Slow-release water-retaining formula material for ecological water replenishment of wetlands and preparation method thereof
By combining a composite water-retaining active mixture with a pH/temperature dual-responsive coating layer, the shortcomings of wetland ecological water replenishment materials in terms of water absorption and retention performance, release rate, and degradation cycle are solved, achieving efficient, intelligent, slow-release, and environmentally friendly wetland ecological water replenishment effects.
Patent Information
- Application Number
- CN202611222658.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-10
AI Technical Summary
Existing wetland ecological water replenishment materials have shortcomings in terms of water absorption and retention performance, release rate and degradation cycle, making it difficult to achieve intelligent response and efficient slow release, and traditional materials may cause secondary pollution.
By combining a composite water-retaining active mixture with a pH/temperature dual-responsive coating layer, and through in-situ compounding of modified biochar, acrylic-acrylamide copolymer, sodium alginate, attapulgite, and potassium humate, combined with a two-stage variable temperature gradient crosslinking and dual curing process, a core-shell structure slow-release water-retaining material is formed.
It achieves a balance between high water absorption capacity and long-lasting intelligent slow-release performance. The material can automatically adjust the water release rate in response to environmental changes, thereby improving its cycle life and avoiding secondary pollution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of wetland ecological restoration and water-retaining materials technology, and in particular to a slow-release water-retaining formulation material and its preparation method for wetland ecological water replenishment. Background Technology
[0002] Wetlands are one of the most important ecosystems on Earth, possessing multiple ecological functions such as flood control, water purification, and maintaining biodiversity. However, due to climate change and human activities, the area of wetlands worldwide is continuously decreasing, and wetland degradation is becoming increasingly serious. Ecological water replenishment of wetlands is a necessary means to restore the ecological functions of degraded wetlands. Its core lies in restoring wetland hydrological conditions by replenishing water to the wetlands, thereby promoting wetland vegetation restoration and ecosystem reconstruction.
[0003] In wetland ecological water replenishment practices, the application of water-retaining materials has received widespread attention. These materials can absorb and retain large amounts of water, releasing it slowly under drought conditions, thereby prolonging the replenishment effect and improving water resource utilization efficiency. Currently, water-retaining materials used in wetland ecological restoration mainly include synthetic polymer water-retaining agents, natural polymer water-retaining materials, and inorganic mineral water-retaining materials.
[0004] Existing water-retaining materials still have many shortcomings in wetland ecological water replenishment applications. First, traditional water-retaining materials have limited water absorption and retention capabilities, lacking the ability to intelligently respond to the complex aquatic environment of wetlands, making it difficult to achieve precise regulation and release of water. Second, most existing water-retaining materials are simple physical mixtures or single polymer products, lacking synergistic effects between components, making it difficult to balance water retention capacity and release rate. Third, some water-retaining materials degrade too quickly or too slowly in wetland environments, failing to meet the actual requirements of slow-release duration for wetland ecological water replenishment. Furthermore, although there are reports of the dual pH / temperature sensitivity of N-isopropylacrylamide-acrylic acid copolymer microgels in existing technologies, there are no reports of combining them with water-retaining material coating layers for wetland ecological water replenishment.
[0005] Therefore, this invention proposes a slow-release water-retaining formulation material and its preparation method for wetland ecological water replenishment. Summary of the Invention
[0006] The purpose of this invention is to address the shortcomings of existing technologies by proposing a slow-release water-retaining formulation material and its preparation method for wetland ecological water replenishment.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 30-55 parts of composite water-retaining active mixture, 5-15 parts of pH / temperature dual-response slow-release coating mixture, 0.5-3 parts of crosslinking agent, 0.3-2 parts of initiator, and 50-100 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is (20-40):(15-30):(5-15):(10-25):(3-10); The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:0.5-1:3.
[0008] As a preferred technical solution of this application, the modified biochar is prepared by pyrolyzing reed straw at 400-600℃ under limited oxygen, oxidizing it with a 10%-20% hydrogen peroxide solution for 2-4 hours, and then impregnating it in a 5%-15% acetic acid aqueous solution containing chitosan for 12-24 hours.
[0009] As a preferred embodiment of this application, the molar ratio of acrylic acid to acrylamide in the acrylic acid-acrylamide copolymer is 1:0.3-1:0.8, and the degree of neutralization of the acrylic acid is 60%-80%.
[0010] As a preferred technical solution of this application, the N-isopropylacrylamide-acrylic acid copolymer microgel has an average particle size of 100-500 nm and a low critical dissolution temperature of 32-38 °C.
[0011] As a preferred technical solution of this application, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 2:1-5:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 1:1-3:1.
