Al-Mg-Si-Sn-Bi Free-Machining Aluminum Alloy and Its Preparation Method
By employing a short-time preheating direct hot extrusion process and online cooling treatment, the problems of Sn/Bi enriched phase coarsening and Mg consumption in the long-term high-temperature homogenization treatment of Al-Mg-Si-Sn-Bi free-cutting aluminum alloys have been solved. This enables the efficient preparation of aluminum alloy extrusions with both good mechanical properties and free-cutting properties, which are suitable for the industrial production of aluminum alloy bars and machined parts of various specifications.
Patent Information
- Application Number
- CN202611291470.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-25
- Publication Date
- 2026-11-10
AI Technical Summary
In the existing production process of 6xxx series aluminum alloys, free-machining aluminum alloys containing Sn and Bi suffer from problems such as Sn/Bi enriched phase coarsening, aggregation, and Mg element consumption during long-term high-temperature homogenization treatment, which affect the uniformity of microstructure and machinability.
A short-time preheating direct hot extrusion process is adopted, eliminating the traditional long-time homogenization treatment. The second phase is broken and dispersed through large plastic deformation of hot extrusion, combined with online cooling and aging treatment, to prepare free-cutting aluminum alloy extrusions.
It significantly shortens the production cycle, reduces energy consumption, improves the uniformity of microstructure, maintains good mechanical properties and machinability, and is suitable for the industrial production of aluminum alloy bars and machined parts of various specifications.
Smart Images

Figure CN123063697A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of aluminum alloy processing technology, specifically relating to Al-Mg-Si-Sn-Bi free-cutting aluminum alloy and its preparation method. Background Technology
[0002] 6xxx series aluminum alloys (also known as Al-Mg-Si series aluminum alloys) are widely used in construction, transportation, electronics, and machinery manufacturing due to their moderate strength, good formability, corrosion resistance, and weldability. To meet the demands of high-speed machining on automatic lathes, low-melting-point elements such as Sn and Bi are often added to Al-Mg-Si aluminum alloys to prepare lead-free free-machining aluminum alloys. Sn and Bi have extremely low solid solubility in the aluminum matrix, existing mainly in free state or as intermetallic compounds. During cutting, they act as lubricants and promote chip breakage, thereby improving the alloy's machinability.
[0003] The typical production process for 6xxx series aluminum alloys includes: melting and casting → ingot homogenization treatment → hot extrusion → online cooling → aging treatment. Among these, ingot homogenization treatment is a key process, generally involving holding at 480℃~580℃ for 4 to 24 hours. Its purpose is to eliminate as-cast segregation, promote the dissolution of the Mg2Si phase, and improve the morphology of harmful phases such as Fe-containing phases, thereby optimizing the alloy's extrusion performance and the mechanical properties of the finished product.
[0004] However, conventional long-term high-temperature homogenization treatment has significant compatibility issues for Al-Mg-Si free-machining aluminum alloys containing Sn and Bi. Sn and Bi have low solid solubility in the aluminum matrix, easily forming Sn / Bi enriched phases or Sn / Bi-containing second phases. During prolonged high-temperature exposure, these enriched or second phases may coarsen, aggregate, or segregate, thus affecting microstructure uniformity, machinability, and subsequent age-hardening effects. Simultaneously, Sn and Bi readily react with Mg in the alloy to form Mg-Sn and Mg-Bi related phases. Prolonged high-temperature environments accelerate this reaction process, potentially consuming some of the effective Mg element used to form the Mg2Si strengthening phase, and possibly weakening the subsequent precipitation strengthening effect of the alloy.
