Flange heat treatment process based on gradient temperature field cooperative control

By using a gradient temperature field-controlled flange heat treatment process, the problems of uneven microstructure and unfavorable residual stress distribution in large-section flanges have been solved. This process achieves a microstructure gradient with priority given to core toughness and high surface strength, as well as a favorable stress distribution, thereby improving the flange's service performance and dimensional stability.

CN123063593APending Publication Date: 2026-11-10JIANGYIN BOHON MASCH FLANGES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611511589.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Large-section flanges, due to differences in cross-sectional dimensions after forging, exhibit uneven microstructure and unfavorable residual stress distribution, which are difficult to effectively control with existing heat treatment processes, easily leading to fatigue cracks and deformation problems.

Method used

The flange heat treatment process employing gradient temperature field coordinated control, through zoned temperature control and zoned differential cooling, allows the flange core and surface to undergo different phase transformation paths, forming a reverse temperature gradient and a favorable residual stress distribution.

Benefits of technology

This achieves a gradient distribution of microstructure with priority given to core toughness and high surface strength, and the residual stress is changed from "external pressure and internal tension" to "external tension and internal pressure", reducing quenching deformation and improving the service performance and dimensional stability of the flange.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application discloses a flange heat treatment process based on gradient temperature field cooperative control and belongs to the technical field of metal heat treatment. The process comprises gradient heating, reverse temperature equalization, partition differential cooling and subcritical tempering steps. The core of the process is that: the core is firstly completed austenitizing through partition temperature control, and then the temperature gradient of the core is higher than the surface through reverse temperature equalization; after discharging, the cooling rate of the neck area is much higher than that of the end surface, so that the neck is firstly phase transition to form a compression stress source, and the end surface is in a tensile state under the constraint of the compression stress after lagging phase transition. The application overcomes the problems of uneven structure and "external compression and internal tension" residual stress distribution caused by conventional homogenization heat treatment, so that the flange obtains the gradient performance of high toughness in the core, high strength on the surface and favorable residual stress distribution, and the quenching deformation is significantly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal heat treatment technology, and more specifically to a heat treatment process for large-section flanges used to eliminate microstructure inhomogeneity and residual stress gradients in flange forgings. Background Technology

[0002] Flanges are critical connecting components in pipelines, wind turbine towers, pressure vessels, and other fields. Their service conditions require flanges to possess both high strength and toughness, as well as dimensional stability. During the cooling process after forging, large-section flanges exhibit inherent gradients in cooling rates due to differences in cross-sectional dimensions. This leads to two core issues: First, a significant difference in microstructure arises between the core and the surface layer. The surface layer, due to its faster cooling rate, tends to form bainite or martensite, while the core, with its slower cooling rate, retains ferrite-pearlite. This microstructure inhomogeneity results in differentiated mechanical responses during subsequent machining and service. Second, residual stress exhibits an unfavorable "external compression, internal tension" distribution. Rapid cooling of the surface layer creates compressive stress, while delayed cooling of the core creates tensile stress. The superposition of residual tensile stress with service loads can easily induce fatigue crack initiation.

[0003] Current flange heat treatment processes mostly employ a homogenization route of "overall heating – overall quenching – high-temperature tempering," attempting to obtain a uniform martensitic structure through sufficient austenitization and rapid cooling, followed by tempering to adjust to the target properties. However, for large-section flanges with a cross-sectional thickness exceeding 200 mm, overall quenching cannot achieve effective hardening of the core; instead, the significant difference in cooling rates between the core and surface layers leads to more severe microstructure gradients and stress concentrations. Some existing technologies attempt to improve temperature uniformity through spray cooling or segmented heating, but these approaches still treat the flange as a "whole body with a temperature field to be homogenized," failing to utilize the temperature gradient itself as a process variable to control the microstructure distribution.

