Film forming methods and film forming apparatus

By selectively adsorbing and oxidizing, the embedding shape of the silicon oxide film within the recess is controlled, solving the problem of difficult shape control of silicon oxide films in the prior art, and achieving precise control of the uniformity and thickness of the silicon oxide film.

CN123063744APending Publication Date: 2026-11-10TOKYO ELECTRON LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610579212.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-29
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing technologies make it difficult to effectively control the shape of the silicon oxide film embedded in the recess.

Method used

By employing a selective adsorption and oxidation method, different types of silicon raw materials and oxidants are supplied to the substrate to control the embedding shape of the silicon oxide film in the recess. This includes selectively adsorbing and oxidizing a first silicon raw material and a second silicon raw material, and repeating the process to form a silicon oxide film with the desired thickness and shape.

Benefits of technology

Precise control over the shape and thickness of the silicon oxide film within the recess was achieved, ensuring that the uniformity and thickness of the silicon oxide film met design requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123063744A_ABST
    Figure CN123063744A_ABST
Patent Text Reader

Abstract

This invention provides a film-forming method and an apparatus capable of controlling the embedding shape when embedding a silicon oxide film within a recess. One aspect of the film-forming method includes the following steps: supplying a first silicon material to a substrate having a recess, causing the first silicon material to selectively adsorb onto the upper portion of the recess; supplying a second silicon material to the substrate, causing the second silicon material to adsorb onto a region within the recess where the first silicon material has not been adsorbed; supplying an oxidant to the substrate, causing the second silicon material adsorbed within the recess to oxidize; and sequentially repeating the steps of adsorbing the first silicon material, adsorbing the second silicon material, and oxidizing the second silicon material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a film-forming method and a film-forming apparatus. Background Technology

[0002] Patent document 1 discloses that when a silicon nitride film is embedded in a recess formed in a substrate, chlorine-containing gas is physically adsorbed in a predetermined area from the top of the recess to a predetermined depth, thereby forming non-adsorption sites for silicon-containing gas in the predetermined area.

[0003] Existing technical documents

[0004] Patent documents

[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-10950 Summary of the Invention

[0006] The problem the invention aims to solve

[0007] This disclosure provides a technique for controlling the embedding shape when embedding a silicon oxide film in a recess.

[0008] Solution for solving the problem

[0009] One aspect of the film formation method disclosed herein includes the following steps: supplying a first silicon material to a substrate having recesses, such that the first silicon material is selectively adsorbed onto the upper portion of the recesses; supplying a second silicon material to the substrate, such that the second silicon material is adsorbed onto a region within the recesses where the first silicon material has not been adsorbed; supplying an oxidant to the substrate, such that the second silicon material adsorbed within the recesses is oxidized; and sequentially repeating the steps of adsorbing the first silicon material, adsorbing the second silicon material, and oxidizing the second silicon material.

[0010] The effects of the invention

[0011] According to this disclosure, the embedding shape can be controlled when embedding a silicon oxide film in a recess. Attached Figure Description

[0012] Figure 1 This is a schematic cross-sectional view showing the film-forming apparatus according to the embodiment.

[0013] Figure 2 yes Figure 1 A top view of the film-forming apparatus.

[0014] Figure 3 This is a cross-sectional view (1) showing a first example of the film-forming method involved in the embodiment.

[0015] Figure 4 This is a cross-sectional view (2) showing a first example of the film-forming method involved in the embodiment.

[0016] Figure 5 This is a cross-sectional view showing a second example of the film-forming method involved in the embodiment. Detailed Implementation

[0017] Hereinafter, non-limiting exemplary embodiments of the present disclosure will be described with reference to the accompanying drawings. In all the drawings, the same or corresponding components or parts are labeled with the same or corresponding reference numerals, and repeated descriptions are omitted.

[0018] [Film-forming device]

[0019] Figure 1 This is a schematic cross-sectional view showing the film-forming apparatus 100 according to the embodiment. Figure 2 yes Figure 1 A top view of the film-forming apparatus 100. Figure 2 For ease of explanation, the illustration of the top plate 11 is omitted.

[0020] The film deposition apparatus 100 includes a generally cylindrical processing container 1 and a rotary table 2 for rotating a substrate W within the processing container 1. The substrate W is, for example, a semiconductor wafer. The film deposition apparatus 100 includes a control unit 110 for controlling various structures of the apparatus.