[0012] A method for preparing a slow-release water-retaining formulation material for wetland ecological water replenishment includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 10%-20%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 40-70℃ for 1-3 hours, and then the temperature is raised to 75-90℃ for the second stage reaction for 1-3 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 2-10 mm, and dry it at 50-80℃ until the water content is no more than 10% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide and acrylic acid are dissolved in deionized water at a molar ratio of 10:1-5:1, a crosslinking agent and an initiator are added, and the polymerization reaction is carried out at 60-80℃ for 4-8 hours to obtain N-isopropylacrylamide-acrylic acid copolymer microgel; the microgel is mixed with calcium alginate-chitosan complex at a weight ratio of 1:0.5-1:3 to prepare a coating solution with a mass fraction of 5%-15%; Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating solution obtained in step S3 for 10-30 min, and then placed in a calcium chloride solution with a mass fraction of 1%-5% for curing and crosslinking for 10-60 min. After removal, they are dried in a forced-air drying oven at 30-50℃ to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0013] As a preferred technical solution of this application, in step S1, the first stage reaction temperature is 50-60℃ and the reaction time is 2h; the second stage reaction temperature is 80-85℃ and the reaction time is 2h.
[0014] As a preferred technical solution of this application, the molar ratio of N-isopropylacrylamide to acrylic acid in step S3 is 8:1-6:1, the polymerization reaction temperature is 70-75℃, and the reaction time is 5-7h.
[0015] As a preferred technical solution of this application, the impregnation and coating time in step S4 is 15-25 min, and the curing and crosslinking time of the calcium chloride solution is 20-40 min.
[0016] Application of a slow-release water-retaining material for wetland ecological water replenishment in wetland soil water retention, wetland vegetation restoration, or wetland ecological water replenishment.
[0017] The beneficial effects of this invention are as follows: 1. By in-situ composite construction of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate into a unified water-retaining functional body, the five components form a multi-synergistic mechanism of physical support, chemical cross-linking, hydrogen bonding association and ion exchange. At the same time, a two-stage temperature gradient cross-linking polymerization process is adopted to make the cross-linking density of the material gradually increase from the inside to the outside, taking into account both the high water absorption capacity inside and the high strength of the surface. The water absorption and retention performance and mechanical strength are significantly better than the simple superposition of the components. 2. By combining N-isopropylacrylamide-acrylic acid copolymer thermosensitive microgel with calcium alginate-chitosan pH-sensitive complex to form a dual-response coating layer, the material can automatically adjust the permeability and water release rate of the coating layer according to changes in ambient temperature and pH, and realize an intelligent water replenishment mode of slowing down release at low temperature, accelerating supply at high temperature, and adaptive regulation of acid and alkaline conditions, effectively overcoming the defect of the single release behavior of traditional water-retaining materials. 3. Through a dual curing process of calcium ion solidification and cross-linking after coating, the coating layer is transformed from physical adhesion to chemical bonding and anchoring, forming a strong interface bond, effectively preventing the coating layer from falling off and breaking, and significantly improving the service life of the cycle; at the same time, modified biochar is prepared from wetland plant waste such as reed straw, and each component can be naturally degraded or participate in the soil material cycle after the use cycle, without causing secondary pollution. 4. Through the core-shell structure design, the water absorption capacity and release rate are independently undertaken by the core and the shell, respectively, so that the two no longer hinder each other, thus achieving an organic unity of high water absorption and retention capacity and long-lasting intelligent slow-release performance.
[0018] This invention forms a complete technical solution for slow-release water-retaining materials for wetland ecological water replenishment by combining the synergistic construction of composite water-retaining active mixtures, the intelligent barrier design of dual-responsive coating layers, and a two-stage temperature gradient crosslinking and dual curing process. It achieves breakthroughs over existing technologies in three dimensions: component design, functional integration, and process innovation, providing a novel material solution with excellent performance, environmental friendliness, and intelligent response for wetland ecological water replenishment. Detailed Implementation
[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0020] I. Raw Material Source and Specifications 1. The main raw materials used in the various embodiments and comparative examples of the present invention are as follows:
[0021] 2. Preparation of modified biochar Naturally air-dried reed stalks were crushed to a particle size of ≤2mm, placed in a tube furnace, and heated to 500℃ at a heating rate of 10℃ / min under nitrogen protection. The temperature was maintained for pyrolysis for 3 hours, and then naturally cooled before being removed to obtain the primary biochar product.
[0022] The above-mentioned biochar primary product was placed in a 15% hydrogen peroxide solution with a solid-liquid ratio of 1:10 (g / mL) and oxidized at room temperature for 3 hours. After filtration and washing until neutral, it was dried at 80°C to constant weight.
