A high-strength, high-plasticity wire rod that is easy to draw and its preparation method

By precisely controlling alloying elements and process parameters, a high-strength and high-plasticity wire rod with a specific microstructure is formed, which solves the segregation and brittleness problems caused by high carbon content, achieves a balance between high strength and high plasticity, and reduces the complexity and cost of the cold drawing process.

CN123063685APending Publication Date: 2026-11-10INST OF RES OF IRON & STEEL JIANGSU PROVINCE +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611592677.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In the current preparation of high-strength steel wire, the high carbon content leads to severe segregation and high brittleness, resulting in complex and costly cold drawing processes, making it difficult to achieve a balance between high strength and high plasticity.

Method used

By finely controlling the composition of the main alloying elements C, Si, Mo, Mn, Cr and V, and controlling the carbon equivalent Ceq between 0.7 and 1.5%, combined with rolling and tempering processes, a microstructure of ferrite + lath martensite + dispersed carbides or lath martensite + plate martensite + dispersed carbides is formed, and the proportion of lath martensite is controlled to be ≥50%.

Benefits of technology

It has achieved a tensile strength of 1720MPa or higher for medium or low carbon wire rods, a shrinkage rate of 45% or higher, and a tensile strength of 2700MPa or higher for cold-drawn steel wires, which significantly improves the plasticity and strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063685A_ABST
    Figure CN123063685A_ABST
Patent Text Reader

Abstract

This application provides a high-strength, high-ductility wire rod that is easy to draw and its preparation method. By finely controlling the composition of the main alloying elements and by limiting the carbon equivalent (Ceq) and effectively controlling the content of impurity elements, the microstructure of the wire rod exhibits a structure that, in addition to dispersed carbides, also contains ferrite and lath martensite, or a combination of lath and plate martensite. The proportion of lath martensite is ≥50%. The medium-carbon system wire rod with this microstructure has a tensile strength of up to 1720 MPa, a reduction of area of ​​45%, and a tensile strength of 2700 MPa after cold drawing, with an elongation at break of 1.7%. The low-carbon system wire rod with this microstructure has a tensile strength of up to 1220 MPa, a reduction of area of ​​56%, and a tensile strength of 1970 MPa after cold drawing, with an elongation at break of 1.9%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metallurgical technology, and in particular to an easy-to-draw high-strength, high-plasticity wire rod and its preparation method. Background Technology

[0002] Currently, commonly used high-strength steel wire is mainly obtained from high-carbon steel wire rod through cold drawing. The microstructure of high-carbon steel wire rod is mainly sorbite, characterized by a fine lamellar structure formed by alternating ferrite and cementite, with lamellar spacing typically in the range of 80-150 nm. This microstructure endows the wire rod with excellent strength-ductility matching, which is the foundation for ensuring subsequent cold drawing performance. During the cold drawing process, the high-carbon steel wire rod undergoes multiple drawing deformations, resulting in coordinated deformation of the internal sorbite structure. The grains are refined along the drawing direction and form a preferred orientation, while the dislocation density increases significantly. Cold drawing work hardening greatly improves the tensile strength of the material. Without heat treatment throughout the process, the tensile strength of the finished steel wire can reach over 2000 MPa.

[0003] To further improve the tensile strength of cold-drawn steel wire, the ideal approach is to increase the strength of the wire rod. Alloying has already increased the tensile strength of wire rod to 1600 MPa, while maintaining a reduction of area of ​​over 30%. Current technologies for alloying to improve the tensile strength of wire rod generally involve adding more carbon and alloying elements. However, the addition of carbon and alloying elements exacerbates material segregation, leading to an increased frequency and severity of abnormal structures such as carbon matrix and martensite, which negatively impact cold drawing. Furthermore, high-carbon wire rod systems are more brittle and cannot be directly cold-drawn, resulting in complex subsequent processing steps and significantly increased processing costs. Summary of the Invention

[0004] This application aims to address the technical problem in existing high-strength wire rod systems where high carbon content easily leads to severe segregation and high brittleness, resulting in complex and costly cold drawing processes. It proposes an easily drawable high-strength, high-plasticity wire rod and its preparation method. This allows the wire rod to achieve the same tensile strength in medium / low carbon systems as in high-carbon systems, while also possessing the excellent plasticity of medium / low carbon systems. This enables the wire rod to be directly cold-drawn to obtain high-strength steel wire in subsequent applications.