[0021] Processing container 1 houses multiple substrates W and has internal processing chambers for forming silicon oxide films on each substrate W. Processing container 1 has a top plate 11, a container body 12, and a sealing member 13. The top plate 11 is detachable from the container body 12. The sealing member 13 is annular and disposed on the upper surface of the outer peripheral wall of the container body 12. Thus, the top plate 11 is hermetically fixed to the container body 12. The sealing member 13 is, for example, an O-ring.

[0022] A separation gas supply pipe 16 for supplying separation gases such as nitrogen (N2) and argon (Ar) is connected to the center of the top plate 11. A purge gas supply pipe 17 for supplying purge gases such as nitrogen and argon is connected to the bottom part 14 of the container body 12. Multiple purge gas supply pipes 17 are arranged along the circumference of the bottom part 14. The bottom part 14 has an annular protrusion 12a at a position close to the outer peripheral surface of the core 21 of the fixed rotating stage 2.

[0023] The outer peripheral wall of the processing container 1 is provided with a transfer port 15 for transferring substrate W between the rotary table 2 and the transfer arm 10, and a gate valve (not shown) for opening and closing the transfer port 15. When the transfer port 15 is closed, the gate valve airtightly seals the processing chamber of the processing container 1. The rotary table 2 is provided with a mounting section 24 for placing substrate W adjacent to the transfer port 15, thereby facilitating the transfer of substrate W between it and the transfer arm 10.

[0024] The rotary table 2 is housed within the processing container 1. The rotary table 2 is fixed to a generally disc-shaped core 21 at the center of the processing container 1. The core 21 is connected to a rotating shaft 22 extending vertically. The rotating shaft 22 is supported by a drive unit 23. The drive unit 23 uses the rotating shaft 22 to rotate the rotary table 2 around the vertical axis (…). Figure 2 (rotate clockwise) in the middle.

[0025] The lower end of the rotating shaft 22 and the drive unit 23 are housed in the housing 20. The housing 20 is hermetically mounted on the bottom part 14 of the processing container 1. A purge gas supply pipe 27 for supplying purge gas to the area below the rotating stage 2 is connected to the housing 20.

[0026] The rotary table 2 has, for example, multiple (five in the illustrated example) circular mounting portions 24 on its surface, each capable of holding a substrate W with a diameter of 300 mm. Multiple mounting portions 24 are arranged at equal intervals along the rotation direction of the rotary table 2. Each mounting portion 24 has an inner diameter slightly larger than the diameter of the substrate W (approximately 1 mm to 4 mm). The depth of the mounting portion 24 is set to be greater than or equal to the thickness of the substrate W.

[0027] The bottom surface of the mounting section 24 has multiple (e.g., three) through holes (not shown) through which multiple lifting pins (not shown) pass. Each lifting pin is located at the junction of the substrate W near the transfer port 15 and is moved up and down in the vertical direction by a lifting mechanism (not shown). Each lifting pin rises to receive the substrate W after the transfer arm 10 holding the substrate W enters, and falls back down to place the substrate W in the mounting section 24 after the transfer arm 10 retracts. Each lifting pin raises the substrate W after substrate processing and transfers the substrate W to the subsequent entering transfer arm 10.

[0028] Above the rotary table 2, processing gas nozzles 31, 32, and 33 and separating gas nozzles 41 and 42 are arranged at intervals around the circumference of the processing container 1. In the illustrated example, they are arranged clockwise (along...) from the conveying port 15 described later. Figure 2 (In the direction of rotation of arrow A) are arranged in sequence: processing gas nozzle 33, separating gas nozzle 41, processing gas nozzle 32, processing gas nozzle 33, and separating gas nozzle 42. Processing gas nozzles 31, 32, 33 and separating gas nozzles 41, 42 are each formed of, for example, quartz. Gas inlets 31a, 32a, 33a, 41a, 42a, respectively, serving as bases of processing gas nozzles 31, 32, 33 and separating gas nozzles 41, 42, are fixed to the outer peripheral wall of the container body 12. Thus, processing gas nozzles 31, 32, 33 and separating gas nozzles 41, 42 are introduced into the processing container 1 from the outer peripheral wall of the processing container 1, and are installed in a manner that extends horizontally relative to the rotating platform 2 along the radial direction of the container body 12.

