in Example 1.

[0105] The high-temperature stable material is water-soluble nano-silica. The particle size of the water-soluble nano-silica is 50 nm.

[0106] The reinforcing filler material is S-glass fiber. The S-glass fiber has a single filament diameter of 15μm, a length of 10mm, a tensile strength of 3000MPa, and an elastic modulus of 86GPa.

[0107] The adaptive retention material is expandable graphite. The initial expansion temperature is 160℃, and the particle size of the expandable graphite is a combination of 30 mesh, 50 mesh, and 80 mesh in a mass ratio of 1:0.5:0.5. The expansion ratio of 30 mesh expandable graphite is 300 mL / g, that of 50 mesh expandable graphite is 250 mL / g, and that of 80 mesh expandable graphite is 220 mL / g.

[0108] The rheological function modifier is polyvinyl alcohol (weight average molecular weight of 15000) and lithium-based bentonite (montmorillonite content ≥90wt%). 50 A mixture of particles with a density of 50 nm (50 nm) in a mass ratio of 4:1.

[0109] The preparation method of the above-mentioned self-consolidating composite resin sealant is the same as that in Example 1, and the self-consolidating composite resin sealant sample B5 is obtained.

[0110] Example 6

[0111] A self-curing composite resin sealant, as described in Example 3, except that in the preparation method of the self-curing composite resin, the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin is set to 20:1; other steps and raw material composition are the same as in Example 3.

[0112] The preparation method of the above-mentioned self-curing composite resin sealant is the same as in Example 3. Sample B6 was obtained.

[0113] Example 7

[0114] A self-curing composite resin sealant, as described in Example 3, except that in the preparation method of the self-curing composite resin, the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin is set to 20:2; other steps and raw material composition are the same as in Example 3.

[0115] The preparation method of the above-mentioned self-curing composite resin sealant is the same as in Example 3. Sample B7 was obtained.

[0116] Example 8

[0117] A self-curing composite resin sealant, as described in Example 3, except that in the preparation method of the self-curing composite resin, the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin is set to 20:4; other steps and raw material composition are the same as in Example 3.

[0118] The preparation method of the above-mentioned self-curing composite resin sealant is the same as in Example 3. Sample B8 was obtained.

[0119] Example 9

[0120] A self-curing composite resin sealant, as described in Example 3, except that in the preparation method of the self-curing composite resin, the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin is set to 20:5; other steps and raw material composition are the same as in Example 3.

[0121] The preparation method of the above-mentioned self-curing composite resin sealant is the same as in Example 3. Sample B9 was obtained.

[0122] Comparative Example 1

[0123] A sealing agent, as described in Example 3, differs in that: the self-consolidating composite resin preparation method does not include water-soluble phenolic resin, i.e., it is a single tetrafunctional epoxy resin; the specific preparation method is as follows:

[0124] (1) Dissolve the tetrafunctional epoxy resin in anhydrous ethanol (the amount of anhydrous ethanol is 5 times the mass of the resin) to obtain solution A1. The index parameters of the tetrafunctional epoxy resin are the same as in Example 3;

[0125] (2) Stir solution A1 at 60℃ and 500 r / min for 3 hours to evaporate most of the anhydrous ethanol; transfer it to a vacuum oven and degas it at 50℃ and vacuum degree -0.08 to -0.09 MPa for 30 min, and treat it with ultrasound for 20 min to remove trapped bubbles.

[0126] (3) After cooling, it is crushed in a universal crusher and passed through a 100-mesh sieve to obtain self-consolidated composite resin powder.

[0127] The types, sources, and preparation methods of the remaining raw materials are the same as in Example 3.

[0128] The preparation method of the above-mentioned sealing agent is the same as in Example 3. The resulting product is designated as Sample D1.

[0129] Comparative Example 2

[0130] A sealing agent, as described in Example 3, except that no high-temperature stabilizing material is added, while the other raw materials, composition, source and preparation method are the same as in Example 3.

[0131] The preparation method of the above-mentioned sealing agent is the same as that described in Example 3, with the same differences. The resulting product is designated as sample D2.

[0132] Comparative Example 3

[0133] A sealing agent, as described in Example 3, except that no reinforcing filler material is added, while the other raw materials, composition, source and preparation method are the same as in Example 3.

[0134] The preparation method of the above-mentioned sealing agent is the same as that described in Example 3, with the same differences. The resulting product is designated as sample D3.

[0135] Comparative Example 4

[0136] A sealing agent, as described in Example 3, except that: no adaptive retention material is added, and the other raw materials, composition, source and preparation method are the same as in Example 3.

[0137] The preparation method of the above-mentioned sealing agent is the same as that described in Example 3, with the same differences. The resulting product is designated as sample D4.

[0138] Comparative Example 5

[0139] A sealing agent, as described in Example 3, except that the adaptive retention material is a single-grain size 30-mesh expandable graphite, excluding 50-mesh and 80-mesh.