[0005] Existing processes for 6xxx series lead-free free-machining aluminum alloys typically follow the conventional long-term homogenization approach. However, this approach is mainly designed for the dissolution of Mg2Si, elimination of segregation, and morphological control of Fe-containing phases in ordinary Al-Mg-Si alloys, without fully considering the microstructural evolution characteristics of Sn and Bi free-machining elements during long-term high-temperature holding and their potential impact on alloy properties. The applicant's preliminary experiments revealed that the tensile properties of the Al-Mg-Si-Sn-Bi alloy in the solution-quenched state showed little difference after holding at different high temperatures for varying times, indicating that the performance enhancement of this alloy is limited by long-term high-temperature homogenization or solution treatment. Therefore, developing a short-process preparation method adapted to the characteristics of this type of alloy and avoiding the drawbacks of long-term homogenization has significant engineering application value. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a free-machining aluminum alloy of Al-Mg-Si-Sn-Bi. This invention addresses the problem that the Sn / Bi enriched phase and the Mg-containing second phase in Sn-Mg-Si free-machining aluminum alloys may coarsen, aggregate, and consume effective Mg during long-term high-temperature homogenization. By eliminating the traditional long-term homogenization-cooling-reheating extrusion route, this invention employs a short-time preheating direct hot extrusion process. This avoids the risks of coarsening, aggregation, and segregation of the Sn / Bi enriched phase and the Sn / Bi-containing second phase during long-term high-temperature residence, reduces the possibility of ineffective consumption of Mg by the Sn / Bi-related phases, and utilizes the large plastic deformation of hot extrusion to achieve the breakage and dispersion of the second phase. Combined with online cooling and subsequent aging processes, this yields aluminum alloy extrusions with both good mechanical properties and free-machining performance.
[0007] To achieve this objective, the present invention adopts the following technical solution: Al-Mg-Si-Sn-Bi free-cutting aluminum alloy, in the preparation process of which aluminum alloy ingots without homogenization treatment are directly subjected to heating and extrusion treatment, and after cooling, aging treatment is completed to obtain the alloy.
[0008] The hot extrusion process involves preheating the unhomogenized aluminum alloy ingot in a furnace at 430°C–540°C for 10–120 minutes, and then transferring it to an extruder for hot extrusion. Preferably, the preheating temperature range is 480°C–520°C, and the holding time is 20–60 minutes.
[0009] The aluminum alloy has the following chemical composition by mass percentage: Mg: 0.50%–1.20%, Si: 0.40%–1.20%, Sn: 0.20%–1.20%, Bi: 0.10%–0.80%, with the balance being Al and unavoidable impurities.
[0010] Preferably, the alloy composition by mass percentage is: Mg: 0.65%–0.95%, Si: 0.55%–0.90%, Sn: 0.50%–0.95%, Bi: 0.30%–0.60%, with the balance being Al and unavoidable impurities.
[0011] The unavoidable impurities include one or more of Fe, Cu, Mn, Cr, Zn, and Ti, wherein the content of a single impurity element does not exceed 0.50%, and the total content of impurity elements does not exceed 1.00%.
[0012] In the hot extrusion process, the extrusion ratio is 5 to 80, the extrusion barrel temperature is 350°C to 500°C, the die temperature is 350°C to 520°C, and the extrusion outlet temperature is controlled at 480°C to 560°C.
[0013] Another object of the present invention is to provide a method for preparing Al-Mg-Si-Sn-Bi free-machining aluminum alloys.
[0014] To achieve this objective, the present invention employs the following technical solution: a method for preparing Al-Mg-Si-Sn-Bi free-cutting aluminum alloy, comprising the following steps: (1) Prepare alloy raw materials according to mass percentage, wherein Mg: 0.50%~1.20%, Si: 0.40%~1.20%, Sn: 0.20%~1.20%, Bi: 0.10%~0.80%, and the balance is Al and unavoidable impurities; (2) The prepared alloy raw materials are smelted in a smelting furnace. After the raw materials are completely melted, a refining agent is added for refining and degassing. After standing and removing slag, the ingot is cast by semi-continuous casting or iron mold casting. (3) Cut the ingot at the head and tail, turn it or grind the surface to remove the surface oxide scale, segregation nodules and casting defects to obtain the billet to be extruded; (4) Place the billet to be extruded directly into the heating furnace for preheating for 10 min to 120 min; (5) Transfer the preheated billet to the extruder for hot extrusion to obtain the extruded material; (6) The extruded material is cooled online immediately after being demolded; (7) Aging treatment is performed on the cooled extruded material.
