A copper-carbon nanofiber filter nonwoven fabric and its preparation method
By blending carbon nanoparticles and copper salt precursors into polymer melt, forming them using melt-blowing, and carrying out in-situ carbothermic reduction reaction, the problems of easy loss of functional components and high wind resistance in non-woven filter materials are solved. This achieves efficient adsorption of VOCs and antibacterial and antiviral functions while simplifying the preparation process.
Patent Information
- Application Number
- CN202611487969.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-10
AI Technical Summary
Existing nonwoven filter materials have functional components that are prone to detachment, high filtration resistance, and difficulty in simultaneously achieving efficient adsorption of volatile organic compounds (VOCs) and antibacterial and antiviral functions.
Carbon nanoparticles and copper salt precursors are directly added to polypropylene/polyester polymer melt for blending. The mixture is then formed by melt-blowing and in-situ carbothermic reduction reaction is carried out under a high-temperature nitrogen atmosphere, causing nano-copper crystals to adhere to the surface of carbon nanoparticles, forming a copper-carbon nanocomposite structure. The functional components are embedded inside the fiber.
It avoids the problems of functional component shedding and pore blockage, maintains the permeability of the filter material, achieves efficient adsorption of VOCs and long-lasting antibacterial and antiviral functions, simplifies the preparation process and improves batch-to-batch consistency.
Smart Images

Figure CN123063941A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of filtration material technology, specifically relating to a copper-carbon nanofiber filter nonwoven fabric and its preparation method. Background Technology
[0002] Nonwoven filter materials are widely used in air purification, water treatment, personal protective equipment, and medical protective equipment due to their advantages such as three-dimensional mesh structure, high porosity, lightweight texture, and low cost. With the acceleration of industrialization and urbanization, pollutants in air and water are becoming increasingly complex, including not only particulate matter (PM) and dust, but also volatile organic compounds (VOCs) and microbial pollutants such as bacteria and viruses. This places higher demands on the comprehensive purification capabilities of filter materials. Polypropylene (PP) and polyester (PET) spunbond nonwoven fabrics, as common filter substrates, possess good mechanical properties and chemical stability, but they do not inherently possess the functions of adsorbing VOCs and sterilizing and antiviral agents. Therefore, functional modification is usually required to expand their application performance.
[0003] Currently, the mainstream technical routes for functional modification of nonwoven fabrics mainly include surface coating and impregnation loading. Surface coating involves mixing active substances such as activated carbon, silver ions, and copper ions with a binder and coating the nonwoven fabric surface. Impregnation involves immersing the nonwoven fabric in a dispersion containing functional particles, and then drying it to allow the particles to adhere to the fiber surface. For example, some existing technologies use activated carbon particles or carbon nanomaterials loaded onto the nonwoven fabric surface to utilize their large specific surface area to adsorb organic gases and odors; other technologies attach nano-silver or nano-copper to the fiber surface through impregnation, utilizing the antibacterial properties of metal ions to impart antibacterial functionality to the material. However, these existing routes have significant shortcomings. First, the active particles mainly adhere to the fiber surface, resulting in weak bonding with the matrix. They are easily detached during use or washing, leading to a significant decrease in filtration performance and service life, and also posing a risk of secondary pollution from the detached nanoparticles. Second, surface coating can clog some of the surface pores of the nonwoven fabric, significantly increasing filtration resistance and affecting air permeability and filtration flux. Third, single-function fillers can usually only solve one aspect of adsorption or antibacterial problems, and it is difficult to meet the comprehensive filtration needs of VOCs and microorganisms at the same time. If multi-layer composites are used, the process will become more complicated and the cost will increase.