[0140] The types, composition, sources and preparation methods of the other raw materials are the same as those in Example 3.

[0141] The preparation method of the above-mentioned sealing agent is the same as in Example 3. The resulting product is designated as Sample D5.

[0142] Comparative Example 6

[0143] A sealing agent is prepared from the following raw materials in the indicated mass fractions: 25 wt% self-consolidating composite resin, 0.5 wt% high-temperature stable material, 8 wt% reinforcing filler material, 2 wt% self-adaptive retention material, 5 wt% rheology modifier material, and the balance being water, with the total content of all components being 100%.

[0144] The types, sources, and preparation methods of the remaining raw materials are the same as in Example 3.

[0145] The preparation method of the above-mentioned sealing agent is the same as in Example 3. The resulting product is designated as Sample D6.

[0146] Comparative Example 7

[0147] A sealing agent is prepared from the following raw materials in the indicated mass fractions: 50 wt% self-consolidating composite resin, 0.5 wt% high-temperature stable material, 25 wt% reinforcing filler, 2 wt% self-adaptive retention material, 5 wt% rheology modifier material, and the balance being water, with the total content of all components being 100%.

[0148] The types, sources, and preparation methods of the remaining raw materials are the same as in Example 3.

[0149] The preparation method of the above-mentioned sealing agent is the same as in Example 3. The resulting product is designated as Sample D7.

[0150] Comparative Example 8

[0151] A sealing agent, as described in Example 3, except that in the preparation method of the self-consolidating composite resin, the water-soluble phenolic resin is replaced with a commercially available water-soluble phenolic resin. The composition, dosage, preparation steps, and conditions of other raw materials are the same as in Example 3. The resulting product is designated as Sample D8.

[0152] Comparative Example 9

[0153] A sealing agent, as described in Example 3, except that urea is not added during the preparation of the water-soluble phenolic resin, and the other preparation steps, conditions, and raw material composition are the same as in Example 3.

[0154] The above-mentioned sealing agent was prepared using the same method as in Example 3, resulting in sample D9.

[0155] Comparative Example 10

[0156] A sealing agent, as described in Example 3, except that the preparation method of the self-consolidating composite resin does not include tetrafunctional epoxy resin, but only water-soluble phenolic resin. The specific method is as follows:

[0157] (1) Dissolve water-soluble phenolic resin in anhydrous ethanol (the amount of anhydrous ethanol is 5 times the mass of the resin) to obtain solution A1.

[0158] (2) Stir solution A1 at 60℃ and 500 r / min for 3 hours to evaporate most of the anhydrous ethanol; transfer it to a vacuum oven and degas it at 50℃ and vacuum degree -0.08 to -0.09 MPa for 30 min, and treat it with ultrasound for 20 min to remove trapped bubbles.

[0159] (3) After cooling, it is crushed in a universal crusher and passed through a 100-mesh sieve to obtain self-consolidated composite resin powder.

[0160] The composition of other raw materials is the same as in Example 3.

[0161] The preparation method of the above-mentioned sealing agent is the same as in Example 3. The resulting product is designated as Sample D10.

[0162] Comparative Example 11

[0163] A sealing agent, as described in Example 3, differs in that: in the preparation method of the self-consolidating composite resin, the toughening resin is a tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide (mass ratio 2:1:1), and the specific method is as follows:

[0164] (1) Dissolve water-soluble phenolic resin, tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide in anhydrous ethanol (the amount of anhydrous ethanol used is 5 times the mass of the resin) to obtain solutions A1, A2, A3, and A4. The mass ratio of water-soluble phenolic resin to toughening resin is 20:3. The mass ratio of tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide is 2:1:1. The parameters of the tetrafunctional epoxy resin are the same as in Example 3; the parameters of the liquid carboxylated nitrile rubber are the same as in Example 4; and the parameters of the polyamide are the same as in Example 1.

[0165] (2) Mix solutions A1, A2, A3 and A4 and stir at a stirring speed of 500 r / min to make the resin blend completely and evenly mixed to obtain mixture B.

[0166] (3) Mixture B is stirred at 60℃ and 500 r / min for 3 hours to evaporate most of the anhydrous ethanol; it is then transferred to a vacuum oven and degassed at 50℃ and vacuum degree -0.08 to -0.09 MPa for 30 min, and then treated with ultrasound for 20 min to remove trapped bubbles.

[0167] (4) After cooling, crush it in a universal crusher and pass it through a 100-mesh sieve to obtain self-consolidated composite resin powder.

[0168] The composition of other raw materials is the same as in Example 3.

[0169] The preparation method of the above-mentioned sealing agent is the same as that in Example 3. The resulting product is designated as Sample D11.

[0170] Test case

[0171] The samples prepared in the examples and comparative examples were tested for compressive strength, dispersion stability, high-temperature and high-pressure plugging performance, high-temperature pumpability, and delayed consolidation performance.