[0015] Preferably, in step (1), the mass percentage of the alloy components is: Mg: 0.65% to 0.95%, Si: 0.55% to 0.90%, Sn: 0.50% to 0.95%, Bi: 0.30% to 0.60%, with the balance being Al and unavoidable impurities.
[0016] The unavoidable impurities include one or more of Fe, Cu, Mn, Cr, Zn, and Ti, wherein the content of a single impurity element does not exceed 0.50%, and the total content of impurity elements does not exceed 1.00%.
[0017] In step (3), considering the alloy's hot deformation capability, extrusion temperature requirements, and the need to avoid prolonged high-temperature exposure, the preheating temperature is controlled between 430℃ and 540℃, and the holding time is controlled between 10 min and 120 min. Preferably, the extrusion preheating temperature range is 480℃ to 520℃, and the holding time is 20 min to 60 min.
[0018] In step (5) of hot extrusion, the extrusion ratio is 5–80, the extrusion barrel temperature is 350℃–500℃, the die temperature is 350℃–520℃, and the extrusion outlet temperature is controlled at 480℃–560℃. The extruded material obtained is extruded bar, wire, or profile. Under the action of large plastic deformation in hot extrusion, the blocky, aggregated Sn / Bi enriched phase, Mg-Sn phase, Mg-Bi phase, and other second phases initially present in the as-cast structure can be mechanically broken, elongated, and uniformly dispersed along the extrusion flow direction, effectively improving the compositional segregation and second-phase agglomeration problems of the as-cast structure.
[0019] In step (6), the cooling method can be air cooling, wind cooling, spray cooling, water cooling, or any combination thereof. Preferably, online cooling begins within 30 seconds after the extruded material exits the mold, in order to preserve the supersaturated solid solution state of Mg and Si elements in the aluminum matrix as much as possible, laying the foundation for subsequent aging precipitation strengthening.
[0020] In step (7), the aging treatment can be natural aging, artificial aging, or a combination of natural and artificial aging. The natural aging time is 1 day to 60 days; the artificial aging temperature is 150℃ to 200℃, and the heat preservation time is 2 hours to 12 hours.
[0021] Beneficial effects This invention does not simply omit the conventional homogenization process. Instead, it innovatively proposes an integrated short-process preparation route of "short-time preheating - direct hot extrusion - online cooling - natural aging or artificial aging" targeting the formation and evolution of the special Sn / Bi low-melting-point free-machining phase and Mg-Sn and Mg-Bi related phases in Al-Mg-Si-Sn-Bi alloys. This is a targeted optimization and reverse improvement of the traditional 6xxx series free-machining aluminum alloy hot extrusion process.
[0022] I. Optimize production processes to significantly improve industrial efficiency Shortened cycle time and energy saving: This invention directly places the billet to be extruded into the heating furnace for short-term preheating, eliminating the need for long-term homogenization, i.e., it does not undergo conventional long-term homogenization treatment. Specifically, this invention abandons the independent long-term homogenization process of holding at 480℃~580℃ for more than 4 hours in the traditional process, as well as the cumbersome route of "homogenization-cooling-reheating". By adopting an integrated short process of "short-term preheating-direct hot extrusion", the billet reaches the uniform temperature required for hot extrusion only through short-term preheating, without long-term homogenization diffusion treatment, which effectively shortens the overall production cycle and significantly reduces energy consumption during the high-temperature holding process.
[0023] Improved equipment utilization: The elimination of long-term homogenization processes reduces the long-term occupancy time of equipment such as heating furnaces, simplifies production processes, and is more suitable for the needs of large-scale industrial production.