[0004] Therefore, developing a nonwoven filter material that can maintain the permeability of the nonwoven matrix pores, achieve efficient adsorption of VOCs and long-lasting antibacterial and antiviral functions, and whose functional components are not easily detached and can be reused has important practical application value. Summary of the Invention
[0005] This invention aims to overcome the shortcomings of the prior art and provide a copper-carbon nanofiber filter nonwoven fabric and its preparation method, solving the technical problems of easy loss of functional components, high filtration resistance, and difficulty in simultaneously achieving VOCs adsorption and antibacterial and antiviral functions in existing nonwoven filter materials.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for preparing a copper-carbon nanofiber filter nonwoven fabric includes the following steps: Step 1: Mix polypropylene chips and polyester chips, melt them, and obtain a polymer melt; Step 2: Mix carbon nanoparticles and copper salt precursor, add to the polymer melt, stir and blend to obtain a blended spinning melt; Step 3: The blended spinning melt is extruded through a meltblown die, and nitrogen hot gas is injected into both sides of the die to stretch and draw the extruded melt stream to form continuous fibers. The continuous fibers are then collected. Step 4: The continuous fibers are collected on the web forming device, and the fibers overlap and stack together to form a nonwoven fabric precursor. Step 5: The nonwoven fabric precursor is hot-pressed and shaped using hot rollers, and then cooled to obtain the copper-carbon nanofiber filter nonwoven fabric.
[0007] Preferably, in step one, the melting temperature is 240-260℃; the mass ratio of the polypropylene chips to the polyester chips is 1:(0.3-0.8); the polypropylene chips are isotactic polypropylene with a melt index of 20-40 g / 10 min at 230℃ and 2.16 kg load; and the polyester chips are polyethylene terephthalate with an intrinsic viscosity of 0.65-0.85 dL / g.
[0008] Preferably, in step one, after the polypropylene chips and polyester chips are mixed, they also need to be dried.
[0009] Preferably, in step two, the mass ratio of the carbon nanoparticles to the copper salt precursor is 1:(0.2-0.6), the particle size of the carbon nanoparticles is 20-200 nm, and the carbon nanoparticles are selected from at least one of carbon nanotubes, graphene nanosheets, or conductive carbon black; the copper salt precursor is selected from at least one of copper nitrate trihydrate, copper acetate monohydrate, copper sulfate pentahydrate, or copper chloride dihydrate.
[0010] Preferably, in step two, the stirring and mixing conditions are: stirring and mixing at a temperature of 240-260℃ and a rotation speed of 200-600 r / min for 15-45 min.
[0011] Preferably, in step three, the blended spinning melt is metered by a gear pump and then delivered to the inlet of the meltblown die before entering the meltblown die, with a delivery pressure of 1-3 MPa. The temperature of the meltblown die head is 250-270℃.
[0012] Preferably, in step three, the meltblown die head is provided with a spinneret orifice, the orifice diameter is 0.2-0.5mm, and the length-to-diameter ratio of the spinneret orifice is (4-10):1; the nitrogen hot gas flow is ejected through slit-type air knives located on both sides of the die head, the slit width is 0.5-1.5mm, and the angle between the direction of the nitrogen hot gas flow and the extrusion direction of the die head is 30-60°.
[0013] Preferably, in step three, the temperature of the nitrogen hot gas flow is 260-280℃ and the pressure is 0.3-0.5MPa; the draw ratio of the nitrogen hot gas flow to the extruded melt is 5-20 times; and the average diameter of the continuous fiber is 1-10μm.
[0014] Preferably, in step four, the web-forming device is a mobile mesh belt, and the moving speed of the mesh belt is 1-10 m / min; the receiving distance between the spinneret of the meltblown die and the mobile mesh belt is 10-40 cm; and the unit area mass of the nonwoven fabric precursor is 50-200 g / m³. 2 .
[0015] Preferably, in step five, the hot rolling rolls are a pair of opposing heating rolls, the hot rolling temperature is 130-150℃, the linear pressure is 30-50N / mm, and the hot pressing and setting time is 0.5-3s; the cooling is natural air cooling or wind cooling.
[0016] The present invention also discloses a copper-carbon nanofiber filter nonwoven fabric, which is prepared by the preparation method described above.