[0172] Test 1: Compressive Strength Test of Leak-Sealing Agent

[0173] A certain amount of sealing agent was weighed and uniformly dispersed at 800 rpm to obtain the sealing slurry to be cured. Then, it was cured at 160℃, 180℃, 200℃, and 220℃ for 24 hours respectively, to prepare cylindrical specimens with a bottom diameter of 25 mm and a height of 25 mm. The compressive mechanical properties were tested using an electronic universal testing machine with a compression speed set to 2 mm / min, and the maximum compressive strength at failure was recorded. Each sample was tested three times, and the average value was taken.

[0174] When the compressive strength is ≥25MPa, it is considered "excellent", indicating that the solidified body is dense and has high strength, and is suitable for large-scale cracks and high-pressure leakage formations;

[0175] A compressive strength greater than or equal to 15 MPa and less than 25 MPa is considered "good," indicating that the solidified body has good strength and can meet the sealing requirements for conventional crack leakage.

[0176] When the compressive strength is <15MPa, it is considered "poor," indicating that the solidified body has insufficient strength or a loose structure, and the sealing effect is unreliable.

[0177] Therefore, the evaluation criteria for compressive strength are as follows: compressive strength ≥ 25 MPa is "excellent", compressive strength greater than or equal to 15 MPa and less than 25 MPa is "good", and compressive strength < 15 MPa is "poor".

[0178] The compressive strength test results of the sealing agents prepared in the above embodiments and comparative examples are shown in Tables 1 and 2.

[0179] Table 1 Compressive strength test results

[0180]

[0181] Table 2 Compressive strength test results

[0182]

[0183] As shown in Tables 1 and 2, the compressive strength of each sample after curing at 160℃, 180℃, 200℃, and 220℃ for 24 hours showed a trend of first increasing and then decreasing with the increase of curing temperature, reaching a peak near 200℃ and slightly decreasing at 220℃; however, the strength differences between different samples were significant.

[0184] All B1-B5 samples exhibit high compressive strength after curing, with B3 showing the best performance. B6-B9 are univariate comparative samples obtained by varying the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin, based on B3. The aforementioned mass ratio has a certain impact on the compressive strength after curing.

[0185] D1 is a single epoxy resin. Lacking the self-crosslinking network of phenolic resin, the single epoxy resin struggles to form a chemically crosslinked cured body at high temperatures, failing to create a high-strength, dense three-dimensional network structure. D2 lacks high-temperature stabilizing materials, leading to thermal degradation and structural relaxation of the resin matrix during high-temperature curing, resulting in a less dense cured network and significantly reduced strength. D3 lacks reinforcing fillers; the cured body relies primarily on the resin matrix for load-bearing capacity, exhibiting insufficient compressive and shear strength, making it prone to overall failure under pressure. D4 lacks adaptive retention materials, and D5 uses a single 30-mesh expandable graphite. While both are superior to D1-D3, they are still significantly lower than B1-B5. This indicates that adaptive retention materials have a synergistic reinforcing effect on the mechanical properties of the cured body: expandable graphite, after expanding at high temperatures, can form a mechanical interlock with the resin matrix and fiber skeleton, improving the density and load-bearing capacity of the cured body; while single-particle-size graphite, lacking gradation fillers, contributes limitedly to the strength of the cured body. D5 (single 30 mesh) is slightly better than D4, indicating that the addition of expandable graphite itself contributes to the strength, but the incomplete particle size distribution prevents it from achieving the effect of B3. D6 uses less self-consolidating composite resin than the scope of this invention, resulting in insufficient curing network and inability to effectively coat and bond reinforcing fibers, expandable graphite, and nanomaterials, leading to a significant decrease in the strength of the cured body. D7 uses more reinforcing filler than the scope of this invention, resulting in insufficient coating and bonding of fibers by the resin matrix, leading to defects and stress concentration within the cured body, and a decrease in compressive strength. D8 uses commercially available water-soluble phenolic resin, but the hydroxymethyl content and molecular weight distribution are uncontrollable, resulting in uneven crosslinking density after curing and a significant decrease in strength. D9 does not contain urea modification, resulting in poor resin toughness, but still retains basic self-consolidation ability, with strength lower than B3. D10 does not contain toughening resin, resulting in high brittleness of the cured body, easy formation of microcracks in the network, and a significant decrease in compressive strength. D11, a compound of tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide (mass ratio 2:1:1), exhibits poor compressive strength, which decreases with increasing curing temperature. This contrasts sharply with B1-B9, which show an initial increase followed by a decrease with increasing temperature. This indicates that the curing network of D11 undergoes unfavorable structural changes during the heating process. The reason for this is the cumulative difference in solubility parameters among the three toughening resins and with the phenolic resin, leading to a decrease in the system's thermodynamic compatibility. This makes macroscopic phase separation more likely during curing, forming phase interfaces and stress concentration points. The higher the temperature, the more severe the phase separation, thus causing the compressive strength to decrease with increasing temperature. This result demonstrates that more types of toughening resin are not necessarily better; rather, the selection and proportions should be controlled within the optimal range.