[0029] The processing gas nozzle 31 has multiple air holes (not shown) on its lower surface side (the side facing the rotary table 2). The processing gas nozzle 31 is connected to a supply source GS1 filled with a first silicon material outside the processing container 1. The processing gas nozzle 31 ejects the first silicon material from the supply source GS1 through the air holes into the first processing area P1 on the lower side of the processing chamber. The flow rate of the first silicon material from the supply source GS1 is controlled by a flow controller FC1. The supply and stop of the first silicon material from the supply source GS1 into the processing container 1 are controlled by valves VA1 and VB1. A supply source filled with other gases, such as argon or other diluent gases, can also be connected to the processing gas nozzle 31.

[0030] The processing gas nozzle 32 has multiple air holes (not shown) on its lower surface side (the side facing the rotary table 2). The processing gas nozzle 32 is connected to a supply source GS2 filled with a second silicon material outside the processing container 1. The processing gas nozzle 32 ejects the second silicon material from the supply source GS2 through the air holes into the second processing area P2 on the lower side of the processing chamber. The flow rate of the second silicon material from the supply source GS2 is controlled by a flow controller FC2. The supply and stop of the second silicon material from the supply source GS2 into the processing container 1 are controlled by valves VA2 and VB2. A supply source filled with other gases, such as argon or other diluent gases, can also be connected to the processing gas nozzle 32. For example, the processing gas nozzle 32 is arranged adjacent to the processing gas nozzle 31 along the rotation direction of the rotary table 2.

[0031] The processing gas nozzle 33 has multiple orifices (not shown) on its lower surface side (the side facing the rotary table 2). The processing gas nozzle 33 is connected to a supply source GS3 filled with oxidant outside the processing container 1. The processing gas nozzle 33 sprays the oxidant from the supply source GS3 through the orifices into the third processing zone P3 on the lower side of the processing chamber. The flow rate of the oxidant from the supply source GS3 is controlled by a flow controller FC3. The supply and stop of the oxidant from the supply source GS3 into the processing container 1 are controlled by valves VA3 and VB3. The oxidant may be, for example, ozone (O3) gas or a mixture of hydrogen and oxygen. A supply source filled with other gases, such as argon or other diluent gases, may also be connected to the processing gas nozzle 33.

[0032] A separating gas nozzle 41 forms a separating region D1 that separates the first processing region P1 from the third processing region P3. The separating gas nozzle 41 has multiple orifices (not shown) on its lower surface side (the side facing the rotary table 2). A supply source GS6 filled with separating gas is connected to the separating gas nozzle 41. The separating gas nozzle 41 sprays the separating gas from the supply source GS6 through the orifices into the separating region D1 on the lower side of the processing chamber. The flow rate of the separating gas from the supply source GS6 is controlled by a flow controller FC6. The supply and stop of the separating gas from the supply source GS6 into the processing container 1 are controlled by valves VA6 and VB6. The separating gas is, for example, an inert gas such as nitrogen or argon.

[0033] A separation gas nozzle 42 forms a separation zone D2 that separates the second processing zone P2 from the third processing zone P3. The separation gas nozzle 42 has multiple orifices (not shown) on its lower surface side (the side facing the rotary table 2). A supply source GS7 filled with separation gas is connected to the separation gas nozzle 42. The separation gas nozzle 42 ejects the separation gas from the supply source GS7 through the orifices into the separation zone D2 on the lower side of the processing chamber. The flow rate of the separation gas from the supply source GS7 is controlled by a flow controller FC7. The supply and stop of the separation gas from the supply source GS7 into the processing container 1 are controlled by valves VA7 and VB7. The separation gas is, for example, an inert gas such as nitrogen or argon.

[0034] In the separation zones D1 and D2, and on the back side of the top plate 11 of the processing container 1, there is a generally fan-shaped protrusion 4. The protrusion 4 protrudes downward from the back side of the top plate 11. The protrusion 4 has a groove (not shown) extending radially in the circumferential center, and each separation gas nozzle 41, 42 is accommodated in the groove.

[0035] A protrusion 5 is provided at the center of the lower surface of the top plate 11. The protrusion 5 is continuous with the portion of the convex portion 4 near the center region C and is formed in a generally circular shape along the circumference. The lower surface of the protrusion 5 is formed to the same height as the lower surface of the convex portion 4.

