A method for separating the oil phase and solid phase in neodymium iron boron sludge waste.
By using azeotropic distillation and reflux extraction with organic solvents, the problem of oil-solid separation in NdFeB sludge waste was solved, achieving efficient, green, and low-energy separation of the oil and solid phases, resulting in high oil removal rate and resource recovery.
Patent Information
- Application Number
- CN202611466036.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies for NdFeB oil sludge waste are difficult to separate from oil, cause heavy pollution, and consume a lot of energy, making it difficult to achieve efficient and green separation and resource recovery.
Azeotropic distillation and reflux extraction with organic solvents are employed. Deep separation of the oil and solid phases is achieved through an azeotropic distillation apparatus and organic solvents LLR1 or LLR2. The non-polar or polar properties of the organic solvents are utilized to form azeotropes with water, simultaneously removing emulsified water and avoiding high-temperature calcination.
It achieves efficient oil-solid separation with an oil removal rate of 97.89%~99.86%, reducing energy consumption, solvent consumption, and environmental pollution, and ensuring the green and low-carbon recycling of rare earth resources.
Smart Images

Figure CN123063601A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of comprehensive utilization technology of rare earth permanent magnet secondary resources, specifically involving a method for separating the oil phase and solid phase in neodymium iron boron sludge waste. Background Technology
[0002] Rare earth elements are a type of non-renewable and scarce strategic mineral resource. The efficient recycling of secondary rare earth resources, exemplified by NdFeB permanent magnet waste, offers a highly valuable and promising solution to the current severe shortage of rare earth elements. As the world's largest producer and consumer of NdFeB permanent magnet materials, China generates 30-40% magnetic waste, including cutting edges and grinding sludge, during the production and processing of NdFeB permanent magnets through multiple steps such as cutting and grinding. The processing uses oily reagents such as mineral oil, coolants, and cleaning agents, which, along with cutting, grinding, and sintering waste, flow into the collection system, ultimately forming a multiphase, high-organic-load, fine-particle, and highly adhesive sludge waste, accounting for approximately 25-30%. In recent years, to improve production efficiency, permanent magnet material production has upgraded cutting equipment, increasing the proportion of NdFeB sludge waste to 40-60%. Oil sludge waste contains 20% to 30% rare earth elements (Nd, Pr, Dy, etc.) and 60% to 70% valuable components such as Fe. The waste also contains impurities such as carbon and oxygen. If not properly treated, it will not only waste resources but also cause serious harm to the environment.
[0003] While current mainstream roasting methods are simple and efficient, they are limited by the inherent defects of rotary kilns. Precise control of temperature and atmosphere is difficult, and incomplete combustion during the oil removal process is a significant problem. This not only produces black waste gas rich in tar, soot, and nitrogen oxides, but also easily damages production equipment. Even with end-of-pipe treatment, it is difficult to achieve emission standards. Furthermore, the direct combustion of high-oil-content materials is itself a waste of oil phase resources. Based on the difference in wettability between the oil phase and NdFeB black powder, oily sludge waste can be divided into two categories: water-based coolant sludge and oil-based sludge waste. Compared to water-based sludge, oil-based sludge exhibits strong adhesion between high-viscosity mineral oils and micron-sized NdFeB particles. On one hand, its composition is highly complex, containing a large amount of high-boiling-point organic matter and high carbon and hydrogen content, making water-based sludge cleaning methods unsuitable. On the other hand, the oil residue tightly coats the particle surface and the interior of agglomerates, severely affecting cleaning efficiency, resulting in high energy consumption and low efficiency in physical separation. Furthermore, residual oil and oxidized impurities on the surface of solid particles significantly interfere with and hinder the efficient leaching and mass transfer of rare earth elements in subsequent hydrometallurgical processes, directly impacting the purity and consistency of the final rare earth product. Therefore, there is an urgent need to develop a novel pretreatment technology for fine-particle, highly adhesive, multiphase mixed, and complex oil-based sludge materials to achieve efficient oil phase removal, dual recovery of oil and NdFeB, and ensure a clean and low-carbon process throughout, thereby supporting the high-value utilization of rare earth secondary resources and the sustainable development of the industry.