[0023] The oxidized biochar was placed in a chitosan acetic acid solution with a chitosan mass fraction of 10% (chitosan dissolved in a 2% acetic acid aqueous solution by volume) at a solid-liquid ratio of 1:8 (g / mL). The mixture was stirred and impregnated at room temperature for 18 hours. After filtration, the biochar was washed with deionized water until neutral and dried under vacuum at 60°C to constant weight to obtain the modified biochar.
[0024] 3. Preparation of calcium alginate-chitosan complex Sodium alginate was dissolved in deionized water to prepare a 2% sodium alginate solution. This solution was then added dropwise to a 3% calcium chloride solution using a constant flow pump (flow rate 1 mL / min). The solution was cross-linked and cured at room temperature for 45 minutes to form calcium alginate microspheres. After filtration and washing three times with deionized water, the calcium alginate microspheres were immersed in a 1% chitosan acetate solution (chitosan dissolved in a 2% acetic acid aqueous solution) for 20 minutes. After filtration and washing with deionized water, the solution was vacuum dried at 40°C to obtain the calcium alginate-chitosan complex.
[0025] 4. Preparation of N-isopropylacrylamide-acrylic acid copolymer microgels N-Isopropylacrylamide and acrylic acid were dissolved in deionized water at a specified molar ratio (total monomer mass fraction: 5%). N,N′-methylenebisacrylamide (2% of total monomer mass) and ammonium persulfate (1% of total monomer mass) were added as crosslinking agent. After purging with nitrogen for 30 minutes to remove oxygen, the mixture was heated to 72°C and polymerized under nitrogen protection for 6 hours to obtain N-isopropylacrylamide-acrylic acid copolymer microgels. The average particle size of the obtained microgels was approximately 300 nm, as determined by a laser particle size analyzer. The transmittance of the microgel dispersion at different temperatures was measured using a UV-Vis spectrophotometer, and its lower critical dissolution temperature was approximately 35°C.
[0026] II. Performance Testing and Instrumentation 1. Determination of water absorption ratio Referring to the standard method of NY / T 886-2022 "Water Retaining Agents for Agriculture and Forestry", under environmental conditions of 25±2℃, weigh 1.00g of dry sample (accurate to 0.001g) and place it in a 2L beaker. Add 1L of tertiary water, stir for 5min, and let stand for 2h to allow the sample to fully absorb water and swell. Transfer the water-absorbed sample to a 0.18mm sieve (the mass of the sieve is recorded as M0), filter naturally for 10min, then tilt the sieve and filter for another 10min. Weigh the mass of the sieve and the expanded sample (recorded as Mf). The water absorption ratio W (g / g) is calculated using the following formula: W = (Mf - M0) / m0 In the formula: M0 is the mass of the sieve; Mf is the total mass of the sieve and the sample after water absorption; m0 is the mass of the dried sample.
[0027] Each sample was measured in triplicate, and the results are expressed as mean ± standard deviation.
[0028] 2. Determination of water absorption ratio under different pH conditions Following the methods described in the literature, buffer solutions with pH values of 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, and 10.0 were prepared (a citrate-sodium citrate buffer system was used for pH 4.0-6.0, a phosphate buffer system was used for pH 7.0-8.0, and a borax-sodium hydroxide buffer system was used for pH 9.0-10.0). The water absorption ratio of the samples was measured under different pH conditions according to the aforementioned method for determining water absorption ratio. Each sample was measured in triplicate.
[0029] 3. Determination of water retention rate Referring to the isothermal dehydration kinetics method reported in the literature, 1.00 g of sample saturated with water was weighed and placed in a constant temperature drying oven at 40±1℃ (relative humidity 45±5%). The sample was weighed every 24 hours until a constant weight was achieved. The water retention rate R (%) was calculated using the following formula: R = (mt / m0) × 100% In the formula: mt is the mass of the sample after drying time t; m0 is the mass of the sample after initial saturation and water absorption.
[0030] Each sample was measured in triplicate.
[0031] 4. Determination of cumulative water release rate 1.00 g of dried sample was placed in deionized water until saturated. After removal, the surface moisture was absorbed with filter paper, and the sample was weighed (recorded as m0). Then, it was placed in a constant temperature water bath at 37±0.5℃ (container covered, relative humidity 60±5%). The sample was removed at different time points (1h, 2h, 4h, 8h, 12h, 24h, 36h, 48h, 72h, 96h, 120h), the surface moisture was absorbed with filter paper, and the sample was weighed (recorded as mt). Finally, the sample was dried at 80℃ to constant weight (recorded as md). The cumulative water release rate E (%) was calculated using the following formula: E = (m0-mt) / (m0-md) × 100% In the formula: m0 is the mass of the sample after initial saturation water absorption; mt is the mass of the sample after release time t; md is the mass of the sample after drying to constant weight.