[0036] A first exhaust port 61 and a second exhaust port 62 are provided on the bottom part 14 of the processing container 1. The first exhaust port 61 is located between the processing gas nozzle 31 and the separation zone D2. The second exhaust port 62 is located between the processing gas nozzle 33 and the separation zone D1. The first exhaust port 61 mainly discharges the first silicon raw material, the second silicon raw material, and the separation gas, while the second exhaust port 62 mainly discharges the oxidant and the separation gas. The first exhaust port 61 and the second exhaust port 62 are respectively connected to an exhaust device 64 such as a vacuum pump via an exhaust pipe 63. A pressure controller 65 such as a butterfly valve is provided on the exhaust pipe 63.

[0037] The film-forming apparatus 100 has a heater unit 7 in the space between the bottom surface 14 of the processing container 1 and the rotating stage 2. The heater unit 7 is housed within a cover 71 supported by a protrusion 12a of the container body 12. The heater unit 7 heats the substrate W on the rotating stage 2 to a predetermined temperature.

[0038] The control unit 110 is an electronic circuit such as a CPU (Central Processing Unit), FPGA (Field Programmable Gate Array), or ASIC (Application Specific Integrated Circuit). The control unit 110 executes various control actions described in this application specification by executing instruction codes stored in memory or by designing circuits for special purposes.

[0039] [Film Formation Method]

[0040] (first example)

[0041] Figure 3 and Figure 4 This is a cross-sectional view showing a first example of the film-forming method according to the embodiment. Hereinafter, an example will be given of forming a silicon oxide film in the recess 200 formed on the surface of the substrate W in the aforementioned film-forming apparatus 100. In the first example, the first silicon raw material is a silicon-containing gas containing one silicon (Si) per molecule, the second silicon raw material is a silicon-containing gas containing two silicon atoms per molecule, the oxidant is ozone gas, and the purge gas and separation gas are nitrogen gas. Examples of silicon-containing gases containing one silicon atom per molecule include, for example, aminosilane gases such as tris(dimethylamino)silane (TDMAS), diisopropylaminosilane (DIPAS), and bis(tert-butylamino)silane (BTBAS), and chlorosilane gases such as dichlorosilane (DCS) and trichlorosilane (TrCS). Examples of silicon-containing gases containing two silicon atoms per molecule include, for example, hexachlorosilane (HCD).

[0042] First, the control unit 110 controls the film-forming apparatus 100, causing each placement section 24 of the rotary table 2, which places the substrate W within the processing container 1, to... Figure 3 As shown in Figure (a), grooves, holes, and other recesses 200 are formed on the surface of the substrate W. Each recess 200 has a bottom surface 201, a side surface 202, and a top surface 203. Hydroxyl groups (OH) are formed, for example, on the bottom surface 201, the side surface 202, and the top surface 203. The lower portions of the bottom surface 201 and the side surface 202 constitute the lower portion of the recess 200, and the upper portions of the side surface 202 and the top surface 203 constitute the upper portion of the recess 200.

[0043] Next, the control unit 110 controls valves VA6 and VB6 and flow controller FC6 to supply nitrogen gas from the separation gas nozzle 41 to the separation zone D1. Additionally, the control unit 110 controls valves VA7 and VB7 and flow controller FC7 to supply nitrogen gas from the separation gas nozzle 42 to the separation zone D2. Furthermore, the control unit 110 controls valves (not shown) and flow controllers (not shown) to supply nitrogen gas from the separation gas supply pipe 16 and purge gas supply pipes 17 and 27 into the processing container 1. Additionally, the control unit 110 controls the pressure controller 65 to achieve the desired pressure within the processing container 1. Furthermore, the control unit 110 controls the drive unit 23 to rotate the rotary table 2 clockwise at the desired rotational speed. Finally, the control unit 110 controls the heater unit 7 to achieve the desired temperature of the substrate W.

[0044] Next, the control unit 110 controls valves VA1 and VB1 and the flow controller FC1 to supply the first silicon material from the processing gas nozzle 31 to the first processing zone P1. Thus, in the first processing zone P1, as... Figure 3 As shown in Figure (b), the first silicon material is selectively adsorbed onto the upper part of the recess 200 of the substrate W. Figure 3 In Figure (b), -R1 represents the substituents contained in the first silicon raw material. The multiple substituents -R1 contained in the first silicon raw material can be all the same or some different. For example, by adjusting the flow rate of the first silicon raw material, the rotation speed of the rotary table 2, the pressure inside the processing container 1, etc., the first silicon raw material can be selectively adsorbed onto the upper part of the recess 200.