[0017] Compared with the prior art, the beneficial effects of the present invention are as follows: In this invention, carbon nanoparticles and copper salt precursors are directly added to the polypropylene / polyester polymer melt for blending, and then extruded through a meltblown die. This ensures that the carbon nanoparticles and copper salt precursors are uniformly dispersed within the polymer matrix before fiber formation. Compared to existing technologies that coat or impregnate the active material onto the fiber surface, in this invention, the substances corresponding to the carbon nanoparticles and copper salt precursors are embedded inside the fiber, rather than adhering to the outer surface. This avoids the problem of the active material detaching from the fiber surface during use or washing, and eliminates the risk of secondary pollution caused by detached nanoparticles. Furthermore, since the active material is located inside the fiber rather than filling the surface pores, the internal interconnected pore structure of the nonwoven fabric matrix is maintained, avoiding the problems of surface pore blockage and increased filtration resistance caused by surface coating processes. This invention employs a melt-blown method to directly form fibers from blended spinning melt. Under the high-temperature nitrogen atmosphere of the melt-blown step, the copper salt precursor first decomposes at the die temperature to generate copper oxide. Subsequently, the copper oxide undergoes an in-situ carbothermal reduction reaction with carbon nanoparticles to generate copper nanocrystals, which adhere to the surface of the carbon nanoparticles, forming a copper-carbon nanocomposite structure inside the fiber. The high-temperature environment and nitrogen atmosphere required for this carbothermal reduction reaction are provided by the melt-blown process itself, without the need for additional reducing agents or separate reduction treatment steps. The copper nanocrystals are anchored to the surface of the carbon nanoparticles through a chemical reaction, resulting in a stronger binding force than physical mixing or adsorption methods. The carbon nanoparticles act as the carrier sites for the copper nanocrystals, allowing them to be dispersed rather than aggregated within the fiber, thereby obtaining a larger effective copper element exposure area per unit volume. This invention directly melt-blown the carbon nanoparticles and copper salt precursor into a polymer melt in a one-step process, eliminating the post-processing steps of preparing a nonwoven fabric matrix and then loading functional particles in the prior art, thus simplifying the preparation process. At the same time, the carbothermic reduction reaction is completed in situ during the fiber forming process, without the need for additional reaction equipment or process sections, resulting in good process continuity and suitability for industrial continuous production. The uniformity of the distribution of carbon nanoparticles and copper salt precursors in the polymer melt is controlled by the blending process parameters, resulting in good batch-to-batch consistency. Attached Figure Description
[0018] Figure 1 The graph shows the results of the antibacterial performance test of the nonwoven fabric samples prepared in Examples 1-3 and Comparative Examples 1-4 of this invention. Figure 2 The graph shows the filtration performance test results of the nonwoven fabric samples prepared in Examples 1-3 and Comparative Examples 1-4 of this invention. Detailed Implementation
[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention. Example 1
[0020] This embodiment discloses a method for preparing copper-carbon nanofiber filter nonwoven fabric, including the following steps: Step 1: Mix isotactic polypropylene chips (melt index of 20g / 10min at 230℃ and 2.16kg load) and polyethylene terephthalate chips (intrinsic viscosity of 0.65dL / g) at a mass ratio of 1:0.3, dry them, and then feed them into a twin-screw extruder to melt them at 240℃ to obtain the polymer melt. Step 2: Mix conductive carbon black with a particle size of 200 nm and copper nitrate trihydrate at a mass ratio of 1:0.2, add it to the polymer melt, and stir and blend at 200 r / min for 45 min at 240°C to obtain the blended spinning melt. Step 3: The blended spinning melt is metered by a gear pump and delivered to the inlet of the meltblown die at a pressure of 1 MPa. It is then extruded through the meltblown die at a temperature of 250°C. The meltblown die is equipped with spinnerets with a diameter of 0.2 mm and an aspect ratio of 4:1. Simultaneously, nitrogen hot air is injected into both sides of the die. The nitrogen hot air is ejected through slit-type air knives located on both sides of the die. The slit width is 0.5 mm, and the angle between the direction of the nitrogen hot air and the extrusion direction of the die is 30°. The temperature of the nitrogen hot air is 260°C, and the pressure is 0.3 MPa. The extruded melt stream is stretched and drawn at a ratio of 5 times to form continuous fibers with an average diameter of 10 μm. The continuous fibers are then collected. Step 4: Collect the continuous fibers onto a moving mesh belt at a speed of 1 m / min. The receiving distance between the spinneret of the meltblown die and the moving mesh belt is 10 cm. The fibers overlap and stack to form a nonwoven fabric precursor with a unit area mass of 50 g / m³. 2 ; Step 5: The nonwoven fabric precursor is hot-pressed and shaped by a pair of opposing heating rollers. The hot pressing temperature is 130℃, the linear pressure is 30N / mm, and the hot pressing and shaping time is 3s. After natural air cooling to room temperature, copper-carbon nanofiber filter nonwoven fabric is obtained. Example 2