[0186] The data in Tables 1 and 2 show that the samples from the embodiments of the present invention exhibit excellent compressive strength after curing. This indicates that the present invention achieves both high strength and good toughness through molecular-level composite of rigid phenolic network and flexible toughening resin in self-consolidating composite resin, nano-reinforcement of high-temperature stable materials, skeletal support of reinforcing filler materials, and mechanical interlocking of self-adaptive retention materials. B6-B9 further demonstrate that the toughening resin ratio has a certain influence on compressive strength. The compressive strength of comparative examples D1-D11 under the same curing conditions is lower than that of the embodiments, fully proving that the types and ratios of raw materials in the present invention are indispensable for obtaining high-strength cured bodies.

[0187] Test 2: Dispersion stability test of plugging agent

[0188] Take 500 mL of the sealing agent prepared by the methods of the examples and comparative examples, and stir at a high speed of 800 rpm for 20 minutes. After stirring, immediately transfer the slurry to a 500 mL stoppered graduated cylinder and let it stand for 72 hours at 0.1 MPa and 25°C. After standing, measure the volume of the supernatant (V1) and the volume of the settling layer (V2). The settling rate is calculated according to the following formula: Settling rate SR = [V2 / (V1+V2)] × 100%.

[0189] Meanwhile, the sample dispersion system was tested using a multiple light scattering (Turbiscan Lab) instrument. 20 mL of the sealing agent prepared by the methods in the examples and comparative examples was placed in a dedicated sample cell and scanned for 72 hours under constant temperature conditions of 0.1 MPa and 25°C. The change rate of backscattered light intensity over 72 hours was calculated as ΔBS = [(BS...] 72h -BS 0h ) / BS 0h ]×100% to evaluate suspension stability.

[0190] When the settling rate is ≤3%, it indicates that after the plugging agent particles have been left to stand for 72 hours, the volume of the settling layer is extremely small, the density difference between the particles and the dispersion medium is small, or the particle size distribution is uniform. The rheological function regulating material forms an effective steric hindrance or electrostatic repulsion layer on the particle surface, keeping the particles in a stable suspension state. No obvious particle agglomeration occurs in the system, and most particles are still uniformly dispersed in the form of primary particles.

[0191] When the sedimentation rate is greater than 3% and less than 8%, it indicates that there is a certain degree of sedimentation in the system, but the amount of sedimentation is still within a controllable range. Some larger particles or slight agglomerates undergo slow sedimentation. The rheological function of the material is not enough to completely counteract the effect of gravity, but it can still maintain the suspension of most particles.

[0192] When the settlement rate is ≥8%, it indicates that the system has experienced severe gravity settlement.

[0193] The dispersion stability test results of the plugging agents prepared in the above embodiments and comparative examples are shown in Table 3.

[0194] Table 3. Dispersion stability test results

[0195]

[0196] As shown in Table 3, the sedimentation rate and backscattered light intensity change rate ΔBS of each sample after standing for 72 hours under the conditions of 0.1 MPa and 25℃ showed significant differences.

[0197] B1-B5 exhibit excellent dispersion stability, with B3 showing the best performance. These results demonstrate that the self-consolidating composite resin formed by blending water-soluble phenolic resin and toughening resin in this invention maintains good dispersion stability under the influence of rheology modifiers, reinforcing fillers, adaptive retention materials, and high-temperature stabilizing materials. The polyvinyl alcohol and lithium-based bentonite in the rheology modifiers adsorb onto the surface of each component particle, forming a steric hindrance layer and an electrostatic repulsion layer, effectively inhibiting particle aggregation and gravitational sedimentation, ensuring that the plugging agent remains uniformly suspended in primary particle form even after 72 hours of standing. B6-B9 are univariate comparative samples obtained by changing only the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin, based on B3. When the proportion of toughening resin is too low (B6), the phenolic network becomes too rigid, the interfacial wettability between the resin and the inorganic filler decreases, and slight agglomeration easily occurs between particles, leading to an increase in sedimentation rate and ΔBS. When the proportion of toughening resin is too high (B9), the viscosity of the resin system increases, the number of flexible segments increases, and the coating layer on the particle surface becomes uneven, which also leads to a decrease in dispersion stability.