[0005] To achieve the above objectives, this application adopts the following technical solution: A high-strength, high-plasticity wire rod that is easy to draw, the chemical composition of which includes, by mass percentage: C 0.20-0.60%, Si 1.0-2.0%, Mo 0.01-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities; Wherein, the carbon equivalent Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo] + [V]) / 5 + ([Ni] + [Cu]) / 15, and Ceq is 0.7~1.5%; where [C] is the mass percentage of C element in the wire rod, [Mn] is the mass percentage of Mn element in the wire rod, [Cr] is the mass percentage of Cr element in the wire rod, [Mo] is the mass percentage of Mo element in the wire rod, [V] is the mass percentage of V element in the wire rod, [Ni] is the mass percentage of Ni element in the wire rod, and [Cu] is the mass percentage of Cu element in the wire rod.

[0006] Furthermore, the chemical composition of the wire rod, by mass percentage, includes: C 0.20-0.30%, Si 1.0-2.0%, Mo 0.2-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities.

[0007] Furthermore, in the wire rod, the largest single brittle inclusion is no larger than 20 μm.

[0008] Furthermore, the microstructure of the wire rod is ferrite + lath martensite + dispersed carbides or lath martensite + plate martensite + dispersed carbides, wherein the proportion of lath martensite is ≥50%, and the ferrite grain size is 0.5-4.0 μm.

[0009] The above-mentioned method for preparing a high-strength, high-plasticity wire rod that is easy to draw includes the following steps: Steelmaking: Steel that meets the above composition requirements is obtained through hot metal desulfurization, converter / electric furnace smelting, and LF refining. Continuous casting: The obtained molten steel is continuously cast into a continuous casting billet with a cross-sectional dimension of (140~300) mm × (140~400) mm; during the continuous casting process, the casting begins with a superheat of ≤20℃; High-speed wire rod rolling: After heating the continuously cast billet, it is sequentially rolled into wire rod through roughing, finishing, and sizing. The soaking temperature during heating is 1080~1100℃, and the air-fuel ratio in the soaking section is <0.60. The initial rolling temperature of the roughing is 1020~1035℃, the entry temperature of the finishing is 830~880℃, and the sizing temperature is 820~850℃. When the carbon content in the wire rod is 0.20-0.50% by mass, the wire drawing temperature is 840~860℃; when the carbon content in the wire rod is 0.50-0.70% by mass, the wire drawing temperature is 860-880℃. Stellmore cooling: The obtained wire rod is placed on the Stellmore cooling line for cooling. Before the temperature of the wire rod drops to 400°C, the cooling rate of the wire rod is controlled to be ≥10°C / s, and the winding temperature is not lower than 300°C. Tempering: After the coiled wire in the Stellmore cooling process is cooled to below 50°C, it is put into an annealing furnace and heated to 300-400°C. It is held at this temperature for 1-2 hours, and then air-cooled to room temperature.

[0010] Furthermore, the desulfurization process of the molten iron involves KR desulfurization of the molten iron until the S content in the molten iron is less than 0.005% by mass percentage to obtain desulfurized molten iron.

[0011] Furthermore, the desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0012] Furthermore, the converter / electric furnace smelting process involves transferring desulfurized molten iron into the converter / electric furnace and adding scrap steel for smelting to obtain molten steel. The tapping temperature is controlled at 1600–1620°C. At the end of smelting, the molten steel composition has a C content of 0.10–0.30% by mass and a P content ≤100ppm. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity.

[0013] Furthermore, the LF refining process involves transferring molten steel into an LF furnace for refining, heating, and alloying to obtain molten steel that meets the above-mentioned composition requirements.

[0014] Furthermore, the binary basicity of the slag produced during the LF refining process is 2.5 to 2.7.

[0015] The above-mentioned application of an easy-to-draw high-strength, high-plasticity wire rod involves using the wire rod to prepare steel wire, and the preparation process is as follows: pickling, drawing, and the total deformation during drawing is greater than or equal to 85%.

