A surface-enhanced Raman material driven by temperature difference solubility, its preparation method and application
By constructing an elemental sulfur active layer on the surface of noble metal materials using a temperature difference solubility-driven method, the portability and selectivity issues of heavy metal detection in existing technologies are solved, enabling rapid and sensitive detection and enrichment of heavy metals, applicable to nanoparticles and solid substrates.
Patent Information
- Application Number
- CN202611072214.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-20
- Publication Date
- 2026-11-10
AI Technical Summary
Existing heavy metal detection technologies rely on large instruments and complex pretreatment processes, which are difficult to meet the needs of rapid on-site screening and portable detection. Furthermore, the selective enrichment and recognition capabilities of precious metal nanostructures for heavy metal ions are limited.
A temperature-dependent solubility-driven method is employed to dissolve elemental sulfur in an organic solvent and form a sulfur active layer by cooling. This layer coats the surface of noble metal materials, creating a stable elemental sulfur active layer for the enrichment and conversion of heavy metals.
This invention provides a simple and widely applicable method for heavy metal detection, suitable for both nanoparticles and solid substrates. It enables rapid and sensitive detection of heavy metals and is suitable for large-scale preparation and field applications.
Smart Images

Figure CN123063776A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface-enhanced Raman scattering detection materials technology, and particularly relates to a surface-enhanced Raman material driven by temperature difference solubility, its preparation method and application. Background Technology
[0002] Heavy metal pollution is widespread in the environment, water bodies, food, and biological samples. Heavy metals such as mercury, lead, cadmium, copper, silver, and arsenic, and their compounds, can accumulate in organisms, causing damage to tissues such as the nervous system, kidneys, and liver. Among these, some organic heavy metal compounds, such as organomercury compounds, exhibit stronger bioaccumulation and toxicity, posing significant risks to human health and ecosystems. Therefore, establishing a rapid, sensitive, and field-applicable method for heavy metal detection is of great importance.
[0003] Existing heavy metal detection technologies mainly include inductively coupled plasma mass spectrometry, atomic absorption spectroscopy, and atomic fluorescence spectroscopy. These methods have high sensitivity, but they usually rely on large instruments, complex pretreatment, and specialized operating environments, making it difficult to meet the needs of rapid on-site screening, grassroots testing, and portable testing.
[0004] Surface-enhanced Raman scattering (SERS) technology boasts high sensitivity, strong fingerprint recognition capabilities, and fast detection speed, making it a promising application in environmental monitoring and biological sample testing. Noble metal nanomaterials such as gold and silver can provide strong electromagnetic enhancement effects and are commonly used surface-enhanced Raman materials. However, pure noble metal nanostructures typically primarily provide physical enhancement, with limited selective enrichment and recognition capabilities for heavy metal ions.
[0005] Sulfur exhibits strong interactions with various heavy metals, forming metal-sulfur coordination structures or metal sulfides. These metal-sulfur structures typically possess characteristic Raman vibration peaks in the low wavenumber region. Therefore, constructing an elemental sulfur active layer on the surface of a noble metal-enhanced Raman spectroscopy material can help create a detection interface that simultaneously possesses electromagnetic enhancement and heavy metal enrichment / conversion capabilities.
[0006] However, existing sulfur layer construction methods often involve complex liquid-phase chemical deposition, which presents problems such as high process temperature, high equipment requirements, incompatibility with flexible substrates, poor deposition uniformity, bulk sulfur particle contamination, and hot spot shading. Summary of the Invention
[0007] To overcome the shortcomings of the prior art, this invention provides a surface-enhanced Raman material driven by temperature difference solubility, its preparation method, and its applications. This invention also provides a mild, controllable, widely applicable, and easily scalable method for constructing sulfur active layers.