[0032] Each sample was measured in triplicate.
[0033] 5. Determination of repeated water absorption ratio Following the standard method of NY / T 886-2022, 1.00 g of dried sample was weighed, and the initial water absorption ratio W1 was determined according to the water absorption ratio determination method. The sample after water absorption was then placed in a forced-air drying oven at 80±2℃ and dried to constant weight (24 h). The dried sample was then weighed again to determine the second water absorption ratio, and this process was repeated for 5 consecutive tests. The repeated water absorption ratio Rr (%) was calculated using the following formula: Rr = (W5 / W1) × 100% In the formula: W1 is the first water absorption ratio; W5 is the fifth water absorption ratio.
[0034] 6. Soil water retention rate determination Following the method described in the literature, 100.0g of sieved (0.6mm aperture) wetland soil was mixed thoroughly with 0.5g of sample and placed into a pre-weighed nylon filter bag (0.05mm aperture). The nylon filter bag was immersed in a container of deionized water for 4 hours to fully absorb water, then removed and allowed to stand naturally for about 10 minutes until no water droplets fell, at which point it was weighed. Subsequently, the filter bag was placed at room temperature (25±2℃) and relative humidity (50±5%), and its mass was measured daily for 15 consecutive days. The water retention rate of the soil sample was then calculated.
[0035] 7. Determination of gel strength Following the method described in the literature, the texture analyzer was used to determine the gel strength. The water-saturated sample was placed on the testing platform, and a P / 0.5R cylindrical probe was used. The testing speed was 1.0 mm / s, and the compression deformation was 70%. The maximum force value was recorded as the gel strength (unit: g). Each sample was measured in parallel five times.
[0036] III. Examples and Comparative Examples Example 1 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 42 parts of composite water-retaining active mixture, 10 parts of pH / temperature dual-response slow-release coating mixture, 1.8 parts of crosslinking agent, 1.0 part of initiator, and 75 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 28:22:10:18:7. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:1.5.
[0037] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0038] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in this embodiment includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 55°C for 2 hours, and then the temperature is increased to 82°C at a heating rate of 2°C / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide-acrylic acid copolymer microgel (average particle size about 300 nm, lower critical dissolution temperature about 35 °C) and calcium alginate-chitosan complex were prepared according to the aforementioned general method. During the preparation process, the molar ratio of N-isopropylacrylamide to acrylic acid was 7:1. Then, the microgel and calcium alginate-chitosan complex were mixed evenly at a weight ratio of 1:1.5 to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 20 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 30 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0039] Example 2 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 35 parts of composite water-retaining active mixture, 8 parts of pH / temperature dual-response slow-release coating mixture, 1.2 parts of crosslinking agent, 0.6 parts of initiator, and 60 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 22:18:8:15:5. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:1.
[0040] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0041] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in this embodiment includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 50°C for 2 hours, and then the temperature is increased to 80°C at a heating rate of 2°C / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide-acrylic acid copolymer microgel (average particle size about 300 nm, lower critical dissolution temperature about 35 °C) and calcium alginate-chitosan complex were prepared according to the aforementioned general method. During the preparation process, the molar ratio of N-isopropylacrylamide to acrylic acid was 6:1. The microgel and calcium alginate-chitosan complex were mixed evenly at a weight ratio of 1:1 to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 15 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 25 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0042] Example 3 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 50 parts of composite water-retaining active mixture, 13 parts of pH / temperature dual-response slow-release coating mixture, 2.5 parts of crosslinking agent, 1.5 parts of initiator, and 90 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 35:28:13:22:9. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:2.
[0043] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0044] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in this embodiment includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 60°C for 2 hours, and then the temperature is increased to 85°C at a heating rate of 2°C / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide-acrylic acid copolymer microgel (average particle size about 300 nm, lower critical dissolution temperature about 35 °C) and calcium alginate-chitosan complex were prepared according to the aforementioned general method. During the preparation process, the molar ratio of N-isopropylacrylamide to acrylic acid was 8:1. Then, the microgel and calcium alginate-chitosan complex were mixed evenly at a weight ratio of 1:1.5 to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 25 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 40 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0045] Comparative Example 1 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 42 parts of composite water-retaining active mixture, 10 parts of pH / temperature dual-response slow-release coating mixture, 1.8 parts of crosslinking agent, 1.0 part of initiator, and 75 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 28:22:10:18:7. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:1.5.
[0046] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0047] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in the comparative example includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 55°C for 2 hours, and then the temperature is increased to 82°C at a heating rate of 2°C / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2, Granulation and Drying: The gel-like composite water-retaining active mixture obtained in step S1 is granulated by an extrusion granulator with a particle size controlled at 5 mm. It is then dried at 65°C with forced air until the moisture content is no more than 8%, thus obtaining the uncoated water-retaining material.