[0004] In the field of NdFeB oil sludge recycling, the difficulty of oil-solid separation, heavy pollution, and high energy consumption have always been key challenges restricting its green and efficient treatment. Researchers have conducted extensive research to address these issues. Patents CN102912112A and CN102899479A disclose a pretreatment method for NdFeB waste oil sludge. This method involves distilling the oil sludge waste at 50-100℃ and 0.01-0.1 MPa. The distillation product is then subjected to acid dissolution, impurity removal, extraction separation, precipitation, and calcination to obtain rare earth oxides. This process, using distillation as a pretreatment method, suffers from high energy consumption, making it difficult to meet the economic requirements of industrial applications. CN114317974B discloses a pretreatment method for NdFeB oily sludge waste. This method uses a process route of "centrifugal solid-liquid separation—leaching—filtration—vacuum drying—sieving" to treat NdFeB oily sludge waste. The solvents used in this method are mostly non-polar or weakly polar organic solvents, which are difficult to destroy the three-phase emulsion structure of oil-water-solid in the sludge waste. The ability to remove emulsion-state oily sludge is limited, so it is necessary to repeat the leaching process six times. The oil-solid separation efficiency cannot be quantitatively measured, and the solvent consumption is large. CN119296943A discloses a treatment process for removing impurities from NdFeB oily sludge. This process uses a five-step washing process of "sieving—washing with organic mixed solution—washing with weakly acidic aqueous solution—washing with alkaline aqueous solution—washing with water—washing with organic solvent—vacuum drying". The ultrasonic washing operation in the pretreatment process of this process is extremely cumbersome, and the processing time per batch is too long, which is difficult to meet the efficiency requirements of large-scale industrial production. Secondly, the oil phase after washing with the organic mixed solution is discharged with the liquid without being recycled, resulting in the waste of oil resources, which is inconsistent with the requirements of green, low-carbon, and resource recycling. Furthermore, acid-base washing and water washing generate large amounts of wastewater containing acids, alkalis, salts, surfactants, and organic matter. The instruction manual does not address wastewater treatment or recycling solutions, posing a significant environmental risk. Therefore, there is an urgent need to develop a pretreatment method for NdFeB oil sludge waste that features high oil-solid separation efficiency, low solvent consumption, short processing time, recoverable oil phase, and low environmental risk, in order to overcome the aforementioned shortcomings of existing technologies and achieve efficient and green separation of the oil and solid phases in NdFeB oil sludge waste. Summary of the Invention
[0005] The purpose of this invention is to provide a method for separating the oil phase and solid phase in NdFeB sludge waste, overcoming the challenge of green dissociation at the oil-solid interface and achieving deep separation of the oil phase and NdFeB solid powder. Addressing the problems of strong adhesion at the oil-solid-water interface in existing technologies, which hinders efficient dissociation, severe environmental pollution and resource waste during calcination degreasing, and the high solvent consumption and low processing efficiency of conventional leaching methods, this invention proposes a green extraction process based on organic solvents. Through azeotropic distillation, it achieves efficient separation and recycling of NdFeB, lubricating oil, and solvent, providing a theoretical basis and technical path for the resource-based and harmless treatment of NdFeB sludge.
[0006] To achieve the above objectives, the present invention adopts the following technical solution:
[0007] A method for separating the oil phase and solid phase in neodymium iron boron sludge waste includes the following steps:
[0008] S1. The NdFeB sludge waste is centrifuged to remove surface free water, and NdFeB sludge with free water removed is obtained.
[0009] S2. Place the neodymium iron boron sludge obtained in step S1 into the porous extraction tube of the azeotropic distillation apparatus.
[0010] S3. Add the organic solvent to the long-necked round-bottom flask, install and fix the porous extraction tube containing NdFeB sludge to the neck of the long-necked round-bottom flask, install the water separator and condenser, and introduce condensate into the condenser; the organic solvent is at least one of LLR1 or LLR2.
[0011] S4. Heating and refluxing to boil the organic solvent and reflux it to circulate and extract the NdFeB sludge in the porous extraction tube. The oil sludge enters the bottom of the flask along with the solvent extraction to form an organic solvent-oil mixture. The emulsified water and organic solvent vapor azeotropically enter the water separator after condensation. The NdFeB powder is retained in the porous extraction tube.
[0012] S5. After the reflux is complete, stop heating, allow it to cool naturally, remove the porous extraction tube, and dry the obtained NdFeB powder.
[0013] S6. Weigh the dried powder and calculate the oil removal efficiency.
[0014] Furthermore, the centrifugation process in step S1 adopts the physical centrifugation method, with a rotation speed of 1000~10000 r / min and a centrifugation time of 1~100 min.
[0015] Furthermore, LLR1 is a saturated cyclic hydrocarbon solvent containing only carbon and hydrogen elements in its molecule, with a cyclic molecular configuration, no unsaturated bonds or heteroatoms, a boiling point range of 75~85℃, a density less than water, insoluble in water, and capable of forming a heterogeneous azeotrope with water; LLR2 is a polar oxygen-containing organic solvent containing only carbon, hydrogen, and oxygen elements in its molecule, with ester functional groups in its molecule, no halogens or heteroatoms such as nitrogen and sulfur, a boiling point range of 85~95℃, a density slightly greater than water, and capable of forming an azeotrope with water.
[0016] Furthermore, the volume ratio of the organic solvent to the mass of the NdFeB sludge in step S3 is 1:1 to 1:5 (mL:g).
[0017] Furthermore, the volume ratio of the organic solvent to the mass of the NdFeB sludge is 1:3 (mL:g).
[0018] Furthermore, the heating and reflux described in step S4 is performed using an oil bath or heating mantle, and the reflux temperature is the boiling point of the organic solvent used to 30°C above the boiling point.
[0019] Furthermore, when using LLR1, the reflow temperature is 112~117℃; when using LLR2, the reflow temperature is 120℃.
[0020] Furthermore, the reflux time for the cyclic extraction in step S4 is 2-8 hours; the drying process in step S5 is vacuum drying or freeze drying, and the temperature of the vacuum drying is 40-80°C, which is lower than the boiling point of the organic solvent used.
[0021] Furthermore, the water separator mentioned in step S3 is a Dean-Stark water separator; the organic solvent-oil mixture mentioned in step S4 is recycled after the organic solvent is recovered by distillation, and the recovered oil phase is used for cutting oil regeneration or as fuel; the neodymium iron boron sludge waste is water-based coolant sludge or oil-based sludge waste.