[0008] To achieve one of the above objectives, the present invention adopts the following technical solution: A method for preparing surface-enhanced Raman materials based on temperature difference solubility, comprising the following steps: S1. At the first temperature T1, elemental sulfur is added to an organic solvent to dissolve the elemental sulfur and obtain a saturated elemental sulfur solution (the organic solvent is saturated at T1). S2. Remove undissolved sulfur particles from the elemental sulfur solution to obtain a clear elemental sulfur solution; S3. Immerse the precious metal material to be coated in the clear elemental sulfur solution obtained in step S2; S4. While keeping the precious metal material to be coated in contact with the clear elemental sulfur solution obtained in step S2, the system is cooled from the first temperature T1 to the second temperature T2, so that the elemental sulfur becomes supersaturated due to the decrease in solubility, and an elemental sulfur active layer is formed by heterogeneous deposition on the surface of the precious metal material. S5. After post-processing, a surface-enhanced Raman material with elemental sulfur coated on noble metals is obtained.
[0009] Preferably, the first temperature T1 is 30-90℃, more preferably 45-60℃; the second temperature T2 is 0-35℃, more preferably 10-30℃; and the temperature of the second temperature T2 is lower than the temperature of the first temperature T1. The temperature difference between the first temperature T1 and the second temperature T2 is 5-70℃, more preferably 10-40℃, and even more preferably 15-30℃.
[0010] Preferably, the solvent is one or a combination of two or more of alcohol solvents, nitrile solvents, ester solvents and ether solvents; the organic solvent is one or a combination of two or more of ethanol, isopropanol, acetonitrile, ethyl acetate and tetrahydrofuran, preferably ethanol.
[0011] Preferably, when the noble metal material to be coated is noble metal nanoparticles, the post-processing in step S5 is as follows: after centrifugation, discarding the supernatant, solvent resuspension and washing, the free sulfur particles are removed and then dispersed in water to obtain elemental sulfur-coated noble metal surface-enhanced Raman material. Furthermore, the noble metal nanoparticles are washed and purified before being immersed in the clarified elemental sulfur solution in step S3 to remove free ligands, salts, and reaction byproducts.
[0012] Preferably, when the noble metal material to be coated is a solid noble metal SERS substrate, the post-processing in step S5 is as follows: first, remove the substrate from the solid noble metal SERS substrate, then rinse and dry the remaining material with an organic solvent to obtain a noble metal surface-enhanced Raman material coated with elemental sulfur.
[0013] Preferably, in step S2, the method for removing undissolved sulfur particles is one of filtration, centrifugation, and settling to obtain the supernatant; Repeat steps S3-S5 1-10 times to adjust the thickness and coverage of the elemental sulfur active layer; In step S4, the cooling method is natural cooling or programmed cooling; the cooling rate of programmed cooling is 0.05-10℃ / min, preferably 0.1-2℃ / min.
[0014] To achieve the second objective mentioned above, the present invention provides a surface-enhanced Raman spectroscopy (SERS) material driven by temperature difference solubility: the material includes a noble metal material and a single-element sulfur active layer deposited on the surface of the noble metal material; the noble metal material is a noble metal nanoparticle or a solid noble metal SERS substrate containing a noble metal nanostructure layer; the single-element sulfur active layer is formed by heterogeneous deposition of a single-element sulfur solution on the surface of the noble metal material due to the decrease in solubility during the cooling process.
[0015] Preferably, the noble metal nanoparticles are one or more of gold nanoparticles, silver nanoparticles, and gold-silver alloy nanoparticles; the particle size of the gold nanoparticles is 5-200 nm, preferably 50-80 nm, and more preferably 60-70 nm. The solid noble metal SERS substrate includes a supporting substrate and a noble metal nanostructure layer located on the surface of the supporting substrate; the supporting substrate is one or more of silicon wafers, glass, quartz, ceramics and polymer films; the noble metal nanostructure layer is one or more of gold, silver and gold-silver alloys; the morphology of the noble metal nanostructure layer is one or more of nanoparticle assembly layers, nanoislands, nanopores, nanopillars, nanocones, nanoshells, rough metal films. The thickness of the elemental sulfur active layer is 0.5-50 nm, preferably 1-20 nm.