[0045] The control unit 110 controls valves VA2 and VB2 and flow controller FC2 to supply the second silicon material from the processing gas nozzle 32 to the second processing zone P2. Thus, in the second processing zone P2, as... Figure 3 As shown in Figure (c), the second silicon material is adsorbed into the region within the recess 200 where the first silicon material is not adsorbed. Figure 3 In Figure (c), -R2 represents a substituent contained in the second silicon material. The multiple substituents -R2 contained in the second silicon material can be all the same or some different. In the substrate W, which moves from the first processing region P1 to the second processing region P2 as the rotary table 2 rotates, the first silicon material is adsorbed onto the upper part of the recess 200. The second silicon material readily adsorbs onto the hydroxyl group (OH) but is difficult to adsorb onto the region where the first silicon material is adsorbed. Therefore, as... Figure 3 As shown in Figure (c), the adsorption of the second silicon material in the upper part of the recess 200 is suppressed, and it is adsorbed in the lower part of the recess 200. For example, by making the flow rate of the second silicon material greater than that of the first silicon material, the second silicon material can easily reach the lower part of the recess 200, and the second silicon material can easily be adsorbed in the lower part of the recess 200.

[0046] The control unit 110 controls valves VA3 and VB3 and flow controller FC3 to supply ozone gas from the treatment gas nozzle 33 to the third treatment zone P3. Thus, in the third treatment zone P3, as... Figure 3 As shown in Figure (d), the first silicon material adsorbed on the upper part of the recess 200 and the second silicon material adsorbed on the lower part of the recess 200 are oxidized. At this time, the first silicon material contains one silicon in one molecule, and the second silicon material contains two silicon in one molecule. Therefore, the number of SiO layers at the lower part of the recess 200 is twice the number of SiO layers at the upper part of the recess 200.

[0047] The control unit 110 controls the drive unit 23 to continue rotating the rotary table 2. Thus, while maintaining the substrate W at the desired temperature, the adsorption of the first silicon material onto the upper part of the recess 200, the adsorption of the second silicon material onto the lower part of the recess 200, and the oxidation of the first and second silicon materials are repeated sequentially. The result is as follows: Figure 4 As shown, a silicon oxide film 210 with a desired thickness is formed on the surface of the recess 200. At this time, the first silicon raw material contains one silicon unit per molecule, and the second silicon raw material contains two silicon units per molecule. Therefore, the number of SiO layers at the lower part of the recess 200 is twice the number of SiO layers at the upper part of the recess 200. As a result, a thicker silicon oxide film 210 can be formed at the lower part compared to the upper part of the recess 200.

[0048] When the silicon oxide film 210 reaches the desired thickness, the control unit 110 controls valves VA1~VA3, VB1~VB3, and flow controllers FC1~FC3 to stop supplying gases from the processing gas nozzles 31, 32, and 33. Additionally, the control unit 110 controls valves VA6~VA7, VB6~VB7, and flow controllers FC6~FC7 to stop supplying nitrogen from the separation gas nozzles 41 and 42. Furthermore, the control unit 110 controls the valves and flow controllers to stop supplying nitrogen from the separation gas supply pipe 16 and the purge gas supply pipes 17 and 27.

[0049] Next, the control unit 110 controls the film forming apparatus 100 to remove the substrates W of each placement part 24 of the rotary table 2 placed in the processing container 1 from the processing container 1.

[0050] exist Figure 3 and Figure 4In the example, the case where the first silicon material is a silicon material containing one silicon in one molecule and the second silicon material is a silicon material containing two silicon in one molecule has been described, but it is not limited to this. For example, the first silicon material could be a silicon material containing one silicon in one molecule, and the second silicon material could be a silicon material containing three or more silicon in one molecule. For example, the first silicon material could be a silicon material containing two silicon in one molecule, and the second silicon material could be a silicon material containing three or more silicon in one molecule. In this case, the second silicon material can be a silicon material containing more silicon in one molecule compared to the first silicon material. In this case, a thicker silicon oxide film 210 can be formed in the lower part compared to the upper part of the recess 200.