[0024] II. Precisely control microstructure to avoid metallurgical defects Suppressing Coarsening and Segregation of Free-Machining Phases: Addressing the potential coarsening, aggregation, and consumption of effective Mg by the Sn / Bi enriched phase and Mg-containing second phase in Sn-Mg-Si free-machining aluminum alloys during long-term high-temperature homogenization, this study eliminates the traditional long-term homogenization-cooling-reheating extrusion route and adopts a short-time preheating direct hot extrusion process. This avoids the risks of coarsening, aggregation, and segregation of the Sn / Bi enriched phase and Sn / Bi-containing second phase during prolonged high-temperature residence, reducing the possibility of ineffective Mg consumption by Sn / Bi-related phases. Furthermore, the large plastic deformation of hot extrusion achieves the fragmentation and dispersion of the second phase. Combined with online cooling and subsequent aging processes, this maintains the fine and dispersed distribution of the free-machining phase, providing a microstructure basis for stable alloy machinability and resulting in aluminum alloy extrusions with both good mechanical properties and free-machining performance.
[0025] Active microstructure control is achieved by utilizing plastic deformation to actively break down the microstructure: This changes the traditional approach of relying on high-temperature diffusion homogenization to optimize the microstructure. Instead, it utilizes the large plastic deformation mechanical action during hot extrusion to actively break down and elongate the agglomerated second phase in the as-cast state, dispersing it along the extrusion direction, thereby improving the unevenness defects of the as-cast microstructure.
[0026] III. Synergistically improve mechanical properties and cutting performance Preservation of precipitation strengthening potential: By significantly shortening the high-temperature residence time of the billet, the probability of side reactions between Mg and Sn and Bi elements is reduced, thus minimizing the ineffective consumption of effective Mg elements. This preserves sufficient Mg and Si solute atoms, ensuring the precipitation ability of the Mg2Si strengthening phase during subsequent aging processes, thereby ensuring the strength of the alloy.
[0027] Achieving comprehensive performance matching: Through the synergistic process of "short-time preheating + direct extrusion + rapid online cooling + aging treatment", the online cooling retains the supersaturated solid solution of Mg and Si, and the subsequent aging precisely controls the precipitation of strengthening phases. The final aluminum alloy extrusion material has both stable machinability and good mechanical properties thanks to the fine and dispersed Sn / Bi phase.
[0028] IV. The process is highly versatile and has broad application prospects. The process of this invention has good versatility and can be adapted to the preparation of various specifications of Al-Mg-Si-Sn-Bi free-cutting aluminum alloy bars, wires and profiles. It is widely applicable to the industrial production of products such as bars, fastener blanks and machined parts blanks processed by automatic lathes. Attached Figure Description
[0029] Figure 1 This is an electron microscope image of the as-cast heterogeneous material.
[0030] Figure 2 This is an electron microscope image of the extruded heterogeneous material in Example 2.
[0031] Figure 3 This is an electron microscope image obtained after a traditional long-term homogenization and coarsening process.
[0032] Figure 4 This is an electron microscope image of a product with an excessively long high-temperature preheating time. Detailed Implementation
[0033] The present invention will be further described in detail below with reference to specific embodiments.
[0034] This invention addresses the problem that Sn / Bi enriched phases and Mg-containing second phases in free-machining Al-Mg-Si aluminum alloys containing Sn and Bi may coarsen, aggregate, and consume available Mg during long-term high-temperature homogenization. It adopts a direct hot extrusion process with short-time preheating that eliminates the need for conventional long-term homogenization. The large plastic deformation of hot extrusion is used to break, elongate, and disperse the second phase, combined with online cooling and aging treatment, to obtain aluminum alloy extrusions with both good mechanical properties and free-machining properties.
[0035] The basic principle is as follows: For Al-Mg-Si alloys containing Sn and Bi, traditional long-term high-temperature homogenization processes offer limited performance gains and pose potential risks of inducing second-phase coarsening and consuming effective solute elements. This invention achieves billet homogenization through short-time preheating, avoiding the problem of high-temperature long-term microstructure deterioration. Simultaneously, it utilizes hot extrusion plastic deformation to refine and disperse the second phase. Combined with cooling and aging process control, it obtains qualified extruded materials that meet application requirements.