[0016] The beneficial effects of this application are: This application achieves a microstructure in medium-carbon or low-carbon wire rod systems by precisely controlling the composition of key alloying elements C, Si, Mo, Mn, Cr, and V, and by limiting the carbon equivalent (Ceq) and effectively controlling the content of impurity elements, combined with restrictions on rolling and tempering processes. This results in a mixed microstructure of ferrite, lath martensite, and dispersed carbides, or a mixed microstructure of lath martensite, plate martensite, and dispersed carbides. The proportion of lath martensite is ≥50%, and the ferrite grain size is 0.5-4.0 μm. The medium-carbon wire rod with this microstructure can achieve a tensile strength of 1720 MPa and a reduction of area of ​​45%. After multiple cold drawing passes, the resulting wire can achieve a tensile strength of 2700 MPa, a total cold drawing deformation of 85%, and an elongation at break of 1.7%. The low-carbon wire rod with this microstructure has a tensile strength of up to 1220 MPa and a reduction of area of ​​56%. After multiple cold drawing processes, the tensile strength of the steel wire can reach 1970 MPa, the total cold drawing deformation reaches 85%, and the elongation after fracture is 1.9%. Attached Figure Description

[0017] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0018] Figure 1 Metallographic photograph of the wire rod provided in Embodiment 1 of this application; Figure 2 Metallographic photograph of the wire rod provided in Embodiment 2 of this application; Figure 3 Metallographic photograph of the wire rod provided in Embodiment 3 of this application; Figure 4 Metallographic photograph of the wire rod provided in Embodiment 4 of this application. Detailed Implementation

[0019] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of the embodiments will be described clearly and completely below. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application. In the description of this application, the experimental methods, unless otherwise specified, are conventional methods; the reagents and materials, unless otherwise specified, are all commercially available.

[0020] The following disclosure provides many different implementations or examples for carrying out this application. To simplify the disclosure of this application, specific examples of components and arrangements are described below. Of course, these are merely examples and are not intended to limit the scope of this application. Those skilled in the art will recognize the application of other processes and / or the use of other materials.

[0021] One embodiment of this application provides an easily drawable, high-strength, and high-plasticity wire rod, the chemical composition of which, by mass percentage, includes: C 0.20-0.60%, Si 1.0-2.0%, Mo 0.01-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities; Wherein, the carbon equivalent Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo] + [V]) / 5 + ([Ni] + [Cu]) / 15, and Ceq is 0.7~1.5%; where [C] is the mass percentage of C element in the wire rod, [Mn] is the mass percentage of Mn element in the wire rod, [Cr] is the mass percentage of Cr element in the wire rod, [Mo] is the mass percentage of Mo element in the wire rod, [V] is the mass percentage of V element in the wire rod, [Ni] is the mass percentage of Ni element in the wire rod, and [Cu] is the mass percentage of Cu element in the wire rod.

[0022] In one or more embodiments, the chemical composition of the wire rod, by mass percentage, may be further defined as follows: C 0.20-0.30%, Si 1.0-2.0%, Mo 0.2-0.3%, Mn 1.0-1.4%, Cr 0.8-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities.

[0023] In one or more embodiments, the maximum single brittle inclusion in the wire rod is no greater than 20 μm.

[0024] In one or more embodiments, the microstructure of the wire rod is ferrite + lath martensite + dispersed carbides or lath martensite + plate martensite + dispersed carbides, wherein the proportion of lath martensite is ≥50% and the ferrite grain size is 0.5-4.0 μm.

[0025] This application, through refined control of the composition of the main alloying elements C, Si, Mo, Mn, Cr, and V in the aforementioned wire rod composition design, and by limiting the carbon equivalent (Ceq) and effectively controlling the content of impurity elements, achieves a microstructure in the medium-carbon or low-carbon wire rod system that is either a mixed microstructure of ferrite + lath martensite + dispersed carbides or a mixed microstructure of lath martensite + plate martensite + dispersed carbides, wherein the proportion of lath martensite is ≥50%, and the ferrite grain size is 0.5-4.0 μm. Medium-carbon / low-carbon wire rods with this microstructure exhibit excellent tensile strength and good cold-drawing performance. The design principles of the chemical composition of the aforementioned easily drawable high-strength, high-ductility wire rods are as follows: Carbon (C) is the most basic strengthening element in steel. When the C content is too low, the carbon atom supersaturation is small, resulting in less lattice distortion and the formation of a dislocation-type substructure, exhibiting a parallel lath-like morphology. The work hardening coefficient of simple low-carbon tempered lath martensite is low, limiting its strength enhancement potential during cold drawing, and its cold working performance is not superior to pearlite. Conversely, when the C content is too high, the high carbon atom supersaturation leads to severe lattice distortion, forming a twinned substructure with a cross-arranged lamellar or acicular morphology. This type of martensite is brittle and prone to brittle fracture during cold deformation, making direct cold drawing impossible. Therefore, in this application, the C content is controlled at 0.20-0.60%, and alloying elements such as Cr and Mo are used to regulate phase transformation, resulting in a final wire rod microstructure with lath or a combination of lath and lamellar characteristics, exhibiting certain plasticity and excellent tensile properties. This allows for direct cold drawing to obtain high-tensile-strength steel wire.