[0022] Furthermore, after processing in steps S1 to S6, the deoiling efficiency is not less than 95%, the surface carbon residue in the NdFeB powder is less than 2.0 wt%, and no α-Fe characteristic peaks appear in X-ray diffraction detection.
[0023] The beneficial effects of this invention are:
[0024] 1. High oil removal rate and thorough oil-solid separation. This invention employs azeotropic distillation for the resource-based pretreatment of NdFeB oily sludge waste. Through organic solvent reflux and recycling extraction, the problem of strong adhesion at the oil-solid interface is effectively solved, achieving deep separation of the oil phase and the black solid powder. Experiments show that the oil removal rate can reach up to 97.89% when using LLR1 as the solvent, and up to 99.86% when using LLR2. Both are significantly higher than the oil removal effects of conventional centrifugal washing and extraction methods.
[0025] 2. Green and environmentally friendly. This invention replaces high-temperature oxidation roasting with physical or physicochemical processes, avoiding incomplete combustion caused by improper temperature and atmosphere control during roasting. It does not produce toxic and harmful waste gases rich in tar, soot, and nitrogen oxides, eliminating the pressure of waste gas treatment. At the same time, it avoids the waste of resources caused by the direct combustion of high-oil-content materials, realizing the green and low-carbon recovery of valuable resources in NdFeB sludge.
[0026] 3. The heating temperature is low, which avoids the high energy consumption and stringent requirements on equipment caused by high-temperature roasting, and reduces the pretreatment cost; the rare earth elements in the NdFeB waste do not undergo significant oxidation, the NdFeB solid powder does not undergo changes in phase structure, and there is no loss of rare earth elements.
[0027] 4. The organic solvent used in this invention can be recycled through distillation, which reduces solvent consumption and waste liquid discharge, meets the requirements of green and environmentally friendly processes, and provides new technical support for the recycling of secondary resources.
[0028] 5. Simultaneous removal of emulsified water. The azeotropic distillation principle used in this invention can remove and separate the emulsified water in the oil sludge through azeotropic action while degreasing oil, avoiding the accumulation of water in the solvent that affects the degreasing efficiency, and also eliminating the need for a separate dehydration process. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0030] Figure 1 This is a schematic diagram of the azeotropic distillation apparatus (Dean-Stark apparatus) designed and manufactured in this embodiment of the invention.
[0031] Figure 2 This is a graph showing the effect of extraction temperature on the deoiling rate of NdFeB sludge in Example 1 of the present invention, using LLR1 as the extraction solvent.
[0032] Figure 3 This is a graph showing the effect of extraction time on the deoiling rate of NdFeB sludge when LLR1 is used as the extraction solvent in Example 2 of the present invention.
[0033] Figure 4 This is a graph showing the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge when LLR1 is used as the extraction solvent in Example 3 of the present invention.
[0034] Figure 5 This is a graph showing the effect of temperature on the deoiling rate of NdFeB sludge in Example 4 of the present invention, using LLR2 as the extraction solvent.
[0035] Figure 6 This is a graph showing the effect of extraction time on the deoiling rate of NdFeB sludge in Example 5 of the present invention, using LLR2 as the extraction solvent.
[0036] Figure 7 This is a graph showing the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge when LLR2 is used as the extraction solvent in Example 6 of the present invention.
[0037] Figure 8 XRD diffraction pattern of solid powder after complete separation of oil phase and solid phase using LLR1 and LLR2 as extraction solvents.
[0038] Explanation of reference numerals in the attached drawings: 1—long-necked round-bottom flask; 2—perforated extraction tube; 3—adapter; 4—water separator; 5—condenser tube; 6—heating device. Detailed Implementation
[0039] To make the technical problems to be solved, the technical solutions, and the beneficial effects of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative of the present invention and are not intended to limit the present invention.
[0040] Based on the information contained herein, various changes to the precise description of the invention can be readily made by those skilled in the art without departing from the spirit and scope of the appended claims. It should be understood that the scope of the invention is not limited to the defined processes, properties, or components, as these embodiments and other descriptions are merely illustrative of specific aspects of the invention. In fact, various modifications to embodiments of the invention that will be apparent to those skilled in the art or related fields are covered within the scope of the appended claims.
[0041] To better understand the invention and not to limit its scope, all figures indicating amounts, percentages, and other numerical values used in this application should, in all cases, be understood to be modified by the word "approximately." Therefore, unless specifically stated otherwise, the numerical parameters listed in the specification and appended claims are approximate values and may vary depending on the desired properties being sought. Each numerical parameter should at least be considered as obtained based on reported significant figures and through conventional rounding methods.
[0042] Unless otherwise specified, the starting materials used in the following embodiments are all considered to be obtained from commercial procurement.
[0043] Figure 1 This is a schematic diagram of the self-designed and manufactured azeotropic distillation apparatus (Dean-Stark apparatus) used in the embodiments of the present invention. Figure 1 An azeotropic distillation apparatus designed and manufactured in-house is used to separate the oil, solid, and emulsified water phases in oil sludge.