[0048] Comparative Example 2 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 42 parts of composite water-retaining active mixture, 10 parts of coating layer, 1.8 parts of crosslinking agent, 1.0 part of initiator, and 75 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 28:22:10:18:7. The coating layer is composed of calcium alginate-chitosan complex.
[0049] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0050] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in the comparative example includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 55°C for 2 hours, and then the temperature is increased to 82°C at a heating rate of 2°C / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of coating solution: Mix deionized water and calcium alginate-chitosan complex evenly to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 20 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 30 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0051] Comparative Example 3 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 42 parts of composite water-retaining active mixture, 10 parts of pH / temperature dual-response slow-release coating mixture, 1.8 parts of crosslinking agent, 1.0 part of initiator, and 75 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is 28:22:10:18:7. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:1.5.
[0052] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0053] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in the comparative example includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially, and the reaction is carried out at 70°C for 4 hours to obtain a gel-like composite water-retaining active mixture; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide-acrylic acid copolymer microgel (average particle size about 300 nm, lower critical dissolution temperature about 35 °C) and calcium alginate-chitosan complex were prepared according to the aforementioned general method. During the preparation process, the molar ratio of N-isopropylacrylamide to acrylic acid was 7:1. Then, the microgel and calcium alginate-chitosan complex were mixed evenly at a weight ratio of 1:1.5 to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 20 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 30 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0054] Comparative Example 4 A slow-release water-retaining formulation material for wetland ecological water replenishment is prepared from the following raw materials in parts by weight: 42 parts of composite water-retaining active mixture, 10 parts of pH / temperature dual-response slow-release coating mixture, 1.8 parts of crosslinking agent, 1.0 part of initiator, and 75 parts of deionized water. The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate and attapulgite, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate and attapulgite is 28:22:10:18. The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:1.5.
[0055] Furthermore, the crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 3:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 2:1.
[0056] The preparation method of the slow-release water-retaining formulation material for wetland ecological water replenishment described in the comparative example includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar and attapulgite are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 15%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 55℃ for 2 hours, and then the temperature is increased to 82℃ at a heating rate of 2℃ / min for the second stage reaction for 2 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 5 mm, and dry it at 65°C until the moisture content is no more than 8% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide-acrylic acid copolymer microgel (average particle size about 300 nm, lower critical dissolution temperature about 35 °C) and calcium alginate-chitosan complex were prepared according to the aforementioned general method. During the preparation process, the molar ratio of N-isopropylacrylamide to acrylic acid was 7:1. Then, the microgel and calcium alginate-chitosan complex were mixed evenly at a weight ratio of 1:1.5 to prepare a coating solution with a mass fraction of 10%. Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating liquid obtained in step S3 for 20 min, then removed and placed in a 3% calcium chloride solution for curing and crosslinking for 30 min. After removal, they are dried in a forced-air drying oven at 40°C to obtain the slow-release water-retaining material for wetland ecological water replenishment.
[0057] IV. Test Results Table 1. Main performance indicators of each embodiment and comparative example
[0058] Table 2. Water absorption ratio (g / g) of each example and comparative example under different pH conditions.
[0059] Table 3. Time (h) required for the cumulative water release rate of each embodiment and comparative example to reach 50% under different temperature conditions.
[0060] V. Results Analysis 1. Water absorption ratio analysis As shown in Table 1, the water absorption ratios of Examples 1-3 in deionized water were 486 g / g, 452 g / g, and 512 g / g, respectively, all significantly higher than Comparative Example 2 (475 g / g) and slightly lower than Comparative Example 1 (498 g / g). This result indicates that the presence of the coating layer has a certain impact on the water absorption ratio—Comparative Example 1 had the highest water absorption ratio without coating, but the water absorption ratio decreased slightly after coating (Example 1 and Comparative Example 2). This is because the coating layer restricts the rapid penetration of water into the core to a certain extent. However, the water absorption ratio of Example 1 (486 g / g) was higher than that of Comparative Example 2 (475 g / g), indicating that the dual-responsive coating mixture has better water permeability than the single calcium alginate-chitosan coating layer. This is due to the microporous channels generated by the swelling of the N-isopropylacrylamide-acrylic acid copolymer microgel during water absorption, which is conducive to water penetration.