[0004] Therefore, a flange heat treatment process is needed that can actively utilize rather than passively eliminate the temperature gradient effect, so as to achieve a controllable distribution of residual stress while ensuring that both the core and the surface layer achieve the target performance. Summary of the Invention

[0005] To address the aforementioned technical problems, this invention provides a flange heat treatment process. Its core concept is: instead of pursuing complete homogenization of the temperature field during heating and cooling, it designs a synergistic scheme of "reverse temperature gradient" and "regional differential cooling" to allow the flange core and surface to undergo different phase transformation paths during heat treatment. This results in a gradient structure where the core is dominated by a tough phase and the surface is dominated by a strengthening phase, and the residual stress is adjusted from "external pressure and internal tension" to a favorable distribution of "external tension and internal pressure".

[0006] To achieve the above objectives, the present invention adopts the following technical solution:

[0007] A flange heat treatment process based on gradient temperature field synergistic control includes the following steps:

[0008] S1. The forged flange is placed into a heat treatment furnace. The temperature is controlled in zones so that the core temperature of the flange reaches the austenitizing temperature T1 first and completes austenitization, while the surface temperature lags behind the core temperature.

[0009] S2, after the core is austenitized, the furnace temperature is lowered to a temperature range T2 below T1, so that the surface temperature is lowered to T2 while the core remains in a fully austenitic state, forming a reverse temperature gradient where the core temperature is higher than the surface temperature.

[0010] S3, remove the flange from the furnace, apply a first cooling rate V1 to the axial end face of the flange, and apply a second cooling rate V2 to the neck region of the flange, where V2>V1, so that the neck region undergoes phase change first and forms a compressive stress source in the flange.

[0011] S4, the cooled flange is subjected to subcritical tempering at a temperature lower than A1.

[0012] S5, cool to room temperature;

[0013] Where T1 is the austenitizing temperature, T2 is the temperature below T1 but above A1, A1 is the eutectoid transformation temperature of the steel, V1 is the cooling rate of the axial end face, and V2 is the cooling rate of the neck region.

[0014] Specifically, in step S1, the core reaches the austenitizing temperature first, which is achieved by setting an induction heating coil or a forced convection nozzle in the core region, so that the heating rate of the core is 20% to 50% higher than that of the surface layer.

[0015] Specifically, in step S2, the reverse temperature gradient is formed as follows: after the austenitization of the core is completed, the active heating of the core region is stopped, the furnace temperature is lowered to T2 and held for 0.8 to 1.5 hours, so that the surface temperature is lowered to T2 while the core maintains a temperature difference of 10 to 30°C higher than the surface due to thermal inertia.

[0016] Specifically, in step S3, the first cooling rate V1 is 5~15°C / s, the second cooling rate V2 is 25~60°C / s, and V2 / V1 is 3~6.

[0017] Specifically, in step S3, the cooling of the axial end face is achieved by uniformly spraying an annular spray device along the outer circumference of the flange, and the cooling of the neck area is achieved by using multiple nozzles arranged along the flange axis for air-water mist mixed cooling.

[0018] Specifically, in step S3, the control method for the neck region to undergo phase transformation first is as follows: after the neck temperature drops below the bainite transformation start temperature, the end face temperature remains above the bainite transformation start temperature, so that the neck phase transformation leads the end face phase transformation by at least 60 seconds.

[0019] Specifically, in step S4, the subcritical tempering temperature is 550~620°C, and the holding time is calculated as 2~3 min / mm based on the maximum cross-sectional thickness of the flange.

[0020] Specifically, in step S4, the subcritical tempering adopts a segmented tempering method: first, the surface strengthening phase is initially softened by holding at 580~620°C for 1~2 hours, and then the temperature is lowered to 550~580°C and held until the total time meets the requirement of sufficient recovery of the core toughness phase.

[0021] Specifically, in step S5, the cooling to room temperature is achieved by furnace cooling, air cooling, or protective atmosphere cooling, with the cooling rate controlled at 0.05~0.5°C / s.

[0022] Specifically, the flange is a carbon steel or low alloy steel flange with a maximum cross-sectional thickness of not less than 150mm, and the process is applicable to necked welding flanges, slip-on flanges, or flange covers.