[0036] SEM-EDS Tissue Characterization Validation Instructions The distribution characteristics of the second phase in this invention can be verified through microstructure testing using SEM-EDS. Scanning electron microscopy allows for direct observation of the morphology, size, and distribution of the Sn / Bi enriched phase, Mg-Sn phase, and Mg-Bi phase in the extruded material's microstructure; combined with energy dispersive spectroscopy (EDS), the elemental composition and enrichment regions of the second phase can be accurately identified. Compared to the coarse, locally agglomerated, and unevenly sized second phase that is prone to occur in traditional long-term homogenization processes (…),… Figure 3-4 This invention avoids the coarsening of the second phase caused by long-term diffusion at high temperatures through short-term preheating, while utilizing the mechanical crushing effect of strong plastic deformation from hot extrusion to break down the untreated cast rod ( Figure 1 Compared with traditional long-term homogenization processes, this method can refine the size of various Sn, Bi, and Mg-containing second phases into a blocky distribution, with a diffuse and uniform distribution along the extrusion direction, without obvious large-sized agglomerates of second phases. This effectively optimizes the uniformity of the alloy's microstructure and matches the microstructure and performance requirements of free-machining aluminum alloys. Figure 2 ).
[0037] When implementing this invention, attention should be paid to controlling the following key process parameters: 1. Alloy composition control: Mg and Si are the main strengthening elements, while Sn and Bi are the core free-machining elements. By limiting the precise composition range, the mechanical properties and machinability of the alloy are balanced, and performance defects caused by abnormal element content are avoided.
[0038] 2. Short-time preheating process: Preheating temperature and holding time are the core process parameters. If the temperature and time are too low, the billet will have insufficient plasticity and be difficult to extrude. If the temperature and time are too high, it will be close to the traditional homogenization process and lose the advantages of the short process and microstructure control of this invention.
[0039] 3. Hot extrusion process: The extrusion ratio and extrusion temperature directly affect the crushing effect of the second phase and the alloy forming quality. Appropriate extrusion parameters can ensure that the second phase is fully dispersed, while avoiding extrusion cracks and surface defects.
[0040] 4. Online cooling process: Rapid cooling can effectively preserve the supersaturated solid solution state of the matrix, providing a solute basis for subsequent aging strengthening and ensuring the mechanical properties of the alloy.
[0041] 5. Aging process: Different aging regimes can be adjusted to enhance the precipitation state of the phase and adapt to the performance requirements under different working conditions.
[0042] Example 1 (1) The chemical composition of the alloy is: Mg: 0.65%, Si: 0.6%, Sn: 0.55%, Bi: 0.33%, with the balance being Al and unavoidable impurities, wherein the content of a single impurity element does not exceed 0.50%, and the total content of impurities does not exceed 1.00%.
[0043] (2) The ingots were melted at 740℃, refined and degassed, and then allowed to stand and remove slag. They were then cast into Φ120mm ingots using a semi-continuous casting method. (3) Cut the ingot at the head and tail, turn it or grind the surface to remove the surface oxide scale, segregation nodules and casting defects, and obtain a billet of Φ110mm×300mm to be extruded; (4) The billet to be extruded is not subjected to long-term homogenization treatment, but is directly placed in the heating furnace and heated to 490°C, and kept at the temperature for 40 minutes for short-term preheating; (5) Hot extrusion was performed using a 500-ton extruder with an extrusion ratio of 31.2, an extrusion barrel temperature of 420°C, a die temperature of 450°C, and an extrusion outlet temperature of 510°C. The extruded product was a Φ22mm bar. (6) The bar stock shall be cooled online by air cooling within 30 seconds after it is demolded; (7) After cooling, the bar stock is naturally aged for 30 days.
[0044] Example 2 (1) The chemical composition of the alloy is: Mg: 0.77%, Si: 0.63%, Sn: 0.67%, Bi: 0.45%, with the balance being Al and unavoidable impurities, wherein the content of a single impurity element does not exceed 0.50%, and the total content of impurities does not exceed 1.00%.