[0021] This embodiment discloses a method for preparing copper-carbon nanofiber filter nonwoven fabric, including the following steps: Step 1: Mix isotactic polypropylene chips (melt index of 40g / 10min at 230℃ and 2.16kg load) and polyethylene terephthalate chips (intrinsic viscosity of 0.85dL / g) at a mass ratio of 1:0.8, dry them, and then feed them into a twin-screw extruder to melt them at 260℃ to obtain a polymer melt. Step 2: Mix carbon nanotubes with a particle size of 20 nm and copper acetate monohydrate at a mass ratio of 1:0.6, add them to the polymer melt, and stir and blend at 260°C and 600 r / min for 15 min to obtain the blended spinning melt. Step 3: The blended spinning melt is metered by a gear pump and delivered to the inlet of the meltblown die at a pressure of 3 MPa. It is then extruded through the meltblown die at a temperature of 270°C. The meltblown die is equipped with spinnerets with a diameter of 0.5 mm and an aspect ratio of 10:1. Simultaneously, nitrogen hot air is injected into both sides of the die. The nitrogen hot air is ejected through slit-type air knives located on both sides of the die. The slit width is 1.5 mm, and the angle between the direction of the nitrogen hot air and the extrusion direction of the die is 60°. The temperature of the nitrogen hot air is 280°C, and the pressure is 0.5 MPa. The extruded melt stream is stretched and drawn at a draw ratio of 20 times to form continuous fibers with an average diameter of 1 μm. The continuous fibers are then collected. Step 4: Collect the continuous fibers onto a moving mesh belt at a speed of 10 m / min. The receiving distance between the spinneret of the meltblown die and the moving mesh belt is 40 cm. The fibers overlap and stack to form a nonwoven fabric precursor with a unit area mass of 200 g / m³. 2 ; Step 5: The nonwoven fabric precursor is hot-pressed and shaped by a pair of opposing heating rollers. The hot pressing temperature is 150℃, the linear pressure is 50N / mm, and the hot pressing and shaped time is 0.5s. After being cooled to room temperature by air cooling, copper-carbon nanofiber filter nonwoven fabric is obtained. Example 3
[0022] This embodiment discloses a method for preparing copper-carbon nanofiber filter nonwoven fabric, including the following steps: Step 1: Mix isotactic polypropylene chips (melt index of 30 g / 10 min at 230℃ and 2.16 kg load) and polyethylene terephthalate chips (intrinsic viscosity of 0.75 dL / g) at a mass ratio of 1:0.55, dry them, and then feed them into a twin-screw extruder to melt them at 250℃ to obtain a polymer melt. Step 2: Graphene nanosheets with a particle size of 110 nm and copper sulfate pentahydrate are mixed at a mass ratio of 1:0.4 and added to the polymer melt. The mixture is stirred and blended at 400 r / min for 30 min at 250 °C to obtain a blended spinning melt. Step 3: The blended spinning melt is metered by a gear pump and delivered to the inlet of the meltblown die at a pressure of 2 MPa. It is then extruded through the meltblown die at a temperature of 260°C. The meltblown die is equipped with spinnerets with a diameter of 0.35 mm and an aspect ratio of 7:1. Simultaneously, nitrogen hot air is injected into both sides of the die. The nitrogen hot air is ejected through slit-type air knives located on both sides of the die. The slit width is 1.0 mm, and the angle between the direction of the nitrogen hot air and the extrusion direction of the die is 45°. The temperature of the nitrogen hot air is 270°C, and the pressure is 0.4 MPa. The extruded melt stream is stretched and drawn at a draw ratio of 12.5 times to form continuous fibers with an average diameter of 5.5 μm. The continuous fibers are then collected. Step 4: Collect the continuous fibers onto a moving mesh belt at a speed of 5.5 m / min. The receiving distance between the spinneret of the meltblown die and the moving mesh belt is 25 cm. The fibers overlap and stack to form a nonwoven fabric precursor with a unit area mass of 125 g / m³. 2 ; Step 5: The nonwoven fabric precursor is hot-pressed and shaped by a pair of opposing heating rollers. The hot pressing temperature is 140℃, the linear pressure is 40N / mm, and the hot pressing and shaped time is 1.75s. After natural air cooling to room temperature, copper-carbon nanofiber filter nonwoven fabric is obtained.