[0044] The structure of the azeotropic distillation apparatus is as follows:
[0045] The azeotropic distillation apparatus includes a long-necked round-bottom flask 1, a porous extraction tube 2, an adapter 3, a water separator 4, a condenser 5, and a heating device 6. The porous extraction tube 2 is disposed inside the long-necked round-bottom flask 1. The upper part of the porous extraction tube 2 is connected to the water separator 4 via the adapter 3. The upper part of the water separator 4 is connected to the condenser 5. The long-necked round-bottom flask 1 is placed on the heating device 6.
[0046] The long-necked round-bottom flask 1 is used to hold organic solvents and accommodate porous extraction tubes 2. Its neck is connected to a water separator 4 via an adapter 3, forming a channel for solvent vapor to rise and condensate to flow back.
[0047] The porous extraction tube 2 is located inside and at the top of the long-necked round-bottom flask 1, and is used to hold NdFeB sludge. The porous extraction tube 2 has an overflow hole. Organic solvent vapor enters the tube through the wall of the porous extraction tube 2, circulating and extracting the NdFeB sludge. The oil is extracted along with the organic solvent and flows to the bottom of the flask, while the NdFeB powder remains inside the porous extraction tube 2. The overflow hole allows the condensate accumulated in the tube to overflow back into the long-necked round-bottom flask 1, ensuring a stable liquid level inside the extraction tube 2 and preventing the NdFeB powder from being soaked, which would affect the extraction effect.
[0048] The adapter 3 is used to connect the long-necked round-bottom flask 1 to the water separator 4, and to position and fix the porous extraction tube 2 to ensure good sealing of the device.
[0049] The water separator 4 is used to receive the azeotropic vapor condensate after condensation by the condenser tube 5, and to separate the emulsion water from the organic solvent by utilizing the density difference between the oil phase, water phase, and organic solvent, ensuring the purity of the refluxed organic solvent. The water separator 4 is a Dean-Stark water separator.
[0050] The condenser 5 is used to condense the rising organic solvent vapor and azeotropic vapor in the long-necked round-bottom flask 1 into liquid. After the condensate is separated by the water separator 4, the organic solvent is returned to the long-necked round-bottom flask 1 for recycling.
[0051] The heating device 6 is used to heat the long-necked round-bottom flask 1 to make the organic solvent boil and reflux. The heating device 6 is an oil bath or a heating mantle.
[0052] The working process of the azeotropic distillation apparatus is as follows: a porous extraction tube 2 containing NdFeB sludge is placed inside a long-necked round-bottom flask 1. The long-necked round-bottom flask 1 is connected to a water separator 4 via an adapter 3. The upper part of the water separator 4 is connected to a condenser 5. The long-necked round-bottom flask 1 is placed on a heating device 6. The heating device 6 heats the long-necked round-bottom flask 1, causing the organic solvent to boil and reflux. The organic solvent vapor enters the tube through the wall of the porous extraction tube to circulate and extract the NdFeB sludge. The oil sludge enters the bottom of the flask along with the organic solvent extraction to form an organic solvent-oil mixture. The emulsified water and the organic solvent vapor azeotropically enter the water separator 4 after being condensed by the condenser 5. The NdFeB powder is retained in the porous extraction tube, thereby achieving efficient separation of the oil phase, water phase and solid phase.
[0053] A method for separating the oil phase and solid phase in neodymium iron boron sludge waste includes the following steps:
[0054] S1. The NdFeB sludge preserved by water seal is taken out of the storage tank and the NdFeB sludge sample is centrifuged by physical centrifugation to remove the free water on the surface of the sludge and obtain NdFeB sludge with free water removed.
[0055] S2. Weigh out the NdFeB sludge that has been dehydrated and place it in the porous extraction tube of the azeotropic distillation apparatus.
[0056] S3. Add a certain volume of organic solvent to a long-necked round-bottom flask, install and fix the porous extraction tube containing NdFeB sludge in the neck of the long-necked round-bottom flask, install a water separator and a condenser, ensure that the entire device is well sealed, and then introduce condensate into the condenser; the organic solvent is at least one of LLR1 or LLR2.
[0057] S4. Place the long-necked round-bottom flask in an oil bath or heating mantle for heating. When the temperature reaches the set temperature, the organic solvent boils and refluxes, using the organic solvent to circulate and extract the NdFeB sludge waste in the porous extraction tube. The lubricating oil, coolant, surfactants, and other oily reagents in the NdFeB sludge drip into the bottom of the round-bottom flask along with the organic solvent extraction, forming a mixed extract of organic solvent and oil. The surfactant-stabilized emulsion water in the NdFeB sludge azeotropically reacts with the organic solvent vapor, condenses in the condenser, and enters the water separator, while the black NdFeB powder remains in the porous extraction tube. This achieves deep separation of the oil-solid-water three-phase components in the three-phase mixed oil-based NdFeB sludge.
[0058] S5. After reflux, stop heating and keep the condensate flowing until the device cools naturally. Remove the azeotropic distillation apparatus, take out the porous extraction tube containing the black powder and place it in a vacuum drying oven or freeze dryer for drying to obtain NdFeB black powder.
[0059] S6. Weigh the dried powder and calculate the oil removal efficiency.