[0198] D1 is a single epoxy resin. Lacking the self-crosslinking network of phenolic resin, the single epoxy resin has poor compatibility with the bentonite particles in the base slurry, failing to form a stable composite suspension system, resulting in severe gravity sedimentation after 72 hours of standing. D2 lacks high-temperature stabilizing materials, affecting not only curing strength and rheological stability but also dispersion stability. The absence of nanoparticles weakens the interfacial bonding between the resin matrix and inorganic fillers, making particle aggregation and sedimentation more likely. D3 lacks reinforcing fillers, contributing little directly to dispersion stability. D4 lacks adaptive retention materials, and D5 uses a single 30-mesh expandable graphite. The sedimentation rate and ΔBS of D5 are slightly lower than D4, indicating that the addition of expandable graphite itself has a certain improving effect on dispersion stability. Both are significantly worse than B1-B5, indicating that the particle size distribution of the adaptive retention material and the introduction of expandable graphite have a synergistic contribution to dispersion stability. D6 uses a self-consolidating composite resin dosage lower than the scope of this invention, and D7 uses a reinforcing filler dosage higher than the scope of this invention, both resulting in poor dispersion stability. This indicates that the amounts of both the self-consolidating composite resin and the reinforcing filler must be controlled within the preferred range of this invention: If the resin is too little, the particle surface coating is insufficient, making it difficult for the rheology modifier to form a complete steric hindrance layer; if there are too many fibers, the fibers are prone to entanglement, forming local aggregates, leading to an increased sedimentation rate. D8 uses commercially available water-soluble phenolic resin, whose molecular weight distribution and hydroxymethyl content are uncontrollable, resulting in poor compatibility with the rheology modifier, uneven particle surface coating, and lower dispersion stability than B3. D9 did not add urea modification, leading to a decrease in the interfacial wettability between the resin and the inorganic filler, but still retaining basic dispersion ability. D10 did not add toughening resin, consisting only of water-soluble phenolic resin, resulting in decreased dispersion stability. D11 is a compound of tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide (mass ratio 2:1:1). Although the compound of the three toughening resins improves the compatibility between the resin and the filler to a certain extent, the thermodynamic compatibility of the system decreases due to the cumulative difference in solubility parameters between the resins, the coating layer on the particle surface is uneven, and the dispersion stability still cannot reach the B3 level.

[0199] The data in Table 3 show that the embodiments of the present invention exhibit excellent dispersion stability. This indicates that the present invention maintains good dispersion stability of the plugging agent through molecular-level composite of water-soluble phenolic resin and toughening resin, adjustment of the steric hindrance and electrostatic repulsion of the material by rheological function, and adaptive particle size distribution of the retention material. B6-B9 further demonstrate that the toughening resin ratio has a certain influence on dispersion stability. In comparative examples D1-D11, none of them achieved the excellent effect of the embodiments, which fully proves the necessity of the raw material type and ratio in obtaining excellent dispersion stability.

[0200] Test 3: High-Temperature and High-Pressure Sealing Performance Test of Leak-Plugging Agent

[0201] The pressure-bearing sealing performance of plugging agents on fractures was studied using a high-temperature and high-pressure fracture physical simulation device. A steel fracture module was used to simulate fractured and leaky formations. The fracture module was a single wedge-shaped fracture with inlet widths of 1, 3, 5, 7 and 10 mm and a fracture length of 160 mm.

[0202] The high-temperature and high-pressure sealing test procedure is as follows:

[0203] (a) Adjust the temperature of the heating chamber to the simulated formation temperature of 200°C as required;

[0204] (b) Place the steel fracture core of the required fracture width into the core holder and apply confining pressure to 25 MPa;

[0205] (c) Inject the plugging agent into the fracture core at an injection rate of 3.0 mL / min until the grout is completely produced at the fracture outlet;

[0206] (d) Seal the fractured core model and let it stand for 24 hours;

[0207] (e) Drilling fluid-based slurry (4wt% bentonite aqueous solution) is injected into the fracture core in reverse at an injection rate of 3.0 mL / min. The injection pressure changes are recorded in real time using data software. The highest pressure reached when the drilling fluid leaks from the outlet end of the fracture model is the pressure-bearing sealing strength of the plugging agent on the fracture.

[0208] When the maximum pressure at the outlet of the wedge fracture is >12MPa, the plugging body forms a quasi-irreversible stable adhesion, mechanical embedding, and high-pressure sealing with the fracture wall, which can withstand strong pressure fluctuations such as high-density drilling fluid circulation and tripping in and out of the well.

[0209] When the highest pressure at the outlet of the wedge-shaped crack is greater than or equal to 8 MPa and less than or equal to 12 MPa, the plugging body has basic consolidation strength and wedge self-locking capability, and can withstand normal cyclic pressure, but cannot cope with severe pressure fluctuations.

[0210] When the highest pressure at the outlet of the wedge-shaped crack is less than 8 MPa, the sealant is weakly bonded to the crack wall, or the material itself is not strong enough. It mainly relies on the geometric shape for plugging and is easily dispersed.

[0211] Therefore, the sealing strength evaluation standard for plugging agents is defined as follows: when the highest pressure at the outlet end of the wedge crack is greater than 12 MPa, the sealing strength is strong; when the highest pressure at the outlet end of the wedge crack is greater than or equal to 8 MPa and less than or equal to 12 MPa, the sealing strength is medium; when the highest pressure at the outlet end of the wedge crack is less than 8 MPa, the sealing strength is weak.