[0026] Si is a ferrite-strengthening element that can improve the strength of ferrite through solid solution strengthening. Si is also an important deoxidizer, helping to reduce the oxygen content in steel and decrease inclusions. Furthermore, Si enrichment at the cementite interface helps prevent spheroidization of cementite during tempering, improving thermal stability during tempering. Too low a Si content leads to a rapid decrease in the strength of tempered martensite, while too high a Si content can cause decarburization. Therefore, in this application, the Si content is controlled between 1.0% and 2.0%.

[0027] The addition of silicon (Si) can easily lead to decarburization of the wire rod, affecting the fatigue performance of the steel wire. Therefore, adding a certain amount of Cr and Mo can reduce decarburization of the wire rod and increase its hardenability. Adding Cr alone has limited improvement in hardenability, while Mo alone is costly. The synergy between the two can significantly reduce the critical cooling rate, enabling a low-cost online cooling method with a cooling rate of ≥10K / s to obtain a high proportion of martensite.

[0028] The work hardening rate of the wire rods in this application is much higher than that of wire rods with conventional ferrite and sorbite structures. Brittle inclusions and residual elements will significantly increase the wire breakage rate. In this application, the requirements for some impurity components are as follows: S≤0.005%, O≤0.005%, H≤0.0001%, and the maximum brittle inclusion is no greater than 20 μm.

[0029] If a single element is adjusted during the production of the wire rod of this application, it may lead to deterioration of welding and toughness. Only by controlling multiple elements simultaneously can it be kept within a reasonable range. Therefore, this application controls multiple main elements simultaneously by limiting the carbon equivalent. In one or more embodiments, the carbon equivalent Ceq is controlled between 0.7 and 1.5.

[0030] This application also provides a method for preparing the above-mentioned easy-to-draw high-strength and high-plasticity wire rod, comprising the following steps: Iron desulfurization The molten iron is subjected to KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron. The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0031] Converter / Electric Furnace Smelting The desulfurized molten iron is transferred to a converter / electric furnace and mixed with scrap steel for smelting to obtain molten steel. The tapping temperature is controlled at 1600-1620℃. At the end of smelting, the molten steel contains 0.10-0.30% C and ≤100ppm P by mass percentage. Deoxidizer is added when the steel is tapped to 1 / 3 of its original volume.

[0032] LF Refining Molten steel is transferred to an LF furnace for refining, heating, and alloying to obtain steel that meets the above-mentioned composition requirements. The binary basicity of the slag formed during the LF refining process is 2.5–2.7.

[0033] Continuous casting The obtained molten steel is continuously cast into a continuous casting billet with a cross-sectional size of (140~300) mm × (140~400) mm; during the continuous casting process, the casting begins with a superheat of ≤20℃.

[0034] High wire rolling After being heated, the continuously cast billet is sequentially rolled into wire rod through roughing, finishing, and sizing. The temperature of the soaking zone during heating is 1080~1100℃, and the air-fuel ratio in the soaking zone is <0.60. The initial rolling temperature of the roughing roll is 1020~1035℃, the inlet temperature of the finishing roll is 830~880℃, and the sizing temperature is 820~850℃. When the carbon content in the wire rod is 0.20-0.50% by mass, the wire drawing temperature is 840~860℃; when the carbon content in the wire rod is 0.50-0.70% by mass, the wire drawing temperature is 860-880℃.

[0035] Stellmore Cooling The obtained wire rod is placed on a Stellmore cooling line for cooling. Before the wire rod temperature drops to 400°C, the cooling rate is controlled to be ≥10°C / s, and the winding temperature is not lower than 300°C. More specifically, before the wire rod temperature drops to 600°C, the cooling rate is controlled to be ≥15°C / s, and before the wire rod temperature drops to 400°C, the cooling rate is controlled to be ≥10°C / s.

[0036] Tempering After the coiled wire is cooled to below 50°C in the Stellmore cooling process, it is put into an annealing furnace and heated to 300-400°C at a heating rate of 200-210°C / h. It is held at this temperature for 1-2 hours, and then air-cooled to room temperature.