[0045] (2) Same as steps (2) to (3) in Example 1; (3) The billet to be extruded is not subjected to long-term homogenization treatment, but is directly placed in the heating furnace and heated to 510°C, and kept at the temperature for 30 minutes for short-term preheating, without long-term homogenization treatment; (4) Hot extrusion was performed using a 500-ton extruder with an extrusion ratio of 15.5, an extrusion barrel temperature of 480℃, a die temperature of 475℃, and an extrusion outlet temperature of 520℃. The extrusion was formed into Φ22mm bars. (4) Spray cooling is used for online cooling within 30 seconds after demolding; (5) After cooling, the bar is artificially aged at 175℃ for 6 hours.
[0046] Example 3 (1) The chemical composition of the alloy is: Mg: 0.95%, Si: 0.88%, Sn: 0.80%, Bi: 0.58%, with the balance being Al and unavoidable impurities, wherein the content of a single impurity element does not exceed 0.50%, and the total content of impurities does not exceed 1.00%.
[0047] (2) Same as steps (2) to (3) in Example 1; (3) The billet to be extruded is not subjected to long-term homogenization treatment, but is directly placed in the heating furnace and heated to 500°C, and kept at the temperature for 50 minutes for short-term preheating, without long-term homogenization treatment; (4) Hot extrusion was performed using a 500-ton extruder with an extrusion ratio of 47, an extrusion barrel temperature of 500℃, a die temperature of 490℃, and an extrusion outlet temperature of 530℃. The extrusion was formed into Φ22mm bars. (5) Use water cooling for online cooling within 30 seconds after demolding; (6) After cooling, the bar is first naturally aged for 7 days, and then artificially aged at 160℃ for 8 hours to complete the composite aging treatment.
[0048] Comparative Example 1: Traditional Long-Term Homogenization Process (1) Same as steps (1) to (2) in Example 2; (2) The billet was kept at 565℃ for 8 hours for conventional long-term homogeneous diffusion treatment; (3) After homogenization, the billet is cooled to room temperature and then reheated to 500℃ and held for 30 minutes for preheating; (4) Samples were prepared using the same extrusion, cooling, and aging process as in Example 2.
[0049] Comparative Example 2: Excessively Long High-Temperature Preheating Process (1) Same as steps (1) to (2) in Example 2; (2) The billet is directly heated to 520°C and held at that temperature for 3 hours for high-temperature preheating, without an independent homogenization process; (3) Samples were prepared using the same extrusion, cooling, and aging process as in Example 2.
[0050] Comparative Example 3: Process with excessively low preheating temperature (1) Same as steps (1) to (2) in Example 2; (2) The billet is directly heated to 410℃ and preheated for 60 minutes; (3) Samples were prepared using the same extrusion, cooling, and aging process as in Example 2.
[0051] Results analysis: 1. The aluminum alloy extruded materials prepared in Examples 1-3 of this invention have complete surface forming, with no obvious extrusion defects visible to the naked eye. The forming quality of the samples meets the basic requirements for industrial use. The second phase in the microstructure is in a broken and dispersed state, possessing the basic conditions for qualified comprehensive mechanical properties and machinability. Figure 2 Electron micrograph of Example 2 shown.
[0052] 2. Comparative Example 1 employs a traditional long-term homogenization process, which involves a longer process flow and longer high-temperature holding time. Its microstructure and properties are affected by the long-term high-temperature diffusion, and the morphology and elemental distribution of the second phase differ significantly from those of the embodiments of this invention (e.g., Figure 3 ).
[0053] 3. Comparative Example 2 employs an excessively long high-temperature preheating process, significantly extending the high-temperature residence time of the billet. This process approaches the traditional homogeneous process, potentially inducing the evolution of a second-phase microstructure and affecting the final alloy properties (e.g., Figure 4 ).