[0212] The results of the high-temperature and high-pressure sealing performance of the plugging agents prepared in the above embodiments and comparative examples are shown in Tables 4 and 5.

[0213] Table 4. Test Results of High Temperature and High Pressure Plugging Performance

[0214]

[0215] Table 5. Test results of high temperature and high pressure sealing performance

[0216]

[0217] As shown in Tables 4 and 5, the sealing strength of each sample at 200℃ and under different suture widths decreased with increasing suture width, but the decrease varied significantly among different samples.

[0218] B1-B5 exhibit excellent high-temperature and high-pressure sealing performance. These results demonstrate that the present invention, through molecular-level compositing of the rigid phenolic network and flexible toughening resin in the self-consolidating composite resin, the skeletal support provided by the reinforcing filler, the adaptive volume expansion of the retention material at high temperatures, and the temporal synergy formed with the resin's self-consolidation process, enables the sealing agent to exhibit excellent sealing ability for cracks of different widths at 200℃. In particular, B3 maintains high sealing strength even under wide crack conditions, indicating that its adaptive filling and wedge-shaped self-locking capabilities are optimal. B6-B9 are single-variable comparative samples obtained by only changing the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin based on B3. When the toughening resin ratio is too low (B6), the phenolic network is too rigid and brittle, easily undergoing brittle failure under pressure in wide cracks, resulting in decreased sealing strength. When the toughening resin ratio is too high (B9), the proportion of flexible segments increases, the rigidity of the cured body is insufficient, and the pressure-bearing capacity decreases.

[0219] D1 is a single epoxy resin. Lacking the self-crosslinking network of phenolic resin, the single epoxy resin struggles to form a high-strength cured body at high temperatures, resulting in weak bonding between the sealant and the crack wall, making it easily dispersed. D2 lacks high-temperature stabilizing materials, leading to thermal degradation and structural relaxation of the cured network at 200℃, resulting in insufficient sealant strength. D3 lacks reinforcing filler materials, resulting in insufficient compressive and shear strength of the cured body, making it prone to overall failure in wide cracks. D4 lacks adaptive retention materials, and D5 uses a single 30-mesh expandable graphite. Both exhibit reduced high-temperature and high-pressure sealing performance. This indicates that adaptive retention materials play a crucial role in wide crack sealing: expandable graphite expands at high temperatures and actively occupies crack space, interacting with the resin's self-consolidation process; without adaptive retention materials or with incomplete particle size distribution, the sealant cannot achieve full lateral filling in wide cracks, significantly reducing sealing strength. The amount of self-curing composite resin in D6 is lower than that of this invention, while the amount of reinforcing filler in D7 is higher. Both exhibit reduced high-temperature and high-pressure sealing performance. This indicates that insufficient resin leads to an inadequate curing network, while excessive fiber prevents the resin matrix from fully coating and bonding the fibers, resulting in defects within the cured body and decreased sealing strength. D8 uses commercially available water-soluble phenolic resin, D9 is not modified with urea, D10 is not reinforced with toughening resin, and D11 is a blend of tetrafunctional epoxy resin, liquid carboxylated nitrile rubber, and polyamide (mass ratio 2:1:1). All of these formulations show significantly lower sealing capabilities in wide seams compared to B3. While D11 exhibits higher sealing strength in narrow seams, it rapidly decreases in wide seams, indicating that the blend of the three toughening resins leads to decreased thermodynamic compatibility, macroscopic phase separation during curing, and the formation of phase interfaces and stress concentration points within the cured body, resulting in insufficient pressure-bearing capacity in wide seams.

[0220] The data in Tables 4 and 5 show that the embodiments of the present invention exhibit excellent high-temperature and high-pressure sealing performance, with B3 showing the best performance. This indicates that the present invention, through the rigid-flexible composite of self-consolidating composite resin, the skeletal support of reinforced filler material, and the synergistic effect of adaptive particle size distribution of the retention material, enables the plugging agent to have excellent adaptive filling and high-strength sealing capabilities under high-temperature and wide-crack conditions. The sealing strength of comparative examples D1-D11 under the same conditions is significantly lower than that of the embodiments, fully demonstrating the necessity of the raw material types and ratios in the present invention for obtaining excellent high-temperature and high-pressure sealing performance.

[0221] Test 4: High-Temperature Pumpability and Delayed Consolidation Performance of Leak-Sealing Agent

[0222] To evaluate the flow stability of the self-consolidating composite resin plugging agent during high-temperature wellbore delivery, as well as its delayed thickening and consolidation performance after reaching the high-temperature lost circulation zone, high-temperature rheological and consolidation time tests were conducted on the plugging agents prepared in the examples and comparative examples.