[0051] Alternatively, for example, the first silicon material may be a silicon material containing more silicon per molecule than the second silicon material. In this case, a thicker silicon oxide film 210 can be formed on the upper part compared to the lower part of the recess 200.

[0052] As explained above, in the first example of the film-forming method of the embodiment, the amount of silicon contained in one molecule of the first silicon raw material is different from the amount of silicon contained in one molecule of the second silicon raw material. Therefore, the embedding shape when the silicon oxide film 210 is embedded in the recess 200 can be controlled.

[0053] (Second example)

[0054] Figure 5 This is a cross-sectional view showing a second example of the film-forming method according to the embodiment. Hereinafter, an example will be given of forming a silicon oxide film in the recess 200 formed on the surface of the substrate W in the aforementioned film-forming apparatus 100. In this second example, the first silicon raw material is a chlorosilane gas, the second silicon raw material is an aminosilane gas, the oxidant is ozone gas, and the purge gas and separation gas are nitrogen. Examples of chlorosilane gases include dichlorosilane (DCS), trichlorosilane (TrCS), and hexachlorosilane (HCD). Examples of aminosilane gases include tris(dimethylamino)silane (TDMAS), diisopropylaminosilane (DIPAS), and bis(tert-butylamino)silane (BTBAS).

[0055] First, the control unit 110 controls the film-forming apparatus 100, causing each placement section 24 of the rotary table 2, which places the substrate W within the processing container 1, to... Figure 5As shown in Figure (a), grooves, holes, and other recesses 200 are formed on the surface of the substrate W. Each recess 200 has a bottom surface 201, a side surface 202, and a top surface 203. Hydroxyl groups (OH) are formed, for example, on the bottom surface 201, the side surface 202, and the top surface 203. The lower portions of the bottom surface 201 and the side surface 202 constitute the lower portion of the recess 200, and the upper portions of the side surface 202 and the top surface 203 constitute the upper portion of the recess 200.

[0056] Next, the control unit 110 controls valves VA6 and VB6 and flow controller FC6 to supply nitrogen gas from the separation gas nozzle 41 to the separation zone D1. Additionally, the control unit 110 controls valves VA7 and VB7 and flow controller FC7 to supply nitrogen gas from the separation gas nozzle 42 to the separation zone D2. Furthermore, the control unit 110 controls valves (not shown) and flow controllers (not shown) to supply nitrogen gas from the separation gas supply pipe 16 and purge gas supply pipes 17 and 27 into the processing container 1. Additionally, the control unit 110 controls the pressure controller 65 to achieve the desired pressure within the processing container 1. Furthermore, the control unit 110 controls the drive unit 23 to rotate the rotary table 2 clockwise at the desired rotational speed. Finally, the control unit 110 controls the heater unit 7 to achieve the desired temperature of the substrate W.

[0057] Next, the control unit 110 controls valves VA1 and VB1 and the flow controller FC1 to supply the first silicon material from the processing gas nozzle 31 to the first processing zone P1. Thus, in the first processing zone P1, as... Figure 5 As shown in Figure (b), the first silicon material is selectively adsorbed onto the upper part of the recess 200 of the substrate W. For example, by adjusting the flow rate of the first silicon material, the rotation speed of the rotary table 2, the pressure inside the processing container 1, etc., the first silicon material can be selectively adsorbed onto the upper part of the recess 200.

[0058] The control unit 110 controls valves VA2 and VB2 and flow controller FC2 to supply the second silicon material from the processing gas nozzle 32 to the second processing zone P2. Thus, in the second processing zone P2, as... Figure 5 As shown in Figure (c), the second silicon material is adsorbed into the region within the recess 200 where the first silicon material is not adsorbed. Figure 5 In Figure (c), -R3 represents a substituent in the second silicon material. The multiple substituents -R3 in the second silicon material can be all the same or some can be different. In the substrate W, which moves from the first processing region P1 to the second processing region P2 as the rotary table 2 rotates, the first silicon material is adsorbed onto the upper part of the recess 200. The second silicon material readily adsorbs onto hydroxyl (OH) groups but is difficult to adsorb onto chlorine (Cl) terminals. Therefore, as... Figure 5As shown in Figure (c), the adsorption of the second silicon material in the upper part of the recess 200 is suppressed, and it is adsorbed in the lower part of the recess 200.