[0060] The organic solvent used in step S3 is selected from one or more of the following: n-hexane, n-heptane, solvent LLR1, methyl acetate, ethyl acetate, butyl acetate, solvent LLR2, ethanol, acetone, and toluene. This organic solvent has good dissolving power for the mineral oil component in NdFeB, effectively weakening the oil-solid interface adhesion and achieving deep separation of the oil phase, aqueous phase, and black solid powder. The volume ratio of the organic solvent in step S3 to the mass ratio of the solid NdFeB sludge treated in step S1 is 0.1–20 (mL:g).
[0061] LLR1 is a saturated cyclic hydrocarbon solvent containing only carbon and hydrogen elements in its molecule. It has a cyclic molecular configuration and contains no unsaturated bonds or heteroatoms. This solvent has a boiling point range of 75–85°C, a density of less than 1.0 g / cm³, and a solubility in water at 20°C of less than 0.1 g / 100 mL. It can form an azeotrope with water. In this invention, LLR1 is used as a deoiling solvent. Utilizing its non-polar cyclic structure and its ability to dissolve oil phase components, as well as its azeotropic properties with water, efficient removal of oil from oil sludge is achieved through azeotropic distillation.
[0062] LLR2 is a polar oxygen-containing organic solvent used in this invention. Its molecule contains only carbon, hydrogen, and oxygen, has a chain-like molecular structure, and contains ester functional groups, but no halogens or heteroatoms such as nitrogen and sulfur. This solvent is a colorless, transparent liquid at room temperature, is volatile, has a boiling point range of 85–95°C, a density slightly greater than water (approximately 1.07 g / cm³), and a solubility in water at 20°C of less than 15 g / 100 mL. It is miscible with most organic solvents such as ethanol and acetone. LLR2 can form an azeotrope with water, with the azeotropic temperature lower than its own boiling point. In this invention, LLR2 is used as a deoiling solvent, utilizing the dual affinity of its polar ester groups for polar oxygen-containing components and non-polar hydrocarbon oils in oil sludge, as well as its azeotropic properties with water, to achieve efficient removal of oil and solvent recovery from oil sludge through azeotropic distillation.
[0063] The heating temperature in step S4 must meet the following conditions: 10 °C ≤ extraction temperature ≤ 200 °C. The reflux heating time in step S4 is 10 min to 8 h.
[0064] The natural cooling time in step S5 is 1 h to 6 h. The vacuum drying in step S5 uses a temperature of 20 °C to 100 °C and a drying time of 1 min to 48 h. After drying, nitrogen gas is introduced to protect the NdFeB black powder and prevent spontaneous combustion in air. The freeze-drying in step S5 uses a temperature of 0 °C to -40 °C and a drying time of 10 min to 48 h. After drying, nitrogen gas is introduced to protect the NdFeB black powder and prevent spontaneous combustion in air.
[0065] The formula for calculating the oil removal rate is:
[0066] η= ×100%
[0067] Where m0 is the initial mass of the sludge, m1 is the sum of the masses of the high-efficiency extraction tube and the NdFeB sludge, and m2 is the sum of the masses of the high-efficiency extraction tube and the solid powder after degreasing and drying.
[0068] The method further includes: after reflux, collecting the extract in the long-necked round-bottom flask, and separating the organic solvent and mineral oil from the extract by heating and evaporation or vacuum distillation, wherein the organic solvent is recycled.
[0069] This invention relates to a method for the efficient separation of the oil phase and solid phase and the recovery of valuable resources from NdFeB sludge waste. The invention first removes free water from the NdFeB sludge waste through physical centrifugation, then places it in an azeotropic distillation apparatus, employing organic solvent reflux extraction to simultaneously dissolve the oil phase, remove emulsified water via azeotropic distillation, and retain the solid powder. The deoiled NdFeB powder is then vacuum-dried or freeze-dried to obtain high-purity NdFeB black powder.
[0070] The azeotropic distillation degreasing system employed in this invention exhibits excellent degreasing effects on fine-particle, highly adhesive oil-based NdFeB sludge. Under optimal process conditions, using LLR1 and LLR2 as solvents, the degreasing rates reach 97.89% and 99.86%, respectively, both significantly superior to conventional centrifugal washing and leaching methods. Simultaneously, the NdFeB main phase structure remains intact after degreasing, with surface carbon residue as low as 1.83 wt%, providing high-quality raw materials for efficient rare earth leaching and mass transfer in subsequent hydrometallurgical processes.
[0071] Example 1
[0072] This embodiment uses LLR1 as a solvent to investigate the effect of extraction temperature on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0073] S1. Take out the NdFeB sludge preserved by water seal and centrifuge it at 3000 rpm for 10 min to remove the surface free water.
[0074] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0075] S3. Add 150 mL of LLR1 to a long-necked round-bottom flask, install the extraction tube, water separator and condenser, and introduce cooling water.
[0076] S4. The mixture was heated to reflux and extracted at 92°C, 102°C, 107°C, 112°C, 117°C, 122°C, and 132°C for 4 hours, with a solid-liquid ratio of 1:3. Oil was extracted with the solvent and entered the bottom of the flask. Emulsified water and LLR1 vapor were azeotropically mixed and then condensed before entering the water separator. The NdFeB powder remained in the extraction tube.