[0023] The flange heat treatment process based on gradient temperature field coordinated control of the present invention has the following advantages compared with the prior art:

[0024] (1) Active regulation of organizational distribution;

[0025] Existing homogenization heat treatment approaches aim for consistency in microstructure between the core and surface layers. However, for large-section flanges, this goal is practically difficult to achieve and is not optimal. The reverse temperature gradient and zoned differential cooling of this invention allow the core cooling path to avoid the martensitic transformation region, retaining more tough phases (such as bainitic ferrite or tempered sorbite), while the surface layer obtains a refined strengthening phase microstructure through a faster cooling rate. The final flange exhibits a gradient distribution with superior core toughness and high surface strength, perfectly matching the stress characteristics of the flange during service: the surface layer bears contact stress and corrosion, while the core bears overall bending and tensile stress.

[0026] (2) Reversal of residual stress distribution;

[0027] In conventional quenching and cooling, the surface layer cools and contracts first, creating compressive stress on the still-warm core. The core cools and contracts later, generating tensile stress due to the constraint of the surface layer, ultimately forming a stress pattern of "surface compression, core tension." The residual tensile stress in the core, combined with the service tensile load, is a major cause of fatigue failure in large-section flanges. This invention preferentially and rapidly cools the neck region, allowing phase transformation expansion in this area to occur while the flange as a whole is still at a relatively high temperature and with weaker constraints, forming an active compressive stress source. When the end face region cools later, its phase transformation expansion is constrained by the already "locked" neck compressive stress, resulting in a favorable tensile state after cooling. This "external tension and internal compression" stress distribution is advantageously superimposed with the direction of the service load.

[0028] (3) Eliminate the need for post-quenching shaping;

[0029] Large-section flanges often exhibit excessive ellipticity or flatness deviations after conventional quenching due to the combined effects of phase transformation and thermal stress, requiring additional straightening processes or machining allowances. The differential cooling scheme of this invention ensures the orderly connection of the phase transformation process between the neck and end face, actively guiding deformation during cooling rather than correcting it afterward, resulting in a significant reduction in the ellipticity and flatness deviations of the flange after cooling. Detailed Implementation

[0030] The present invention will be further described in detail below with reference to the embodiments.

[0031] Example 1: 16Mn necked welding flange (maximum cross-sectional thickness 180mm)

[0032] Flange specifications and materials: DN800PN16 welding neck flange, material 16Mn (chemical composition: C0.17%, Si0.35%, Mn1.45%, P0.018%, S0.012%, balance Fe), forged and pre-treated by normalizing, maximum cross-sectional thickness is about 180mm, flange outer diameter is about 1015mm, and neck diameter is about 820mm.

[0033] S1 Gradient Heating: The flange is placed into a bogie-type heat treatment furnace, and three silicon carbide heating rods (each with a power of 15kW) are inserted into the inner bore of the flange, with the rods approximately 30mm from the inner wall of the flange. Resistance heating elements on both sides of the furnace heat to 920°C at a rate of 8°C / min, while the core heating rod is heated separately with a power supply at 12°C / min. The core thermocouple (embedded at 1 / 2 of the flange wall thickness) reaches 910°C after 1.8 hours, while the surface thermocouple (embedded 10mm below the flange surface) reaches 845°C at the same time, with the core leading the surface by approximately 65°C. After holding at this temperature for another 0.6 hours, the surface temperature reaches 905°C, and the core reaches 915°C, both having entered the fully austenitic region.

[0034] S2 Reverse Isostatic Temperature Control: Power supply to the core heating rod is stopped, and the furnace temperature is controlled to drop to 860°C. After holding for 1.2 hours, the core thermocouple temperature is 865°C, and the surface thermocouple temperature is 848°C. The core temperature is still about 17°C higher than the surface temperature, and the core temperature is in the fully austenitic region (A3 of 16Mn is about 830°C). Although the surface temperature is lower than the core temperature, it is still higher than A1 (about 720°C), and no proeutectoid ferrite precipitation has occurred.