[0061] The water absorption ratio of Comparative Example 4 was only 412 g / g, significantly lower than that of Example 1 (486 g / g), a decrease of 15.2%. This indicates that potassium humate is not simply a nutrient additive, but rather participates in the formation of the polymer network through active groups such as carboxyl and phenolic hydroxyl groups in its molecular structure. It undergoes grafting or cross-linking reactions with the acrylic acid-acrylamide copolymer, significantly enhancing the hydrophilicity and ion exchange capacity of the three-dimensional network structure, resulting in a synergistic effect. This experimental evidence of "significant performance decline due to missing components" strongly demonstrates the indispensable synergistic effect of each component in the composite water-retaining active mixture.
[0062] Regarding the water absorption ratio in 0.9% NaCl solution, Examples 1-3 were 68 g / g, 62 g / g, and 72 g / g, respectively, all of which were superior to Comparative Example 1 (65 g / g) and Comparative Example 2. This indicates that the calcium alginate-chitosan complex in the coating layer has a certain barrier effect on salt ions, reducing the negative impact of salt ions on the water absorption performance of the core polymer.
[0063] 2. Water retention performance analysis As shown in Table 1, after being placed at 40℃ for 72 hours, the water retention rates of Examples 1-3 were 68.5%, 64.2%, and 71.8%, respectively, while those of Comparative Example 1 were only 42.3%, Comparative Example 2 was 55.6%, Comparative Example 3 was 58.2%, and Comparative Example 4 was 60.5%. After being placed for 120 hours, the water retention rates of Examples 1-3 were 52.3%, 48.6%, and 56.1%, respectively, while those of Comparative Example 1 decreased to 25.8%, Comparative Example 2 decreased to 38.4%, Comparative Example 3 decreased to 40.5%, and Comparative Example 4 decreased to 43.2%.
[0064] The 72-hour water retention rate of Example 1 was 23.2% higher than that of Comparative Example 2, 17.7% higher than that of Comparative Example 3, and 13.2% higher than that of Comparative Example 4. This result indicates that: First, the pH / temperature dual-responsive coating mixture exhibits superior water retention performance compared to a single calcium alginate-chitosan coating layer. This is because the N-isopropylacrylamide-acrylic acid copolymer microgel undergoes a volume phase transition shrinkage upon temperature increase, forming a "valve" effect in the coating layer, further slowing down the water release rate. Second, the "two-stage variable temperature gradient crosslinking" process significantly improves water retention performance compared to the isothermal polymerization process. This is because the gradient crosslinking structure results in a gradient distribution of crosslinking density within the material—lower internal crosslinking density to ensure high water absorption capacity, and higher surface crosslinking density to enhance mechanical strength and water retention effect. Third, the addition of potassium humate significantly improves water retention performance, confirming its synergistic crosslinking effect with the polymer network.
[0065] 3. Analysis of sustained-release performance The time required for the cumulative water release rate to reach 80% is an important indicator for evaluating the sustained-release performance of materials. As shown in Table 1, the times required for Examples 1-3 to reach 80% cumulative water release rate were 96h, 88h, and 104h, respectively, which are much longer than the 36h of Comparative Example 1, 62h of Comparative Example 2, 68h of Comparative Example 3, and 75h of Comparative Example 4.
[0066] The time required for the cumulative water release rate of Example 1 to reach 80% was extended by 54.8% compared to Comparative Example 2, by 41.2% compared to Comparative Example 3, and by 28.0% compared to Comparative Example 4. This result fully demonstrates the synergistic contribution of the three core technical features of this invention: the slow-release barrier effect of the dual-response coating layer, the optimization of the network structure by the two-stage temperature gradient crosslinking process, and the regulation of network density by potassium humate participating in crosslinking.
[0067] As shown in Table 3, the water release rates of Examples 1-3 all exhibited significant temperature response characteristics under different temperature conditions—the time required to reach a cumulative water release rate of 50% was significantly shortened as the temperature increased from 25℃ to 45℃. This temperature response characteristic stems from the low critical dissolution temperature (approximately 32-38℃) of the N-isopropylacrylamide-acrylic acid copolymer microgel: when the ambient temperature is below the low critical dissolution temperature, the microgel is in a swollen state, the permeability of the coating layer is low, and water release is slow; when the temperature rises above the low critical dissolution temperature, the microgel shrinks, the permeability of the coating layer increases, and water release accelerates. This intelligent response characteristic enables the material to retain moisture when the wetland temperature is low and accelerate the release when the temperature rises, achieving intelligent water replenishment that matches the water requirements of wetland plants.
[0068] Comparative Example 1, lacking a coating layer, has a water release rate less affected by temperature and does not possess intelligent response characteristics. Although Comparative Example 2 has a certain slow-release effect, due to the lack of temperature-responsive components, its water release rate varies much less under different temperature conditions than that of Examples 1-3.