[0077] S5. After reflux, allow to cool naturally for 2 hours, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0078] S6. Weigh and calculate the deoiling efficiency. The deoiling rates at various temperatures were 90.87%, 97.21%, 98.19%, 97.89%, 102.60%, 101.10%, and 99.97%, respectively. The results show that the deoiling rate reaches a peak of 102.60% at 112°C, and slightly decreases to 99.97% when the temperature is further increased to 132°C. Considering both deoiling efficiency and energy consumption, 112°C was determined to be the optimal extraction temperature for LLR1. In this example, LLR1 was used as the solvent to investigate the effect of extraction temperature on the deoiling rate of NdFeB sludge waste.
[0079] Figure 2 This is a graph showing the effect of extraction temperature on the deoiling rate of NdFeB sludge in Example 1 of this invention, using LLR1 as the extraction solvent. Figure 2 It can be seen that as the extraction temperature increases from 92°C to 112°C, the oil removal rate continues to rise and reaches a peak of 102.60% at 112°C; if the temperature is further increased to 132°C, the oil removal rate drops slightly to 99.97%. Taking into account both oil removal efficiency and energy consumption, 112°C is determined to be the optimal extraction temperature for LLR1.
[0080] Example 2
[0081] This embodiment uses LLR1 as a solvent to investigate the effect of extraction time on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0082] S1. Take out the NdFeB sludge preserved by water seal and centrifuge it at 3000 rpm for 10 min to remove the surface free water.
[0083] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0084] S3. Add 150 mL of LLR1 to a long-necked round-bottom flask, install the extraction tube, water separator and condenser, and introduce cooling water.
[0085] S4. Heat under reflux and circulate at 112°C for 2 h, 3 h, 4 h, 5 h, 6 h and 8 h respectively, with a solid-liquid ratio of 1:3. Oil is extracted with solvent and enters the bottom of the flask. Emulsified water and LLR1 vapor are azeotropically mixed and then condensed into the water separator. NdFeB powder is retained in the extraction tube.
[0086] S5. After reflux, allow the mixture to cool naturally, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0087] S6. Weigh and calculate the oil removal efficiency. The oil removal rates at different times were 81.45%, 92.81%, 97.21%, 101.58%, 93.31%, and 94.05%, respectively. The results show that the oil removal rate continuously increased from 2 h to 5 h, reaching a peak of 101.58% at 5 h. Further extending the extraction time to 6 h and 8 h resulted in a decrease in the oil removal rate. Considering both oil removal efficiency and energy consumption, 4–5 h was determined to be the optimal extraction time for LLR1.
[0088] Figure 3 This is a graph showing the effect of extraction time on the deoiling rate of NdFeB sludge in Example 2 of the present invention, using LLR1 as the extraction solvent. Figure 3 It can be seen that when the extraction time is extended from 2 h to 5 h, the oil removal rate continues to increase and reaches a peak of 101.58% at 5 h. However, when the extraction time is further extended to 6 h and 8 h, the oil removal rate decreases. Taking into account both oil removal efficiency and energy consumption, 4–5 h is determined to be the optimal extraction time for LLR1.
[0089] Example 3
[0090] This embodiment uses LLR1 as a solvent to investigate the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0091] S1. Take out the NdFeB sludge preserved by water seal and centrifuge it at 3000 rpm for 10 min to remove the surface free water.
[0092] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0093] S3. Add LLR1 at solid-liquid ratios of 1:1, 1:2, 1:3, 1:4 and 1:5 (g:mL), respectively, install extraction tubes, water separators and condensers, and introduce condensate;
[0094] S4. Heat to reflux and circulate for 4 hours at 117°C. Oil is extracted with solvent and enters the bottom of the flask. Emulsified water and LLR1 vapor azeotropically and then condense into the water separator. NdFeB powder is retained in the extraction tube.
[0095] S5. After reflux, allow the mixture to cool naturally, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0096] S6. Weigh and calculate the deoiling efficiency. The deoiling rates at various solid-liquid ratios were 67.81%, 85.00%, 97.89%, 91.29%, and 87.68%, respectively. The results show that the deoiling rate continuously increases as the solid-liquid ratio increases from 1:1 (g:mL) to 1:3 (g:mL), reaching a peak of 97.89% at 1:3 (g:mL). Further increases to 1:4 (g:mL) and 1:5 (g:mL) result in a decrease in the deoiling rate. Considering both deoiling efficiency and solvent usage, 1:3 (g:mL) was determined to be the optimal solid-liquid ratio for LLR1.
[0097] Figure 4 This is a graph showing the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge when using LLR1 as the extraction solvent in Example 3 of this invention. Figure 4 It can be seen that as the solid-liquid ratio increases from 1:1 (g:mL) to 1:3 (g:mL), the oil removal rate continuously increases, reaching a peak of 97.89% at 1:3 (g:mL). Further increases to 1:4 (g:mL) and 1:5 (g:mL) result in a decrease in the oil removal rate. Considering both oil removal efficiency and solvent usage, 1:3 (g:mL) is determined to be the optimal solid-liquid ratio for LLR1.
[0098] Example 4
[0099] This embodiment uses LLR2 as a solvent to investigate the effect of extraction temperature on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0100] S1. Take out the NdFeB sludge preserved by water seal and centrifuge to remove the free water on the surface;
[0101] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0102] S3. Add 150 mL of LLR2 to a long-necked round-bottom flask, install the extraction tube, water separator and condenser, and introduce cooling water.