[0016] To achieve the third objective mentioned above, this invention provides an application of a surface-enhanced Raman spectroscopy material driven by temperature difference: this material is used in the detection of heavy metals, including inorganic heavy metal ions and organic heavy metal compounds; the inorganic heavy metal ions are Hg. 2+ Pb 2+ Cd 2+ Cu 2+ Ag + As 3+ And As 5+ One or more of the following: the organomercury compound is an organomercury compound, a heavy metal compound containing a metal-carbon bond, or a heavy metal compound containing a metal-organic group structure.
[0017] Preferably, the specific steps are as follows: The sample to be tested is brought into contact with a surface-enhanced Raman spectroscopy material; heavy metal ions in the sample are enriched, coordinated, or transformed on the surface of the elemental sulfur active layer, forming a metal-sulfur interaction structure or metal sulfide; samples are collected at depths less than 500 cm. -1Surface-enhanced Raman spectroscopy in the low wavenumber region; qualitative or quantitative analysis based on metal-sulfur vibrational peaks or characteristic peaks of metal sulfides; The detection was performed using surface-enhanced Raman spectroscopy in the low wavenumber region, which is less than 500 cm⁻¹. -1 The Raman shift region; a 785 nm laser was used as the excitation source during detection; The sample to be tested can be one or more of the following: water sample, serum, plasma, whole blood, urine, food extract, and environmental sample extract.
[0018] The advantages of this invention are: (1) A material is provided that can be prepared under mild conditions without the need for high-temperature sublimation or vacuum equipment. It is suitable for nanoparticle and solid noble metal SERS substrate systems and can be used for the enrichment, conversion and surface-enhanced Raman detection of heavy metal ions and organoheavy metal compounds. This method is simple, has a wide range of applications and strong scalability, and is suitable for large-scale preparation and rapid on-site detection.
[0019] (2) The preparation method of the present invention utilizes the characteristic that the solubility of elemental sulfur in organic solvents decreases with decreasing temperature. By cooling, elemental sulfur preferentially nucleates and deposits on the surface of noble metals to form a stable ultrathin sulfur active layer. It is suitable for noble metal nanoparticles (preferably 60–70 nm and cleaned) and solid SERS substrates, and can be extended to general noble metal SERS substrate systems.
[0020] (3) The present invention also provides a method for detecting inorganic heavy metal ions and organic heavy metal compounds by using the above-mentioned elemental sulfur coated noble metal surface enhanced Raman material. The core of this method is to achieve "dissolution-supersaturation-heterogeneous deposition" by controlling the solution temperature to ensure uniform coating of sulfur layer; preparing a clear elemental sulfur solution first and then cooling and depositing can reduce the precipitation of bulk free sulfur particles and improve the uniformity of coating.
[0021] (4) The method of this invention can be used for sulfur coating of dispersed noble metal nanoparticles as well as sulfur coating of solid SERS substrates, making it widely applicable. It is preferably applied to 60–70 nm cleaned and purified gold nanoparticles to form a sulfur-coated gold nanoparticle system that is easy to drop-coat, disperse, composite, or assemble. After coating, sulfur-related peaks appear in the low wavenumber region of the solid substrate, which can serve as spectroscopic evidence of successful sulfur active layer construction. The resulting sulfur active layer can serve as a heavy metal enrichment and transformation interface for SERS detection of inorganic heavy metal ions and organic heavy metal compounds. The process is mild, the equipment is simple, and it has good potential for batch preparation and on-site detection applications. Attached Figure Description
[0022] Figure 1 This is a schematic diagram illustrating the principle of temperature difference solubility-driven sulfur active layer deposition in this invention.
[0023] Figure 2 This is a transmission electron microscope image of Embodiment 1 of the present invention.
[0024] Figure 3-5 This is a schematic diagram of the characterization of the surface-enhanced Raman material in Embodiment 2 of the present invention, wherein... Figure 5 The image on the right is a magnified version of the image on the left.
[0025] Figure 6 This is a schematic diagram comparing the low wavenumber Raman spectra before and after coating with a solid surface-enhanced Raman substrate in Embodiment 2 of the present invention.