[0035] S3 Differential Cooling: After the flange exits the furnace, the outer annular end face is cooled at a rate of 10°C / s by 12 circumferentially arranged air atomizing nozzles (nozzle orifice diameter 1.5mm, air pressure 0.4MPa, water flow rate 0.8L / min); simultaneously, the flange neck is cooled at a rate of 40°C / s by 6 axially arranged high-pressure air-water mist mixing nozzles (air pressure 0.6MPa, water flow rate 1.5L / min). The neck temperature drops below 450°C in approximately 90s (monitored by thermocouples 10mm below the surface), and the end face temperature drops below 450°C after approximately 360s. The neck phase transformation precedes the end face phase transformation by approximately 120 seconds, and the bainitic structure formed first in the neck establishes a compressive stress field in the flange.

[0036] S4 subcritical tempering: Temper at 580°C, hold for 4.5 hours (calculated at 180mm × 2.5min / mm), then air cool. After tempering, the core microstructure consists of tempered sorbite + bainitic ferrite, and the surface layer consists of tempered bainite + a small amount of tempered martensite.

[0037] S5 final cooling: air cooling to room temperature.

[0038] Performance test results (Table 1):

[0039] Table 1

[0040]

[0041] As can be seen from the comparison, Example 1 maintains high hardness on the neck surface while exhibiting significantly better core toughness than the comparative example. Furthermore, the residual stress distribution changes from "external pressure and internal tension" to "external tension and internal pressure," resulting in a reduction of approximately 70% in quenching deformation.

[0042] Example 2: Q345E weld neck flange (maximum cross-sectional thickness 250mm)

[0043] Flange specifications and materials: DN1200PN25 necked welding flange, material Q345E (chemical composition: C0.15%, Si0.30%, Mn1.50%, Nb0.03%, V0.05%, P0.015%, S0.010%, balance Fe), maximum cross-sectional thickness approximately 250mm.

[0044] S1 gradient heating: The flange is installed in a bogie-type heat treatment furnace, and five silicon carbide heating rods (each with a power of 20kW) are inserted into the inner hole of the flange. The core heating rods are heated at 10°C / min, and the heating elements in the furnace are heated at 7°C / min to 930°C. The core reaches 920°C in 2.5 hours, and the surface layer reaches 915°C in 3.2 hours, with the core leading by 0.7 hours.

[0045] S2 Reverse Irrigation: Power supply to the core heating rod is stopped, furnace temperature drops to 870°C, and held for 1.5 hours. Core temperature is 878°C, surface temperature is 858°C, temperature difference is 20°C, and the core is still in the fully austenitic region.

[0046] S3 zone differential cooling: The end face is cooled by 16 air atomizing nozzles at 8°C / s, and the neck is cooled by 8 high-pressure air-water mist mixing nozzles at 35°C / s. The neck temperature drops below 480°C in approximately 120 seconds, and the end face temperature drops below 480°C after approximately 480 seconds. The neck phase change leads the end face by approximately 150 seconds.

[0047] S4 subcritical tempering: segmented tempering is adopted: first, hold at 610°C for 1.5h, then lower to 570°C and hold for 5.0h (total time is calculated at 250mm×2.6min / mm), and then air cool after furnace cooling to 300°C.

[0048] S5 final cooling: air cooling to room temperature.

[0049] Performance test results (Table 2):

[0050] Table 2

[0051]

[0052] Example 3: 40Cr flat-face welding flange (maximum cross-sectional thickness 150mm)

[0053] Flange specifications and materials: DN600PN40 flat welding flange, material 40Cr (chemical composition: C0.40%, Si0.25%, Mn0.65%, Cr0.95%, P0.020%, S0.015%, balance Fe), maximum cross-sectional thickness approximately 150mm.