[0103] S4. The mixture was heated to reflux and extracted at 101°C, 110°C, 115°C, 120°C, 125°C, 130°C, and 140°C for 4 h, with a solid-liquid ratio of 1:3 (g:mL). Oil was extracted with the solvent and deposited at the bottom of the flask. Emulsified water and LLR2 vapor were azeotropically mixed and then condensed before entering the water separator. The NdFeB powder remained in the extraction tube.
[0104] S5. After reflux, allow the mixture to cool naturally, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0105] S6. Weigh and calculate the oil removal efficiency. The oil removal rates at various temperatures were 59.17%, 69.97%, 91.92%, 99.86%, 95.36%, 95.26%, and 92.96%, respectively. The results show that the oil removal rate continuously increases as the extraction temperature rises from 101°C to 120°C, reaching a peak of 99.86% at 120°C. Further increasing the temperature to 140°C results in a decrease in the oil removal rate. Considering both oil removal efficiency and energy consumption, 120°C was determined to be the optimal extraction temperature for LLR2.
[0106] Figure 5 This is a graph showing the effect of temperature on the deoiling rate of NdFeB sludge in Example 4 of this invention, using LLR2 as the extraction solvent. Figure 5 It can be seen that as the extraction temperature increases from 101°C to 120°C, the oil removal rate continues to rise and reaches a peak of 99.86% at 120°C. However, if the temperature is further increased to 140°C, the oil removal rate decreases. Considering both oil removal efficiency and energy consumption, 120°C is determined to be the optimal extraction temperature for LLR2.
[0107] Example 5
[0108] This embodiment uses LLR2 as a solvent to investigate the effect of extraction time on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0109] S1. Take out the NdFeB sludge preserved by water seal and centrifuge to remove the free water on the surface;
[0110] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0111] S3. Add 150 mL of LLR2 to a long-necked round-bottom flask, install the extraction tube, water separator and condenser, and introduce cooling water.
[0112] S4. Heat to reflux and circulate at 120°C for 2 h, 3 h, 4 h, 5 h, 6 h and 8 h respectively, with a solid-liquid ratio of 1:3 (g:mL). Oil is extracted with solvent and enters the bottom of the flask. Emulsion water and LLR2 vapor are azeotropically mixed and then condensed into a water separator. NdFeB powder is retained in the extraction tube.
[0113] S5. After reflux, allow the mixture to cool naturally, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0114] S6. Weigh and calculate the oil removal efficiency. The oil removal rates at different times were 84.50%, 85.79%, 99.86%, 99.01%, 98.02%, and 98.29%, respectively. The results show that extending the extraction time from 2 h to 4 h significantly increases the oil removal rate, reaching a peak of 99.86% at 4 h. Further extending the time to 5–8 h slightly decreases the oil removal rate and then tends to stabilize. Considering both oil removal efficiency and energy consumption, 4 h was determined to be the optimal extraction time for LLR2.
[0115] Figure 6 This is a graph showing the effect of extraction time on the deoiling rate of NdFeB sludge in Example 5 of the present invention, using LLR2 as the extraction solvent. Figure 6 It can be seen that extending the extraction time from 2 h to 4 h significantly increases the oil removal rate, reaching a peak of 99.86% at 4 h. Further extending the time to 5–8 h slightly decreases the oil removal rate and then tends to stabilize. Considering both oil removal efficiency and energy consumption, 4 h is determined to be the optimal extraction time for LLR2.
[0116] Example 6
[0117] This embodiment uses LLR2 as a solvent to investigate the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge waste. The method includes the following steps:
[0118] S1. Take out the NdFeB sludge preserved by water seal and centrifuge to remove the free water on the surface;
[0119] S2. Weigh 50.0 g of NdFeB sludge after removing free water and place it in the porous high-efficiency extraction tube of the azeotropic distillation apparatus.
[0120] S3. Add LLR2 at solid-liquid ratios of 1:1, 1:2, 1:3, 1:4 and 1:5 (g:mL), respectively, install extraction tubes, water separators and condensers, and introduce condensate.
[0121] S4. Heat to reflux and circulate for 4 hours at 120°C. Oil and grease are extracted with solvent and enter the bottom of the flask. Emulsified water and LLR2 vapor are azeotropically mixed and then condensed into the water separator. NdFeB powder is retained in the extraction tube.
[0122] S5. After reflux, allow the mixture to cool naturally, remove the extraction tube, and vacuum dry or freeze dry to obtain NdFeB black powder.
[0123] S6. Weigh and calculate the deoiling efficiency. The deoiling rates at various solid-liquid ratios were 72.36%, 85.79%, 99.85%, 85.30%, and 85.33%, respectively. The results show that the deoiling rate continuously increases as the solid-liquid ratio increases from 1:1 (g:mL) to 1:3 (g:mL), reaching a peak of 99.85% at 1:3 (g:mL). Further increases to 1:4 (g:mL) and 1:5 (g:mL) result in a decrease in the deoiling rate, which then tends to stabilize. Considering both deoiling efficiency and solvent usage, 1:3 (g:mL) was determined to be the optimal solid-liquid ratio for LLR2.