[0026] Figure 7 These are schematic diagrams of two morphologies of the solid noble metal SERS substrate of the present invention.
[0027] Figure 8 This is a schematic diagram illustrating the application principle of the elemental sulfur-coated noble metal surface-enhanced Raman material of this invention for heavy metal detection.
[0028] Figure 9 This is a qualitative analysis diagram of Example 3. Detailed Implementation
[0029] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.
[0030] Example 1
[0031] Preparation method of sulfur-coated gold nanoparticles (AuNPs@S) (main line: 70 nm, cleaned thoroughly)
[0032] S1, Gold Nanoparticles (AuNPs): Cleaning and Solvent Replacement: The colloidal solution of gold nanoparticles was transferred to a centrifuge tube and centrifuged at 10,000 rpm for 5 min. The supernatant was discarded. Ethanol was added for resuspension and the mixture was gently ultrasonically dispersed. The centrifugation and resuspension were repeated twice to remove free ligands, salts or impurities, resulting in a clean AuNPs ethanol dispersion system. The preferred AuNPs particle size was 70 nm.
[0033] S2. Preparation of a clear sulfur-saturated ethanol solution: Add excess elemental sulfur to ethanol and stir at 50°C for 30 min in a water bath until it reaches saturation or near saturation; then filter or centrifuge to remove undissolved sulfur particles to obtain a clear elemental sulfur solution.
[0034] S3, Temperature-driven deposition of sulfur active layer: The AuNPs ethanol dispersion system obtained in step S1 was mixed with the clarified sulfur solution obtained in step S2, and pre-contaminated at 50°C for 60 min; then, while maintaining contact, the system was cooled to 25°C. As the temperature decreased, the solubility of elemental sulfur in ethanol decreased, the solution became supersaturated, and elemental sulfur preferentially deposited heterogeneously on the surface of gold nanoparticles to form an elemental sulfur active layer.
[0035] S4. Remove free sulfur and obtain AuNPs@S: Centrifuge the reaction system, discard the supernatant, resuspend in ethanol and wash twice to remove bulk free sulfur particles, and finally disperse in water to obtain the AuNPs@S dispersion system.
[0036] like Figure 2 As shown, the obtained AuNPs@S particles are nearly spherical in shape, and the particle size and original outline are basically maintained. A thin coating structure can be observed on the outer edge of the particles, indicating that a sulfur active layer can be constructed on the surface of gold nanoparticles through temperature difference driven deposition.
[0037] Example 2
[0038] Preparation method of sulfur-coated solid noble metal SERS substrate (Au@S) (General line: general SERS substrates can be coated)
[0039] S1. Pretreatment of solid noble metal SERS substrate: A solid noble metal SERS substrate is provided, comprising a supporting substrate (silicon wafer) and a surface noble metal nanostructure layer (Au nanocones). The supporting substrate is sequentially rinsed with ethanol and dried with nitrogen; if necessary, low-power plasma or ultraviolet ozone cleaning can be performed to remove organic contaminants.
[0040] S2. Preparation of a clear sulfur-saturated ethanol solution: Same as step S2 in Example 1.
[0041] S3, Immersion Contact and Temperature Difference Deposition: The solid substrate was immersed in a clear sulfur solution at 50°C for 5 min; then, while maintaining the immersion state, the system was cooled to 25°C to induce sulfur deposition on the surface of the noble metal to form a sulfur active layer.
[0042] S4. Rinsing and drying: Remove the support substrate and rinse it twice with ethanol to remove any loosely attached sulfur particles; dry it with nitrogen or vacuum at room temperature to obtain a sulfur-coated solid SERS substrate (Au@S).
[0043] Technical effects: Performance testing was performed after coating the solid substrate, and the results are as follows: Figure 3-6 As shown, Figure 6In the middle, obvious sulfur-related characteristic peaks appear in the low wavenumber region, indicating that the sulfur active layer has been successfully constructed.
[0044] The morphology and spectroscopic characterization of the sulfur-coated solid SERS substrate were performed, and the results are as follows: Figure 3-6 As shown.