[0059] The control unit 110 controls valves VA3 and VB3 and flow controller FC3 to supply ozone gas from the treatment gas nozzle 33 to the third treatment zone P3. Thus, in the third treatment zone P3, as... Figure 5 As shown in Figure (d), the oxidation of the first silicon material is suppressed by the chlorine terminals contained in the first silicon material adsorbed on the upper part of the recess 200, while the second silicon material adsorbed on the lower part of the recess 200 is oxidized. In the substrate W, which moves from the second processing region P2 to the third processing region P3 as the rotary table 2 rotates, a large number of Si-H bonds exist in the lower part of the recess 200, while a large number of Si-Cl bonds exist in the upper part of the recess 200. The binding energy of the Si-Cl bonds is greater than that of the Si-H bonds. Therefore, when ozone gas is supplied to the substrate W, the TDMAS gas adsorbed on the lower part of the recess 200 reacts more readily with the ozone gas than the TDMAS gas adsorbed on the upper part of the recess 200. As a result, the TDMAS gas adsorbed on the lower part of the recess 200 is selectively oxidized, and hydroxyl groups (OH) are selectively formed in the lower part of the recess 200.

[0060] The control unit 110 controls the drive unit 23 to continue rotating the rotary table 2. Thus, while maintaining the substrate W at the desired temperature, the adsorption of the first silicon material onto the upper part of the recess 200, the adsorption of the second silicon material onto the lower part of the recess 200, and the oxidation of the second silicon material are repeated sequentially. As a result, a silicon oxide film 210 with the desired thickness is formed on the surface of the recess 200. At this time, the first silicon material is a chlorosilane gas, and the second silicon material is an aminosilane gas. Therefore, oxidation of the first silicon material gas can be suppressed at the upper part of the recess 200, and oxidation of the second silicon material can be achieved at the lower part of the recess 200. As a result, a thicker silicon oxide film 210 can be formed at the lower part of the recess 200 compared to the upper part.

[0061] When the silicon oxide film 210 reaches the desired thickness, the control unit 110 controls valves VA1~VA3, VB1~VB3, and flow controllers FC1~FC3 to stop supplying gases from the processing gas nozzles 31, 32, and 33. Additionally, the control unit 110 controls valves VA6~VA7, VB6~VB7, and flow controllers FC6~FC7 to stop supplying nitrogen from the separation gas nozzles 41 and 42. Furthermore, the control unit 110 controls the valves and flow controllers to stop supplying nitrogen from the separation gas supply pipe 16 and the purge gas supply pipes 17 and 27.

[0062] Next, the control unit 110 controls the film forming apparatus 100 to remove the substrates W of each placement part 24 of the rotary table 2 placed in the processing container 1 from the processing container 1.

[0063] exist Figure 5 The example illustrates a scenario where the first silicon material is a chlorosilane gas and the second silicon material is an aminosilane gas, but this is not a limitation. The second silicon material can be any silicon material whose oxidation rate against ozone gas is greater than that against ozone gas. In this case, a thicker silicon oxide film 210 can be formed in the lower portion compared to the upper portion of the recess 200. For example, the first silicon material could be a halogen-containing silane gas, and the second silicon material could be a halogen-free silane gas.

[0064] Alternatively, for example, the second silicon material can be a silicon material containing more silicon per molecule than the first silicon material, and having a higher oxidation rate against ozone gas than the first silicon material against ozone gas. In this case, a particularly thick silicon oxide film 210 can be formed in the lower part compared to the upper part of the recess 200.

[0065] Furthermore, for example, the oxidation rate of the first silicon material for ozone gas can be greater than the oxidation rate of the second silicon material for ozone gas. In this case, a thicker silicon oxide film 210 can be formed on the upper part compared to the lower part of the recess 200.

[0066] As explained above, in the second example of the film-forming method according to the embodiment, the oxidation rate of the first silicon material for ozone gas is different from the oxidation rate of the second silicon material for ozone gas. Therefore, the embedding shape when embedding the silicon oxide film 210 in the recess 200 can be controlled.

[0067] [experiment]

[0068] In the experiment, the effect of the type of silicon raw material on the cycle rate of silicon oxide film 210 was evaluated.