[0037] In the aforementioned wire rod manufacturing process, the processes for each step are specifically designed based on the wire rod's carbon equivalent and specific composition. In particular, the process parameters in the high-speed wire rolling, Stellmore cooling, and tempering processes are adjusted to ensure sufficient martensitic transformation, effectively control the martensitic transformation ratio, and significantly improve wire rod performance. The final wire rod has a microstructure of ferrite + lath martensite + dispersed carbides or lath martensite + plate martensite + dispersed carbides, with lath martensite accounting for ≥50% and ferrite grain size of 0.5-4 μm. Simultaneously, the wire rod has a tensile strength of 1120~1900 MPa. When this wire rod is used to manufacture steel wire, it can achieve a cold drawing deformation of greater than 85%. The tensile strength of the medium-carbon steel wire obtained after cold drawing can reach over 2640 MPa, and the tensile strength of the low-carbon steel wire obtained after cold drawing can reach over 1960 MPa.

[0038] The specific implementation methods of this application will be further described in detail below through specific examples.

[0039] Example 1 A type of easily drawable, high-strength, and highly ductile wire rod, the chemical composition of which is as follows (by mass percentage):

[0040] C 0.6%, Si 1.5%, Mo 0.05%, Mn 0.6%, Cr 0.4%, V 0.02%, S 0.003%, O 0.005%, H 0.0001%, with the remainder being Fe and unavoidable impurities.

[0041] This wire rod possesses characteristics such as ultra-high strength, high plasticity, and suitability for cold drawing. Its preparation method includes the following steps: Iron desulfurization The molten iron is subjected to KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron. The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0042] Converter smelting The desulfurized molten iron is transferred to a converter and mixed with scrap steel for oxygen blowing smelting to obtain molten steel. The tapping temperature is controlled at 1600-1620℃. At the end of smelting, the content of C in the molten steel is 0.17% by mass and the content of P is ≤80ppm. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity, and slag is avoided during tapping.

[0043] LF Refining The molten steel is transferred to an LF furnace for refining, heating, and alloying to obtain molten steel that meets the above composition requirements. During the LF refining process, the binary basicity of the slag is 2.6. After the composition and temperature meet the requirements, the slag is gently stirred with argon gas for 23 minutes, and carbonized rice husks are added as a heat preservation agent.

[0044] Continuous casting The obtained molten steel is continuously cast into a continuously cast billet with a cross-sectional dimension of 140mm×140mm; during the continuous casting process, the casting begins at a superheat of 20°C.

[0045] High wire rolling After being heated, the continuously cast billet is sequentially rolled into a wire rod with a diameter of 13 mm through roughing, finishing, and sizing. The temperature of the soaking zone during heating is 1080~1100℃, the air-fuel ratio of the soaking zone is 0.55, the initial rolling temperature of the roughing is 1020~1035℃, the inlet temperature of the finishing is 850~880℃, the sizing temperature is 820~850℃, and the wire rod extrusion temperature is 860-870℃.

[0046] Stellmore Cooling The obtained wire rod was placed on the Stellmore cooling line for cooling. It was first cooled to 600°C at a cooling rate of 12 K / s, and then cooled to 400°C at a cooling rate of 10 K / s before being wound up. The temperature after winding up was 310°C.

[0047] Tempering When the coiled wire is cooled to below 50°C in the Stellmore cooling process, it is put into an annealing furnace and heated to 350°C at a heating rate of 200°C / h. After reaching the temperature, it is held at that temperature for 60 minutes, and then air-cooled to room temperature.

[0048] Example 2

[0049] A type of easily drawable, high-strength, and highly ductile wire rod, the chemical composition of which is as follows (by mass percentage): C 0.20%, Si 1.5%, Mo 0.25%, Mn 1.2%, Cr 1.2%, V 0.09%, S 0.004%, O 0.005%, H 0.0001%, with the remainder being Fe and unavoidable impurities.

[0050] This wire rod possesses characteristics such as ultra-high strength, high plasticity, and suitability for cold drawing. Its preparation method includes the following steps: Iron desulfurization The molten iron is subjected to KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron. The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0051] Converter smelting The desulfurized molten iron is transferred to a converter and mixed with scrap steel for oxygen blowing smelting to obtain molten steel. The tapping temperature is controlled at 1600-1620℃. At the end of smelting, the molten steel contains 0.12% C and 100ppm P by mass percentage. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity, and slag is avoided during tapping.

[0052] LF Refining The molten steel is transferred to an LF furnace for refining, heating, and alloying to obtain steel that meets the above composition requirements. During the LF refining process, the binary basicity of the slag is 2.5. After the composition and temperature meet the requirements, the slag is gently stirred with argon for 20 minutes, and carbonized rice husks are added as a heat-insulating agent.