[0124] Figure 7 This is a graph showing the effect of the solid-liquid ratio on the deoiling rate of NdFeB sludge when LLR2 was used as the extraction solvent in Example 6 of the present invention. Figure 7 It can be seen that as the solid-liquid ratio increases from 1:1 (g:mL) to 1:3 (g:mL), the oil removal rate continuously increases, reaching a peak of 99.85% at 1:3 (g:mL). Further increases to 1:4 (g:mL) and 1:5 (g:mL) result in a decrease in the oil removal rate, which then tends to stabilize. Considering both oil removal efficiency and solvent usage, 1:3 (g:mL) is determined to be the optimal solid-liquid ratio for LLR2.
[0125] Figure 8 XRD diffraction patterns of solid powders after complete separation of the oil and solid phases, using LLR1 and LLR2 as extraction solvents. Figure 8 It can be seen that when LLR1 and LLR2 are used as extraction solvents, after the oil phase and solid phase are completely separated, no α-Fe characteristic peaks appear in the XRD diffraction pattern of the solid powder, indicating that the main phase structure of NdFeB remains intact after deoiling and no phase structure change occurs.
[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for separating the oil phase and solid phase in neodymium iron boron sludge waste, characterized in that, Includes the following steps: S1. The NdFeB sludge waste is centrifuged to remove surface free water, and NdFeB sludge with free water removed is obtained. S2. Place the neodymium iron boron sludge obtained in step S1 into the porous extraction tube of the azeotropic distillation apparatus. S3. Add the organic solvent to the long-necked round-bottom flask, install and fix the porous extraction tube containing NdFeB sludge in the neck of the long-necked round-bottom flask, install a water separator between the long-necked round-bottom flask and the condenser, so that the water separator is connected to the long-necked round-bottom flask and the condenser respectively, and introduce condensate into the condenser; the organic solvent is at least one of LLR1 or LLR2. S4. Heating and refluxing to boil the organic solvent and reflux it to circulate and extract the NdFeB sludge in the porous extraction tube. The oil sludge enters the bottom of the flask along with the solvent extraction to form an organic solvent-oil mixture. The emulsified water and organic solvent vapor azeotropically enter the water separator after condensation. The NdFeB powder is retained in the porous extraction tube. S5. After the reflux is complete, stop heating, allow it to cool naturally, remove the porous extraction tube, and dry the obtained NdFeB powder. S6. Weigh the dried powder and calculate the oil removal efficiency.
2. The method according to claim 1, characterized in that, The centrifugation process described in step S1 uses physical centrifugation, with a rotation speed of 1000~10000 r / min and a centrifugation time of 1~100 min.
3. The method according to claim 1, characterized in that, The LLR1 is a saturated cyclic hydrocarbon solvent containing only carbon and hydrogen elements in its molecule. It has a cyclic molecular configuration, does not contain unsaturated bonds or heteroatoms, has a boiling point range of 75~85℃, a density less than water, is insoluble in water, and can form a heterogeneous azeotrope with water. The LLR2 is a polar oxygen-containing organic solvent containing only carbon, hydrogen, and oxygen elements in its molecule. It contains ester functional groups, does not contain halogens or heteroatoms such as nitrogen and sulfur, has a boiling point range of 85~95℃, a density slightly greater than water, and can form an azeotrope with water.
4. The method according to claim 1, characterized in that, The ratio of the volume of the organic solvent to the mass of the NdFeB sludge in step S3 is 1:1 to 1:5 (mL:g).
5. The method according to claim 4, characterized in that, The volume ratio of the organic solvent to the mass of the NdFeB sludge is 1:3 (mL:g).
6. The method according to claim 1, characterized in that, The heating and reflux described in step S4 is performed using an oil bath or heating mantle, with the reflux temperature being the boiling point of the organic solvent used to 30°C above the boiling point.
7. The method according to claim 6, characterized in that, When using LLR1, the reflow temperature is 112℃; when using LLR2, the reflow temperature is 120℃.
8. The method according to claim 1, characterized in that, The reflux time for the cyclic extraction in step S4 is 2-8 hours; the drying process in step S5 is vacuum drying or freeze drying, and the temperature of the vacuum drying is 40-80°C, which is lower than the boiling point of the organic solvent used.
9. The method according to claim 1, characterized in that, The water separator mentioned in step S3 is a Dean-Stark water separator; the organic solvent-oil mixture mentioned in step S4 is recycled after the organic solvent is recovered by distillation, and the recovered oil phase is used for cutting oil regeneration or as fuel; the neodymium iron boron sludge waste is water-based coolant sludge or oil-based sludge waste.
10. The method according to claim 1, characterized in that, After processing in steps S1 to S6, the deoiling efficiency is not less than 95%, the surface carbon residue in the NdFeB powder is less than 2.0 wt%, and no α-Fe characteristic peaks appear in X-ray diffraction detection.
Citation Information
Patent Citations
Pretreatment method of oil sludge obtained after neodymium-iron-boron material grinding through machine tool
CN102899479A
Method for pre-processing neodymium iron boron wire cutting waste oil sludge
CN102912112A
A pretreatment method for NdFeB oil sludge waste
CN114317974B
Treatment process for removing impurities in neodymium iron boron oil sludge
CN119296943A