[0223] High-temperature rheological testing methods

[0224] 500 ml of the sealing agent prepared by the method of the examples or comparative examples was loaded into a high-temperature and high-pressure rheological testing device and subjected to a pressure of 10 MPa and constant shear conditions (170 s). -1 The test was conducted at 200℃. Timing was started after the set temperature was reached, and the change in apparent viscosity of the plugging slurry over time was continuously recorded. The initial apparent viscosity after reaching the set temperature was recorded as η0. When the apparent viscosity reached 5 times the initial apparent viscosity, the corresponding time was defined as the relative pumpable time tp. It should be noted that this indicator is mainly used to compare the high-temperature thickening rate between different formulations and is not directly equivalent to the absolute pumping limit of the on-site equipment. The initial gel time tg was also recorded; that is, when the system's storage modulus G' reaches the loss modulus G'', and subsequently G' remains higher than G'', this time is defined as the system's initial gel time tg. Each group of tests was conducted in parallel three times, and the average value was taken. The test results are shown in Table 6.

[0225] Table 6. Test results of high-temperature pumpability and delayed consolidation properties

[0226]

[0227] The results in Table 6 show that different compositions have a significant impact on the high-temperature thickening, gelation, and final solidification properties of the self-consolidating composite resin sealant at 200℃. B1-B5 all maintained flowability for a certain period after reaching 200℃, and gradually entered the thickening and gelation stages as the high-temperature treatment time increased, indicating that the sealant of this invention has a certain delayed solidification characteristic.

[0228] Among them, B3's relative pumpability time and initial gel time were not the highest values ​​among all samples, but combined with the test results of compressive strength and high temperature and high pressure crack sealing performance, it showed a good overall match between high temperature pumpability, subsequent gelation rate and final consolidation performance.

[0229] The univariate ratio test of B6-B9 further showed that the mass ratio of water-soluble phenolic resin to tetrafunctional epoxy resin can regulate the high-temperature gelation process of the system: when the proportion of tetrafunctional epoxy resin is low, the high-temperature thickening and gelation process is relatively advanced; when the proportion is too high, the gelation process is significantly delayed.

[0230] The D1-D11 results show from different compositional perspectives that the self-consolidating composite resin, high-temperature stable material, reinforcing filler material, self-adaptive retention material, and their proportions all affect the high-temperature rheology, consolidation, or final sealing performance of the system.

[0231] Therefore, this invention does not achieve sealing by making the plugging agent solidify as quickly as possible under high temperature conditions. Instead, it adjusts the composition and ratio to allow the plugging agent to retain a certain flow time in the initial stage of high-temperature action, and gradually thicken, gel, and solidify after continuous heating. This balances the wellbore delivery requirements with the solidification and sealing performance after entering the leakage channel. In actual construction, the expected delivery time of the plugging slurry should be less than the relative pumpable time measured under the corresponding well temperature conditions, and necessary safety margins should be reserved for construction.

[0232] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A self-curing composite resin sealant, characterized in that, The raw materials are prepared by including the following mass fractions: 35-50 wt% self-consolidating composite resin, 0.5-1.5 wt% high-temperature stable material, 8-18 wt% reinforcing filler material, 2-8 wt% adaptive retention material, 2-5 wt% rheology modifier material, and the balance is water. The total content of each component is 100%. The preparation method of the self-consolidating composite resin includes the following steps: fully dissolving water-soluble phenolic resin and toughening resin in a solvent, evaporating the solvent, degassing, pulverizing, and sieving to obtain the self-consolidating composite resin; the toughening resin is selected from one or two of polyamide, liquid nitrile rubber, liquid carboxylated nitrile rubber, or tetrafunctional epoxy resin. The preparation method of water-soluble phenolic resin includes the following steps: in the presence of alkali, antioxidant and modifier, phenol and formaldehyde aqueous solution undergo addition and condensation reactions to obtain water-soluble methyl phenolic resin solution; then, after neutralization, stabilization, filtration and drying, water-soluble phenolic resin is obtained; the modifier is urea. The high-temperature stabilizing material is one or a combination of two of ultrafine alumina, water-soluble nano-silica, or boron carbide; the reinforcing filler is one or a combination of two of E-glass fiber, S-glass fiber, or graphite fiber; the adaptive retention material is expandable graphite, and the particle size of the expandable graphite is a combination of 30 mesh, 50 mesh, and 80 mesh expandable graphite; the rheological function modulating material is a mixture of polyvinyl alcohol and lithium-based bentonite.

2. The self-curing composite resin sealant according to claim 1, characterized in that, The preparation method of water-soluble phenolic resin includes one or more of the following conditions: i. The alkali is one of ammonia, triethylamine, or hexamethylenetetramine with a mass concentration of 5%-25%; the pH of the system is controlled to be 8.5-10.0 by adding the alkali; ii. The antioxidant is sodium bisulfite, and the mass of the antioxidant is 0.1wt%-0.3wt% of the mass of phenol; iii. The mass of the modifier is 10wt%-25wt% of the mass of phenol; iv. The mass concentration of the formaldehyde aqueous solution is 37%-40%; the molar ratio of phenol to formaldehyde is 1:1.8-2.2; v. The addition reaction temperature is 55-65℃, and the addition reaction time is 30-60 min; the polycondensation reaction temperature is 75-85℃, and the polycondensation reaction time is 40-80 min. vi. The stabilization method is as follows: Add sodium bisulfite or ascorbic acid to the system and mix thoroughly; the mass of sodium bisulfite or ascorbic acid is 0.05%-0.2% of the mass of the water-soluble methyl phenolic resin solution.