[0054] 4. Comparative Example 3 used too low a preheating temperature, resulting in insufficient thermoplasticity of the billet and surface defects during the extrusion molding process, making it impossible to prepare qualified aluminum alloy extrusions. This proves that the lower limit of the preheating temperature specified in this invention is necessary for the process.
[0055] 5. From a process flow perspective, the embodiments of this invention do not require a long-term high-temperature homogenization process, resulting in a shorter production process, lower high-temperature energy consumption, and less equipment downtime, demonstrating significant advantages in industrial production efficiency and cost control. The specific performance differences and microstructure variations among the samples can be further quantified and verified through subsequent precise experimental testing.
[0056] The above description is not intended to limit the present invention in any way. Any modifications, alterations, or variations made by those skilled in the art without departing from the scope of the present invention using the disclosed technical content are equivalent embodiments of the present invention. At the same time, any modifications, alterations, or variations made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the present invention.
Claims
1. Al-Mg-Si-Sn-Bi free-machining aluminum alloy, characterized in that... In its preparation process, aluminum alloy ingots that have not undergone homogenization are directly heated and extruded, and after cooling, they are aged to obtain the final product.
2. The Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 1, characterized in that, The hot extrusion process involves preheating the unhomogenized aluminum alloy ingot in a heating furnace at 430°C to 540°C for 10 to 120 minutes, and then transferring it to an extruder for hot extrusion.
3. The Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 1, characterized in that, The aluminum alloy has the following chemical composition by mass percentage: Mg: 0.50%–1.20%, Si: 0.40%–1.20%, Sn: 0.20%–1.20%, Bi: 0.10%–0.80%, with the balance being Al and unavoidable impurities.
4. The Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 3, characterized in that, The preheating temperature range is 480℃~520℃, and the holding time is 20min~60min.
5. The Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 1, characterized in that, In the hot extrusion process, the extrusion ratio is 5 to 80, the extrusion barrel temperature is 350°C to 500°C, the die temperature is 350°C to 520°C, and the extrusion outlet temperature is controlled at 480°C to 560°C.
6. A method for preparing Al-Mg-Si-Sn-Bi free-machining aluminum alloy, characterized in that, Includes the following steps: (1) Prepare alloy raw materials according to mass percentage, wherein Mg: 0.50%~1.20%, Si: 0.40%~1.20%, Sn: 0.20%~1.20%, Bi: 0.10%~0.80%, and the balance is Al and unavoidable impurities; (2) The prepared alloy raw materials are smelted in a smelting furnace. After the raw materials are completely melted, they are refined and degassed. After being allowed to stand and slag is removed, they are poured using semi-continuous casting or iron mold casting to obtain ingots. (3) Cut the ingot at the head and tail, turn it or grind the surface to remove the surface oxide scale, segregation nodules and casting defects, and obtain the billet to be extruded; (4) The billet to be extruded is directly placed into the heating furnace for preheating; (5) Transfer the preheated billet to the extruder for hot extrusion to obtain the extruded material; (6) The extruded material is cooled online immediately after being demolded; (7) Aging treatment is performed on the cooled extruded material.
7. The method for preparing the Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 6, characterized in that, In step (3), the preheating temperature is controlled at 430℃~540℃ and the heat preservation time is controlled at 10min~120min.
8. The method for preparing the Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 6, characterized in that, In the hot extrusion of step (5), the extrusion ratio is 5 to 80, the extrusion cylinder temperature is 350°C to 500°C, the die temperature is 350°C to 520°C, and the extrusion outlet temperature is controlled at 480°C to 560°C.
9. The method for preparing the Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 6, characterized in that, In step (6), the cooling method can be air cooling, wind cooling, spray cooling, water cooling, or any combination thereof.
10. The method for preparing the Al-Mg-Si-Sn-Bi free-machining aluminum alloy according to claim 6, characterized in that, In step (7), the aging process can be natural aging, artificial aging, or a combination of natural and artificial aging. The natural aging time is 1 day to 60 days; the artificial aging temperature is 150℃ to 200℃, and the heat preservation time is 2 hours to 12 hours.