[0069] In the experiment, a silicon oxide film 210 was formed by sequentially repeating the adsorption of silicon material onto the substrate W and the oxidation of silicon material. Furthermore, the cycle rate of the silicon oxide film 210 was calculated by measuring its thickness. The cycle rate is the thickness of the silicon oxide film 210 formed during one cycle of silicon material adsorption onto the substrate W and silicon material oxidation.

[0070] In the experiment, a substrate W with a silicon oxide film formed on its surface was used. TDMAS and TrCS gases were used as silicon raw materials, and a mixture of hydrogen and oxygen was used as an oxidant. The temperature of the substrate W was set to 760°C, and the pressure inside the processing container 1 was set to 6.7 Torr.

[0071] The experimental results show that the cycling rate when the silicon feedstock is TrCS gas is approximately 0.4 times that when the silicon feedstock is TDMAS gas. Based on this result, it can be concluded that the cycling rate of the silicon oxide film 210 can be varied by changing the type of silicon feedstock.

[0072] The embodiments disclosed herein should be considered illustrative in all respects and not restrictive. The above embodiments may also be omitted, substituted, or modified in various ways without departing from the appended claims and their spirit.

[0073] In the above embodiments, the oxidant was described as ozone gas or a mixture of hydrogen and oxygen, but this disclosure is not limited to this. The oxidant may also be hydrogen peroxide gas. Alternatively, plasma may be generated from the oxidant.

[0074] Explanation of reference numerals in the attached figures

[0075] 200: concave portion; 201: bottom surface; 202: side surface; 203: upper surface; W: substrate.

Claims

1. A film-forming method, comprising the following steps: A first silicon material is supplied to a substrate having a recess, so that the first silicon material is selectively adsorbed onto the upper part of the recess; A second silicon material is supplied to the substrate, causing the second silicon material to be adsorbed onto the area within the recess where the first silicon material has not been adsorbed. An oxidant is supplied to the substrate to oxidize the second silicon material adsorbed in the recess; and The process of adsorbing the first silicon material, adsorbing the second silicon material, and oxidizing the second silicon material are repeated sequentially.

2. The film-forming method according to claim 1, wherein, The second silicon material contains more silicon per molecule than the first silicon material.

3. The film-forming method according to claim 2, wherein, The first silicon raw material contains one silicon atom in one molecule. The second silicon raw material contains more than two silicon atoms in one molecule.

4. The film-forming method according to claim 1, wherein, The oxidation rate of the second silicon material with respect to the oxidant is greater than the oxidation rate of the first silicon material with respect to the oxidant.

5. The film-forming method according to claim 4, wherein, The first silicon raw material contains halogens. The second silicon raw material does not contain halogens.

6. The film-forming method according to claim 5, wherein, The first silicon raw material is a chlorosilane gas. The second silicon raw material is an aminosilane gas.

7. The film-forming method according to claim 1, wherein, The process of adsorbing the first silicon material, the process of adsorbing the second silicon material, and the process of oxidizing the second silicon material are performed while maintaining the substrate at the same temperature.

8. The film-forming method according to any one of claims 1 to 7, wherein, The substrate is placed circumferentially on a rotating table disposed within a processing container. The substrate passes sequentially through a first processing area, a second processing area, and a third processing area, which are separately arranged along the rotation direction of the rotating table, thereby performing a process of adsorbing the first silicon material, a process of adsorbing the second silicon material, and a process of oxidizing the second silicon material. The first processing area is the area where the process of adsorbing the first silicon material can be performed, the second processing area is the area where the process of adsorbing the second silicon material can be performed, and the third processing area is the area where the process of oxidizing the second silicon material can be performed.

9. A film-forming apparatus for forming a silicon oxide film, wherein, The film-forming apparatus includes a control unit configured to control the film-forming apparatus. The control unit controls the film-forming apparatus to perform the following steps: A first silicon material is supplied to a substrate having a recess, so that the first silicon material is selectively adsorbed onto the upper part of the recess; A second silicon material is supplied to the substrate, causing the second silicon material to be adsorbed onto the area within the recess where the first silicon material has not been adsorbed. An oxidant is supplied to the substrate to oxidize the second silicon material adsorbed in the recess; and The process of adsorbing the first silicon material, adsorbing the second silicon material, and oxidizing the second silicon material are repeated sequentially.

Citation Information

Patent Citations

  • Deposition method of silicon nitride film

    JP2018010950A