[0054] S1 gradient heating: The flange is installed in a pit-type heat treatment furnace, and an induction heating coil (frequency 2kHz, power 30kW) is installed in the core. The furnace resistance heating raises the temperature to 850°C at 9°C / min, and the induction coil assists in heating the core at 14°C / min. The core reaches 845°C in 1.5 hours, and the surface layer reaches 840°C in 2.0 hours.

[0055] S2 Reverse Temperature Equalization: Induction heating is stopped, furnace temperature drops to 800°C, and held for 1.0 h. Core temperature is 808°C, surface temperature is 790°C, temperature difference is 18°C.

[0056] S3 zone differential cooling: The end face is cooled by 10 air atomizing nozzles at 12°C / s, and the neck is cooled by 6 high-pressure air-water mist mixing nozzles at 50°C / s. The neck temperature drops below 400°C in approximately 70 seconds, and the end face temperature drops below 400°C after approximately 280 seconds. The neck phase change leads the end face by approximately 100 seconds.

[0057] S4 subcritical tempering: segmented tempering is adopted: first, hold at 600°C for 1.2h, then lower to 560°C and hold for 3.5h, followed by air cooling.

[0058] S5 final cooling: air cooling to room temperature.

[0059] Performance test results (Table 3):

[0060] Table 3

[0061]

[0062] Example 4: 16Mn flange cover (maximum cross-sectional thickness 200mm)

[0063] Flange specifications and materials: DN1000PN16 flange cover, material 16Mn, maximum cross-sectional thickness approximately 200mm.

[0064] S1 gradient heating: The flange cover is installed in a bogie-type heat treatment furnace, and three forced convection nozzles (wind speed 15m / s, temperature 950°C) are set at the corresponding position in the core, so that the heating rate of the core is 30% higher than that of the surface. The core reaches 915°C in 2.0h, and the surface reaches 910°C in 2.6h.

[0065] S2 Reverse Temperature Irrigation: Forced convection is stopped, furnace temperature drops to 865°C, and held for 1.3 hours. Core temperature is 872°C, surface temperature is 855°C, temperature difference is 17°C.

[0066] S3 zone differential cooling: The flange end face is cooled by 14 air atomizing nozzles at 9°C / s, while the neck is cooled by 7 high-pressure air-water mist mixing nozzles at 38°C / s. The neck cools to below 460°C within approximately 100 seconds, and the end face cools to below 460°C after approximately 400 seconds. The neck phase change leads the end face by approximately 130 seconds.

[0067] S4 subcritical tempering: 590°C for 5.0h (calculated at 200mm×2.5min / mm), then air cooling.

[0068] S5 final cooling: air cooling to room temperature.

[0069] Performance test results (Table 4):

[0070] Table 4

[0071]

[0072] Comparative Example 1: Conventional integral quenching process

[0073] For the flange of the same specifications as in Example 1, conventional processes were used: overall heating and holding at 920°C for 3 hours, water quenching (cooling rate approximately 80°C / s), tempering at 600°C for 4 hours, and air cooling. Test results are shown in the comparison table for Example 1.

[0074] Comparative Example 2: Gradient heating only, without zoned cooling

[0075] For the flange of the same specifications as in Example 1, after gradient heating (S1) and reverse uniform cooling (S2), the entire flange was uniformly cooled at 20°C / s (at the same speed as the neck) and tempered at 580°C for 4.5 hours. Test results: residual stress at the neck +15MPa (tensile), residual stress at the end face +48MPa (tensile), core impact energy 42J, and ellipticity deviation 1.5mm. It is evident that without zoned differential cooling, the residual stress distribution was not reversed, and the improvement in core toughness was limited.

[0076] Comparative Example 3: Zoned cooling only, no gradient heating

[0077] For the flange of the same specification as in Example 1, conventional overall heating to 920°C and holding for 3 hours was followed by differential cooling in S3 zones (10°C / s for the end face and 40°C / s for the neck), and tempering at 580°C for 4.5 hours. Test results: residual stress at the neck -45MPa (compressive), residual stress at the end face +50MPa (tensile), core impact energy 38J, and ellipticity deviation 1.2mm. It is evident that without gradient heating and reverse homogenization, the core did not achieve sufficient austenitizing temperature advantage, resulting in minimal improvement in toughness and a small reversal of residual stress.