[0053] Continuous casting The obtained molten steel is continuously cast into a continuously cast billet with a cross-sectional dimension of 140mm×140mm; during the continuous casting process, the casting begins at a superheat of 25°C.

[0054] High wire rolling After being heated, the continuously cast billet is sequentially rolled into a wire rod with a diameter of 6.5 mm through roughing, finishing, and sizing. The temperature of the soaking zone during heating is 1080~1100℃, the air-fuel ratio of the soaking zone is 0.55, the initial rolling temperature of the roughing is 1020~1035℃, the inlet temperature of the finishing is 830~880℃, the sizing temperature is 820~850℃, and the wire drawing temperature is 840~850℃ when the carbon mass percentage content in the wire rod is 0.20-0.50%.

[0055] Stellmore Cooling The obtained wire rod was placed on the Stellmore cooling line for cooling. It was first cooled to 600°C at a cooling rate of 20 K / s, and then cooled to 400°C at a cooling rate of 15 K / s before being wound up. The temperature after winding up was 310°C.

[0056] Tempering When the coiled wire is cooled to below 50°C in the Stellmore cooling process, it is put into an annealing furnace and heated to 350°C at a heating rate of 210°C / h. It is held at this temperature for 105 minutes and then air-cooled to room temperature.

[0057] Example 3

[0058] A type of easily drawable, high-strength, and highly ductile wire rod, the chemical composition of which is as follows (by mass percentage): C 0.40%, Si 1.3%, Mo 0.12%, Mn 1.0%, Cr 0.5%, V 0.06%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities.

[0059] This wire rod possesses characteristics such as ultra-high strength, high plasticity, and suitability for cold drawing. Its preparation method includes the following steps: Iron desulfurization The molten iron is subjected to KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron. The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0060] Converter smelting The desulfurized molten iron is transferred to a converter and mixed with scrap steel for oxygen blowing smelting to obtain molten steel. The tapping temperature is controlled at 1600-1620℃. At the end of smelting, the molten steel contains 0.15% C and 98ppm P by mass percentage. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity, and slag is avoided during tapping.

[0061] LF Refining The molten steel is transferred to an LF furnace for refining, heating, and alloying to obtain molten steel that meets the above composition requirements. During the LF refining process, the binary basicity of the slag is 2.5. After the composition and temperature are in place, the slag is gently stirred with argon gas for 20 minutes, and carbonized rice husks are added as a heat-insulating agent.

[0062] Continuous casting The obtained molten steel is continuously cast into a continuously cast billet with a cross-sectional dimension of 140mm×140mm; during the continuous casting process, the casting begins at a superheat of 25°C.

[0063] High wire rolling After being heated, the continuously cast billet is sequentially rolled into a wire rod with a diameter of 6.5 mm through roughing, finishing, and sizing. The temperature of the soaking zone during heating is 1080~1100℃, the air-fuel ratio of the soaking zone is 0.55, the initial rolling temperature of the roughing is 1020~1035℃, the inlet temperature of the finishing is 830~880℃, the temperature of the sizing is 820~850℃, and the wire drawing temperature is 840-850℃.

[0064] Stellmore Cooling The obtained wire rod was placed on the Stellmore cooling line for cooling. It was first cooled to 600°C at a cooling rate of 20 K / s, and then cooled to 400°C at a cooling rate of 15 K / s before being wound up. The temperature after winding up was 310°C.

[0065] Tempering When the coiled wire is cooled to below 50°C in the Stellmore cooling process, it is put into an annealing furnace and heated to 350°C at a heating rate of 200°C / h. It is held at this temperature for 105 minutes and then air-cooled to room temperature.

[0066] Example 4

[0067] A type of easily drawable, high-strength, and highly ductile wire rod, the chemical composition of which is as follows (by mass percentage): C 0.5%, Si 1.8%, Mo 0.20%, Mn 0.45%, Cr 0.55%, V 0.09%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities.

[0068] This wire rod possesses characteristics such as ultra-high strength, high plasticity, and suitability for cold drawing. Its preparation method includes the following steps: Iron desulfurization The molten iron is subjected to KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron. The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

[0069] Converter smelting The desulfurized molten iron is transferred to a converter and mixed with scrap steel for oxygen blowing smelting to obtain molten steel. The tapping temperature is controlled at 1600-1620℃. At the end of smelting, the molten steel contains 0.13% C and 89ppm P by mass percentage. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity, and slag is avoided during tapping.