3. The self-curing composite resin sealant according to claim 1, characterized in that, The preparation method of self-consolidated composite resin includes one or more of the following conditions: i. The mass ratio of water-soluble phenolic resin to toughening resin is 4-20:1-3; ii. The weight-average molecular weight of polyamide is 10,000-20,000; iii. The number average molecular weight of the liquid nitrile rubber is 1,000-10,000, and the acrylonitrile content is 18wt%-40wt%. iv. The carboxyl content of liquid carboxylated acrylonitrile butadiene rubber is 0.5wt%-3.0wt%, and the number average molecular weight is 5,000-15,000; v. The epoxy equivalent of tetrafunctional epoxy resin is 100-200 g / eq, and the viscosity at 125℃ is 0.5-2.0 Pa·s; vi. The solvent is anhydrous ethanol; the mass of the solvent is 1-5 times the total mass of the water-soluble phenolic resin and the toughening resin. vii. The conditions for evaporating the solvent are as follows: stir at 40-80℃ for 1-6 hours.

4. The self-curing composite resin sealant according to claim 1, characterized in that, Includes one or more of the following conditions: i. The particle size of ultrafine alumina is 20-50 nm, the crystal form is α-Al₂O₃ or γ-Al₂O₃, and the specific surface area is 15-40 m². 2 / g; the particle size of water-soluble nano-silica is 10-50nm; the particle size of boron carbide is 20-50nm; ii. E-glass fiber has a monofilament diameter of 5-20μm, a length of 3-15mm, a tensile strength of 2200-2800Mpa, and an elastic modulus of 72-80Gpa; S-glass fiber has a monofilament diameter of 7-15μm, a length of 5-10mm, a tensile strength of 3000-4000Mpa, and an elastic modulus of 86-95Gpa; graphite fiber has a monofilament diameter of 5-8μm, a length of 4-6mm, a tensile strength of 3000-3500Mpa, an elastic modulus of 250-300Gpa, and a carbon content ≥95%. iii. The initial expansion temperature of expandable graphite is 160-220℃; the mass ratio of 30 mesh, 50 mesh and 80 mesh expandable graphite is 1:(0.5-0.6):(0.5-0.6); the expansion ratio of 30 mesh expandable graphite is 250-400mL / g, the expansion ratio of 50 mesh expandable graphite is 220-300mL / g, and the expansion ratio of 80 mesh expandable graphite is 180-250mL / g.

5. The self-curing composite resin sealant according to claim 1, characterized in that, Includes one or more of the following conditions: i. The high-temperature stable material is a combination of ultrafine alumina and water-soluble nano-silica, with a mass ratio of ultrafine alumina to water-soluble nano-silica of 1:1-10; or a combination of ultrafine alumina and boron carbide, with a mass ratio of ultrafine alumina to boron carbide of 1:3-15; or a combination of water-soluble nano-silica and boron carbide, with a mass ratio of water-soluble nano-silica to boron carbide of 1:0.5-5. ii. The reinforcing filler material is a combination of E-glass fiber and S-glass fiber, with a mass ratio of E-glass fiber to S-glass fiber of 1:0.5-2; or a combination of E-glass fiber and graphite fiber, with a mass ratio of E-glass fiber to graphite fiber of 1:0.3-1.5; or a combination of S-glass fiber and graphite fiber, with a mass ratio of S-glass fiber to graphite fiber of 1:0.5-2.

6. The self-curing composite resin sealant according to claim 1, characterized in that, The mass ratio of polyvinyl alcohol to lithium-based bentonite is 2-4:

1.

7. The self-consolidating composite resin sealant according to claim 1, characterized in that, Lithium-based bentonite particle size D 50 It is 30-50nm.

8. The method for preparing the self-consolidating composite resin sealant according to any one of claims 1-7, characterized in that, Including the following steps: The rheological function regulating material is fully dispersed in water; a high-temperature stabilizing material is added and fully dispersed; a self-consolidating composite resin is added and fully dispersed; then an adaptive retention material and a reinforcing filler are added and fully dispersed to obtain a self-consolidating composite resin sealant.

9. The application of the self-consolidating composite resin plugging agent as described in any one of claims 1-7 in drilling fluid plugging.

Citation Information

Patent Citations

  • Self-consolidation type plugging agent, preparation method thereof and drilling fluid

    CN121064805A

  • Self-consolidation leaking stoppage material as well as preparation method and application thereof

    CN121064810A