[0045] like Figure 3 As shown, the noble metal nanostructures coated with sulfur exhibit a relatively uniform and dense array distribution on the substrate surface, and the original nanoarray morphology is preserved.
[0046] like Figure 4 As shown, the substrate cross-section consists of a silicon wafer, a SiO2 nanosphere array, and an S-Au array above it. The interfaces of each structural layer are clear after the coating treatment, indicating that the temperature difference deposition process did not significantly damage the original substrate structure.
[0047] like Figure 5 As shown, the transmission electron microscope image reveals an S-Au composite layer formed on the outer side of the SiO2 microspheres; a magnified view of the area shows a sulfur layer approximately 3 nm thick on the outer side, indicating that the sulfur active layer is formed on the surface of the noble metal.
[0048] like Figure 6 As shown, compared with the uncoated sulfur substrate, the sulfur-coated substrate exhibits obvious sulfur-related Raman characteristic peaks in the low wavenumber region, indicating that the sulfur active layer has been successfully constructed and can provide a detectable low wavenumber spectral response.
[0049] Comparative Example 1
[0050] Wrapping without cooling steps
[0051] The process was completed directly after contacting AuNP or a solid substrate with a sulfur solution at 50°C, without cooling from 50°C to 25°C. The results showed that sulfur layer deposition was indistinct or unstable, and the low-wavenumber sulfur-related peaks were significantly weakened, indicating that temperature-driven supersaturated deposition was the key step.
[0052] Comparative Example 2
[0053] No filtration / clarification treatment is performed on the sulfur solution.
[0054] Direct coating with a sulfur solution containing undissolved sulfur particles can easily lead to co-deposition and contamination of bulk sulfur particles, resulting in uneven coverage and hot spot shading. This indicates that the combination of "clarified sulfur solution + temperature difference deposition" plays an important role in obtaining a uniform sulfur layer.
[0055] Example 3
[0056] Heavy metal ion detection
[0057] like Figure 7 As shown, AuNP@S or Au@S / M@S is mixed with Hg²+ Pb² + Cu² + Ag + Samples of As(III) / As(V) were incubated in contact (samples can be water or diluted serum / plasma / whole blood / urine), followed by low wavenumber SERS spectra; qualitative analysis was performed based on the peak position and / or peak intensity of characteristic peaks, such as... Figure 9 As shown, Figure 9 Characteristic peaks can be used to identify different heavy metals in a sample, enabling rapid detection and screening of heavy metal ions.
[0058] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for preparing surface-enhanced Raman materials based on temperature difference solubility, characterized in that, The specific steps are as follows: S1. Under the first temperature T1, elemental sulfur is added to an organic solvent to dissolve the elemental sulfur and obtain a saturated elemental sulfur solution. S2. Remove undissolved sulfur particles from the elemental sulfur solution to obtain a clear elemental sulfur solution; S3. Immerse the precious metal material to be coated in the clear elemental sulfur solution obtained in step S2; S4. While keeping the precious metal material to be coated in contact with the clear elemental sulfur solution obtained in step S2, the system is cooled from the first temperature T1 to the second temperature T2, so that the elemental sulfur becomes supersaturated due to the decrease in solubility, and an elemental sulfur active layer is formed by heterogeneous deposition on the surface of the precious metal material. S5. After post-processing, a surface-enhanced Raman material with elemental sulfur coated on noble metals is obtained.
2. The method for preparing a surface-enhanced Raman material based on temperature difference solubility as described in claim 1, characterized in that: The first temperature T1 is 30-90℃; the second temperature T2 is 0-35℃; and the temperature of the second temperature T2 is lower than the temperature of the first temperature T1.
3. The method for preparing a surface-enhanced Raman material based on temperature difference solubility as described in claim 1, characterized in that: One or more of the following solvents: alcohols, nitriles, esters, and ethers.