[0070] LF Refining The molten steel is transferred to an LF furnace for refining, heated, and alloyed to obtain steel that meets the above composition requirements. During the LF refining process, the binary basicity of the slag is 1.6. After the temperature and composition are in place, the slag is gently stirred with argon for 20 minutes, and carbonized rice husks are added as a heat-insulating agent.

[0071] Continuous casting The obtained molten steel is continuously cast into a continuously cast billet with a cross-sectional dimension of 140mm×140mm; during the continuous casting process, the casting begins at a superheat of 25°C.

[0072] High wire rolling After being heated, the continuously cast billet is sequentially rolled into a wire rod with a diameter of 6.5 mm through roughing, finishing, and sizing. The temperature of the soaking zone during heating is 1080~1100℃, the air-fuel ratio of the soaking zone is 0.58, the initial rolling temperature of the roughing is 1020~1035℃, the inlet temperature of the finishing is 830~880℃, the temperature of the sizing is 820~850℃, and the wire drawing temperature is 850-860℃.

[0073] Stellmore Cooling The obtained wire rod was placed on the Stellmore cooling line for cooling. It was first cooled to 600°C at a cooling rate of 20 K / s, and then cooled to 400°C at a cooling rate of 15 K / s before being wound up. The temperature after winding up was 310°C.

[0074] Tempering When the coiled wire is cooled to below 50°C in the Stellmore cooling process, it is put into an annealing furnace and heated to 350°C at a heating rate of 200°C / h. It is held at this temperature for 110 minutes and then air-cooled to room temperature.

[0075] Application and performance testing The wire rods obtained in the above embodiments were tested for tensile strength, reduction of area, and elongation. Simultaneously, the wire rods obtained in the above embodiments were used to prepare steel wires, and the tensile strength and elongation after fracture of the obtained steel wires were tested. The test results are shown in Table 1 below. The process steps for preparing the steel wires included: pickling the wire rods with 40% hydrochloric acid to remove the oxide scale from the wire rod surface; drawing using a continuous wire drawing machine; and total deformation amounts of 85%, 86%, 90%, and 88%, respectively.

[0076] Table 1. Test results of various properties of wire rods and prepared steel wires in each embodiment.

[0077] As can be clearly seen from Table 1 above, the tensile strength of low-carbon steel wire rod with a carbon content of 0.2% after cold drawing deformation of 86% can reach 1970 MPa, and its work hardening rate exceeds that of ordinary high-carbon steel. The tensile strength of medium-carbon steel wire rod with a carbon content of 0.60% after cold drawing deformation of 85% can reach 2700 MPa.

[0078] Furthermore, the metallographic structure of the wire rod obtained in the embodiments of this application was subjected to SEM examination, and the results are shown in the attached figures. Figures 1 to 4 As shown, the microstructure of low-carbon wire rod consists of ferrite + lath martensite + dispersed carbides, with lath martensite accounting for ≥50% and ferrite grain size of 0.5-4μm; the microstructure of medium-carbon steel wire rod consists of lath martensite + plate martensite + dispersed carbides, with lath martensite accounting for ≥50%.

[0079] In the above embodiments, the descriptions of each embodiment have different focuses. For parts not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.

[0080] The foregoing has provided a detailed description of an easy-to-draw high-strength, high-plasticity wire rod and its preparation method, as provided in the embodiments of this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the technical solutions and core ideas of this application. Those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.

Claims

1. A high-strength, high-plasticity wire rod that is easy to draw, characterized in that, Its chemical composition, by mass percentage, includes: C 0.20-0.60%, Si 1.0-2.0%, Mo 0.01-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities; Wherein, the carbon equivalent Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo] + [V]) / 5 + ([Ni] + [Cu]) / 15, and Ceq is 0.7~1.5%; where [C] is the mass percentage of C element in the wire rod, [Mn] is the mass percentage of Mn element in the wire rod, [Cr] is the mass percentage of Cr element in the wire rod, [Mo] is the mass percentage of Mo element in the wire rod, [V] is the mass percentage of V element in the wire rod, [Ni] is the mass percentage of Ni element in the wire rod, and [Cu] is the mass percentage of Cu element in the wire rod.

2. The easily drawable, high-strength, high-plasticity wire rod as described in claim 1, characterized in that: The chemical composition of the wire rod, by mass percentage, includes: C 0.20-0.30%, Si 1.0-2.0%, Mo 0.2-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities.