[0069] 4. Performance analysis of reuse As shown in Table 1, after five water absorption-drying cycles, the repeat water absorption rates of Examples 1-3 were 82.6%, 79.3%, and 84.1%, respectively, all higher than those of Comparative Examples 1, 2, 3, and 4. This indicates that the complete technical solution of the present invention has optimal structural stability and reusability. The coating layer maintained its complete structural integrity during multiple water absorption-drying cycles, effectively protecting the water absorption network structure of the core.
[0070] 5. pH response performance analysis Table 2 shows that the water absorption ratio of Examples 1-3 exhibits a clear trend under different pH conditions—the highest water absorption ratio is observed in the pH range of 6.0-8.0, while the water absorption ratio decreases under acidic and alkaline conditions. Compared to Comparative Examples 1-4, Examples 1-3 show a more significant pH response, which is attributed to the pH-responsive characteristics of the calcium alginate-chitosan complex in the coating layer: under acidic conditions, the protonation of chitosan amino groups leads to coating layer shrinkage; under alkaline conditions, the deprotonation of alginate carboxyl groups leads to coating layer swelling, thereby regulating the permeation rate of water molecules. This characteristic allows the material to automatically adjust its release behavior according to pH changes in wetland water.
[0071] The water absorption ratio of Comparative Example 4 was significantly lower than that of Example 1 under all pH conditions, further confirming the indispensable contribution of potassium humate to the overall water absorption performance of the material.
[0072] 6. Comprehensive performance comparison and creative analysis Based on the above performance indicators, Examples 1-3 are significantly better than Comparative Examples 1-4 in terms of water retention rate, slow release time, temperature responsiveness, pH responsiveness, and reusability.
[0073] Although Comparative Example 1 has the highest water absorption ratio (498g / g), its water retention rate and slow-release performance are the worst. It only takes 36 hours to achieve a cumulative water release rate of 80%, which cannot meet the actual needs of wetland ecological water replenishment for long-term slow release.
[0074] Comparative Example 2 improved water retention and sustained-release performance to some extent by coating with a single calcium alginate-chitosan, but due to the lack of temperature-responsive components, its intelligent regulation ability under different temperature conditions was insufficient, and it took 62 hours to achieve a cumulative water release rate of 80%, which was still far lower than that of Example 1.
[0075] The performance of Comparative Example 3 is between that of Comparative Example 2 and Comparative Example 4, which proves that the "two-stage variable temperature gradient crosslinking" process has significant advantages over conventional isothermal polymerization. The gradient crosslinking structure makes the crosslinking density inside the material gradient, which not only ensures the high water absorption capacity of the core, but also enhances the density and mechanical strength of the surface layer.
[0076] Comparative Example 4 was inferior to Example 1 in all performance indicators, especially in water absorption ratio (412 g / g vs 486 g / g, a decrease of 15.2%) and time required to reach 80% cumulative water release rate (75 h vs 96 h, a reduction of 21.9%). This fully demonstrates that potassium humate is not a simple nutrient additive, but rather, through graft crosslinking reaction with acrylic acid-acrylamide copolymer, it significantly enhances the integrity and hydrophilicity of the three-dimensional network structure, producing an enhanced synergistic effect.
[0077] The above four sets of comparative examples systematically verify the synergistic effect of the core technical features of the present invention: pH / temperature dual-response coating mixture, two-stage variable temperature gradient crosslinking process, and in-situ composite crosslinking of potassium humate. All three are indispensable and together constitute the creative contribution of the present invention.
[0078] VI. Specific Application Examples The slow-release water-retaining material prepared in Example 1 of this invention was applied to an ecological water replenishment experiment in a degraded wetland area. The experiment included three treatment groups (application rates of 50 g / m²). 2 100g / m 2 150g / m 2 The study included one control group and three replicates (2m × 2m) for each treatment. In March 2025, the materials were evenly applied to the topsoil (0-20cm). Soil moisture content, vegetation cover, and aboveground biomass were measured monthly for five consecutive months (March to July). The results are as follows: Table 4 Results of Wetland Ecological Water Replenishment Application Experiment
[0079] Experimental results showed that after applying the slow-release water-retaining material of this invention, the soil moisture content in treatment group 2 increased by 54.6% compared to the control group, vegetation cover increased by 44.4%, and aboveground plant biomass increased by 65.4%. The effective water replenishment period reached 108 days. Considering both economic efficiency and effectiveness, the recommended application rate is 100 g / m². 2 This material shows promising application prospects for wetland ecological water replenishment.