4. The method for preparing a surface-enhanced Raman material based on temperature difference solubility driven according to claim 1, characterized in that, When the noble metal material to be coated is a noble metal nanoparticle, the post-processing in step S5 is as follows: after centrifugation, discarding the supernatant, solvent resuspension and washing, the free sulfur particles are removed and then dispersed in water to obtain elemental sulfur coated noble metal surface-enhanced Raman material. Furthermore, the precious metal nanoparticles are cleaned and purified before being immersed in the clarified elemental sulfur solution in step S3.
5. The method for preparing a surface-enhanced Raman material based on temperature difference solubility driven according to claim 1, characterized in that, When the noble metal material to be coated is a solid noble metal SERS substrate, the post-processing in step S5 is as follows: first, remove the substrate from the solid noble metal SERS substrate, then rinse and dry the remaining material with an organic solvent to obtain elemental sulfur coated noble metal surface-enhanced Raman material.
6. The method for preparing a surface-enhanced Raman material based on temperature difference solubility as described in claim 1, characterized in that: In step S2, the method for removing undissolved sulfur particles is one of filtration, centrifugation, or settling and taking the supernatant. Repeat steps 1-10 of S3-S5; In step S4, the cooling method is natural cooling or programmed cooling; the cooling rate of the programmed cooling is 0.05-10 ℃ / min.
7. A surface-enhanced Raman material based on temperature difference solubility driven by the preparation method according to any one of claims 1-6, characterized in that: The material comprises a noble metal material and an elemental sulfur active layer deposited on the surface of the noble metal material; the noble metal material is a noble metal nanoparticle or a solid noble metal SERS substrate containing a noble metal nanostructure layer; the elemental sulfur active layer is formed by heterogeneous deposition of elemental sulfur solution on the surface of the noble metal material due to the decrease in solubility during the cooling process.
8. The surface-enhanced Raman material based on temperature difference solubility driven according to claim 7, characterized in that: The noble metal nanoparticles are one or more of gold nanoparticles, silver nanoparticles, and gold-silver alloy nanoparticles; the particle size of the gold nanoparticles is 5-200 nm. The solid noble metal SERS substrate includes a supporting substrate and a noble metal nanostructure layer located on the surface of the supporting substrate; The supporting substrate is one or more of silicon wafers, glass, quartz, ceramics, and polymer films; the noble metal nanostructure layer is one or more of gold, silver, and gold-silver alloys; the morphology of the noble metal nanostructure layer is one or more of nanoparticle assembly layers, nanoislands, nanopores, nanopillars, nanocones, nanoshells, and rough metal films. The thickness of the elemental sulfur active layer is 0.5-50 nm.
9. An application of the surface-enhanced Raman material based on temperature difference solubility driven as described in any one of claims 7-8, characterized in that: This material is used in the detection of heavy metals, including inorganic heavy metal ions and organic heavy metal compounds; the inorganic heavy metal ions are Hg. 2+ Pb 2+ Cd 2+ Cu 2+ Ag + As 3+ And As 5+ One or more of the following: the organic heavy metal compound is an organomercury compound, a heavy metal compound containing a metal-carbon bond, or a heavy metal compound containing a metal-organic group structure.
10. The application of the surface-enhanced Raman material based on temperature difference solubility driven according to claim 9, characterized in that, The specific steps are as follows: The sample to be tested is brought into contact with a surface-enhanced Raman spectroscopy (SERS) material; heavy metal ions in the sample are enriched, coordinated, or transformed on the surface of the elemental sulfur active layer, forming a metal-sulfur interaction structure or metal sulfides; samples are collected at depths of less than 500 cm. -1 Surface-enhanced Raman spectroscopy in the low wavenumber region; qualitative or quantitative analysis based on metal-sulfur vibrational peaks or characteristic peaks of metal sulfides; The detection method is surface-enhanced Raman spectroscopy in the low wavenumber region, where the low wavenumber region is less than 500 cm⁻¹. -1 The Raman shift region; a 785 nm laser was used as the excitation source during detection; The sample to be tested is one or more of the following: water sample, serum, plasma, whole blood, urine, food extract, and environmental sample extract.