3. The easily drawable, high-strength, high-plasticity wire rod as described in claim 1, characterized in that: In the wire rod, the largest single brittle inclusion is no larger than 20 μm.

4. The easily drawable, high-strength, high-plasticity wire rod as described in claim 1, characterized in that: The microstructure of the wire rod is ferrite + lath martensite + dispersed carbides or lath martensite + plate martensite + dispersed carbides, wherein the proportion of lath martensite is ≥50% and the ferrite grain size is 0.5-4.0 μm.

5. A method for preparing an easily drawable, high-strength, high-plasticity wire rod, characterized in that, Includes the following steps: Steelmaking: Through hot metal desulfurization, converter / electric furnace smelting, and LF refining, steel is obtained that meets the following mass percentage composition requirements: C 0.20-0.60%, Si 1.0-2.0%, Mo 0.01-0.3%, Mn 0.4-1.4%, Cr 0.4-1.2%, V 0-0.10%, S≤0.005%, O≤0.005%, H≤0.0001%, with the remainder being Fe and unavoidable impurities; Wherein, the carbon equivalent Ceq = [C] + [Mn] / 6 + ([Cr] + [Mo] + [V]) / 5 + ([Ni] + [Cu]) / 15, and Ceq is 0.7~1.5%; where [C] is the mass percentage of C element in the wire rod, [Mn] is the mass percentage of Mn element in the wire rod, [Cr] is the mass percentage of Cr element in the wire rod, [Mo] is the mass percentage of Mo element in the wire rod, [V] is the mass percentage of V element in the wire rod, [Ni] is the mass percentage of Ni element in the wire rod, and [Cu] is the mass percentage of Cu element in the wire rod; Continuous casting: The obtained molten steel is continuously cast into a continuous casting billet with a cross-sectional dimension of (140~300) mm × (140~400) mm; during the continuous casting process, the casting begins with a superheat of ≤20℃; High-speed wire rod rolling: After heating the continuously cast billet, it is sequentially rolled into wire rod through roughing, finishing, and sizing. The soaking temperature during heating is 1080~1100℃, and the air-fuel ratio in the soaking section is <0.

60. The initial rolling temperature of the roughing is 1020~1035℃, the entry temperature of the finishing is 830~880℃, and the sizing temperature is 820~850℃. When the carbon content in the wire rod is 0.20-0.50% by mass, the wire drawing temperature is 840~860℃; when the carbon content in the wire rod is 0.50-0.60% by mass, the wire drawing temperature is 860-880℃. Stellmore cooling: The obtained wire rod is placed on the Stellmore cooling line for cooling. Before the temperature of the wire rod drops to 400°C, the cooling rate of the wire rod is controlled to be ≥10°C / s, and the winding temperature is not lower than 300°C. Tempering: After the coiled wire in the Stellmore cooling process is cooled to below 50°C, it is heated in an annealing furnace to 300-400°C, held for 1-2 hours, and then air-cooled to room temperature.

6. The method for preparing easily drawable high-strength, high-plasticity wire rod as described in claim 5, characterized in that: The process of desulfurizing molten iron involves KR desulfurization until the sulfur content in the molten iron is less than 0.005% by mass to obtain desulfurized molten iron.

7. The method for preparing easily drawable high-strength, high-plasticity wire rod as described in claim 5, characterized in that: The desulfurizing agent used in the molten iron desulfurization process is calcium oxide.

8. The method for preparing easily drawable high-strength, high-plasticity wire rod as described in claim 5, characterized in that: The converter / electric furnace smelting process involves transferring desulfurized molten iron into the converter / electric furnace and adding scrap steel for smelting to obtain molten steel. The tapping temperature is controlled at 1600–1620°C. At the end of smelting, the molten steel composition has a carbon content of 0.10–0.30% and a phosphorus content of ≤100 ppm by mass percentage. Deoxidizer is added when the steel is tapped to 1 / 3 of its capacity.

9. The method for preparing easily drawable high-strength, high-plasticity wire rod as described in claim 5, characterized in that: The LF refining process involves transferring molten steel into an LF furnace for refining, heating, and alloying to obtain molten steel that meets the above-mentioned composition requirements.

10. An application of an easily drawable, high-strength, high-plasticity wire rod, characterized in that: The high-strength, high-plasticity wire rod of any one of claims 1-4 or the wire rod obtained by any one of the preparation methods of claims 5-9 is used to prepare steel wire, wherein the process of preparing steel wire is as follows: pickling and drawing; wherein the total deformation of drawing is greater than or equal to 85%.