[0078] As can be seen from the comparison of Examples 5-7, the three core steps of the present invention—gradient heating, reverse temperature equalization, and zoned differential cooling—have a synergistic effect. The expected tissue gradient and stress reversal effect cannot be achieved without any of these steps.

[0079] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited to the embodiments described. Those skilled in the art can make various equivalent modifications or substitutions without departing from the spirit of the present invention, and these equivalent modifications or substitutions are all included within the scope defined by the claims of this application.

Claims

1. A flange heat treatment process based on gradient temperature field synergistic control, characterized in that, Includes the following steps, S1. The forged flange is placed into the heat treatment furnace. The temperature is controlled in zones so that the core temperature of the flange reaches the austenitizing temperature T1 first and completes austenitizing, while the surface temperature lags behind the core temperature. S2, after the core is austenitized, the furnace temperature is lowered to a temperature range T2 below T1, so that the surface temperature is lowered to T2 while the core remains in a fully austenitic state, forming a reverse temperature gradient where the core temperature is higher than the surface temperature. S3, remove the flange from the furnace, apply a first cooling rate V1 to the axial end face of the flange, and apply a second cooling rate V2 to the neck region of the flange, where V2>V1, so that the neck region undergoes phase change first and forms a compressive stress source in the flange. S4, the cooled flange is subjected to subcritical tempering at a temperature lower than A1. S5, cool to room temperature; Where T1 is the austenitizing temperature, T2 is the temperature below T1 but above A1, A1 is the eutectoid transformation temperature of the steel, V1 is the cooling rate of the axial end face, and V2 is the cooling rate of the neck region.

2. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S1, the core reaches the austenitizing temperature first, which is achieved by setting an induction heating coil or a forced convection nozzle in the core region, so that the heating rate of the core is 20% to 50% higher than that of the surface layer.

3. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S2, the reverse temperature gradient is formed as follows: after the austenitization of the core is completed, the active heating of the core region is stopped, the furnace temperature is lowered to T2 and held for 0.8 to 1.5 hours, so that the surface temperature is lowered to T2 while the core maintains a temperature difference of 10 to 30°C higher than the surface due to thermal inertia.

4. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S3, the first cooling rate V1 is 5~15°C / s, the second cooling rate V2 is 25~60°C / s, and V2 / V1 is 3~6.

5. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S3, the axial end face is cooled by uniformly spraying an annular spray device along the outer circumference of the flange, and the neck area is cooled by a combination of air and water mist from multiple nozzles arranged along the flange axis.

6. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S3, the specific control method for the neck region to undergo phase transformation first is as follows: after the neck temperature drops below the bainite transformation start temperature, the end face temperature remains above the bainite transformation start temperature, so that the neck phase transformation leads the end face phase transformation by at least 60 seconds.

7. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S4, the subcritical tempering temperature is 550~620°C, and the holding time is calculated as 2~3 min / mm based on the maximum cross-sectional thickness of the flange.

8. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S4, the subcritical tempering adopts a segmented tempering method: first, the surface strengthening phase is initially softened by holding at 580~620°C for 1~2 hours, and then the temperature is reduced to 550~580°C and held until the total time meets the requirement of sufficient recovery of the core toughness phase.

9. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, In step S5, the cooling to room temperature is achieved by furnace cooling, air cooling, or protective atmosphere cooling, with the cooling rate controlled at 0.05~0.5°C / s.

10. The flange heat treatment process based on gradient temperature field synergistic control according to claim 1, characterized in that, The flange is made of carbon steel or low alloy steel, with a maximum cross-sectional thickness of not less than 150 mm, and the process is applicable to weld neck flanges, slip-on flanges, or flange covers.