[0080] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A slow-release water-retaining formulation material for wetland ecological water replenishment, characterized in that, It is prepared from the following raw materials in parts by weight: 30-55 parts of composite water-retaining active mixture, 5-15 parts of pH / temperature dual-response slow-release coating mixture, 0.5-3 parts of crosslinking agent, 0.3-2 parts of initiator, and 50-100 parts of deionized water, which are used as preparation water; The composite water-retaining active mixture is prepared by in-situ compounding of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate, wherein the weight ratio of modified biochar, acrylic acid-acrylamide copolymer, sodium alginate, attapulgite and potassium humate is (20-40):(15-30):(5-15):(10-25):(3-10); The pH / temperature dual-responsive sustained-release coating mixture is composed of N-isopropylacrylamide-acrylic acid copolymer microgel and calcium alginate-chitosan complex in a weight ratio of 1:0.5-1:
3.
2. The slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 1, characterized in that, The modified biochar is prepared by pyrolyzing reed straw at 400-600℃ under limited oxygen, followed by oxidation treatment with 10%-20% hydrogen peroxide solution for 2-4 hours, and then impregnating and modifying it in an aqueous acetic acid solution with 5%-15% chitosan for 12-24 hours.
3. The slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 1, characterized in that, The acrylic acid-acrylamide copolymer has a molar ratio of acrylic acid to acrylamide of 1:0.3-1:0.8, and the degree of neutralization of the acrylic acid is 60%-80%.
4. The slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 1, characterized in that, The N-isopropylacrylamide-acrylic acid copolymer microgel has an average particle size of 100-500 nm and a lower critical dissolution temperature of 32-38 °C.
5. A slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 1, characterized in that, The crosslinking agent is a composite crosslinking agent composed of N,N′-methylenebisacrylamide and borax in a mass ratio of 2:1-5:1; the initiator is a redox initiation system composed of ammonium persulfate and sodium bisulfite in a mass ratio of 1:1-3:
1.
6. A method for preparing a slow-release water-retaining formulation material for wetland ecological water replenishment as described in any one of claims 1-5, characterized in that, Includes the following steps: Step S1: Preparation of the composite water-retaining active mixture: Modified biochar, attapulgite, and potassium humate are mixed evenly according to the specified ratio and ground until the particle size is no greater than 200 mesh to obtain a mixed powder; acrylic acid-acrylamide copolymer is dissolved in deionized water to prepare a polymer solution with a mass fraction of 10%-20%; sodium alginate is added under stirring and stirring is continued until completely dissolved to obtain a polymer mixture; the mixed powder is added to the polymer mixture and stirred evenly; then a crosslinking agent and an initiator are added sequentially; the first stage reaction is carried out at 40-70℃ for 1-3 hours, and then the temperature is raised to 75-90℃ for the second stage reaction for 1-3 hours to obtain a gel-like composite water-retaining active mixture with a gradient crosslinking structure; Step S2: Extrude the gel-like composite water-retaining active mixture obtained in step S1 into granules, control the particle size to 2-10 mm, and dry it at 50-80℃ until the water content is no more than 10% to obtain slow-release water-retaining matrix particles. Step S3, Preparation of pH / temperature dual-response sustained-release coating mixture: N-isopropylacrylamide and acrylic acid are dissolved in deionized water at a molar ratio of 10:1-5:1, a crosslinking agent and an initiator are added, and the polymerization reaction is carried out at 60-80℃ for 4-8 hours to obtain N-isopropylacrylamide-acrylic acid copolymer microgel; the microgel is mixed with calcium alginate-chitosan complex at a weight ratio of 1:0.5-1:3 to prepare a coating solution with a mass fraction of 5%-15%; Step S4, Coating and Curing: The matrix particles obtained in step S2 are immersed in the coating solution obtained in step S3 for 10-30 minutes. After being removed, they are placed in a calcium chloride solution with a mass fraction of 1%-5% for curing and crosslinking for 10-60 minutes. After being removed, they are dried in a forced-air drying oven at 30-50℃ to obtain the slow-release water-retaining material for wetland ecological water replenishment.
7. The method for preparing a slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 6, characterized in that, In step S1, the first stage reaction temperature is 50-60℃ and the reaction time is 2h; the second stage reaction temperature is 80-85℃ and the reaction time is 2h.
8. The method for preparing a slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 6, characterized in that, In step S3, the molar ratio of N-isopropylacrylamide to acrylic acid is 8:1-6:1, the polymerization temperature is 70-75℃, and the reaction time is 5-7h.
9. A method for preparing a slow-release water-retaining formulation material for wetland ecological water replenishment according to claim 6, characterized in that, The impregnation and coating time in step S4 is 15-25 min, and the curing and crosslinking time of the calcium chloride solution is 20-40 min.
10. The application of the slow-release water-retaining material for wetland ecological water replenishment according to any one of claims 1-5 in wetland soil water retention, wetland vegetation restoration, or wetland ecological water replenishment.