[0023] Comparative Example 1 This comparative example discloses a method for preparing carbon nanoparticle-modified meltblown nonwoven fabric. The only difference from Example 1 is that no copper salt precursor (copper nitrate trihydrate) is added. All other steps and parameters are exactly the same as in Example 1.
[0024] Comparative Example 2 This comparative example discloses a method for preparing copper nanoparticle-modified meltblown nonwoven fabric. The only difference from Example 1 is that carbon nanoparticles (conductive carbon black) are not added. All other steps and parameters are exactly the same as in Example 1.
[0025] Comparative Example 3 This comparative example discloses a method for preparing copper-carbon nanofiber filter nonwoven fabric. The only difference from Example 1 is that air hot air flow is used instead of nitrogen hot air flow. All other steps and parameters are exactly the same as in Example 1.
[0026] Comparative Example 4 This comparative example discloses a method for preparing copper-carbon nanofiber filter nonwoven fabric, including the following steps: Step 1: Mix isotactic polypropylene chips (melt index of 20g / 10min at 230℃ and 2.16kg load) and polyethylene terephthalate chips (intrinsic viscosity of 0.65dL / g) at a mass ratio of 1:0.3, dry them, and then feed them into a twin-screw extruder to melt them at 240℃ to obtain the polymer melt. Step 2: The polymer melt is metered by a gear pump and delivered to the inlet of the meltblown die head at a pressure of 1 MPa. It is then extruded through the meltblown die head at a temperature of 250°C. The meltblown die head is equipped with spinnerets with a diameter of 0.2 mm and an aspect ratio of 4:1. Simultaneously, nitrogen hot air is injected into both sides of the die head. The nitrogen hot air is ejected through slit-type air knives located on both sides of the die head. The slit width is 0.5 mm, and the angle between the direction of the nitrogen hot air and the extrusion direction of the die head is 30°. The temperature of the nitrogen hot air is 260°C, and the pressure is 0.3 MPa. The extruded melt stream is stretched and drawn at a stretch ratio of 5 times to form continuous fibers with an average diameter of 10 μm. The continuous fibers are then collected. Step 3: The continuous fibers are collected on a moving mesh belt at a speed of 1 m / min. The receiving distance between the spinneret of the meltblown die and the moving mesh belt is 10 cm. The fibers overlap and stack to form a nonwoven fabric precursor with a unit area mass of 50 g / m³. 2 ; Step 4: The nonwoven fabric precursor is hot-pressed and shaped by a pair of opposing heating rollers. The hot pressing temperature is 130℃, the linear pressure is 30N / mm, and the hot pressing and shaping time is 3s. After natural air cooling to room temperature, the nonwoven fabric matrix is obtained. Step 5: Mix conductive carbon black with a particle size of 200nm and copper nitrate trihydrate at a mass ratio of 1:0.2. The amount of deionized water is 10 times the total mass of conductive carbon black and copper nitrate trihydrate. Add polyacrylate adhesive (AE-35 rigid nonwoven fabric special emulsion adhesive, solid content of 45±1%, Tg=50℃). The amount of adhesive is 5% of the total mass of conductive carbon black and copper nitrate trihydrate. Stir and disperse evenly to prepare a functional particle dispersion. The nonwoven fabric matrix was immersed in the functional particle dispersion for 30 minutes and then removed. The excess liquid was removed by squeezing with rollers and then dried at 100°C to obtain a nonwoven fabric loaded with carbon nanoparticles and copper salt precursors. The nonwoven fabric obtained in step three is placed in a nitrogen atmosphere furnace and heated at 260°C for 5 seconds to decompose the copper salt precursor and generate nano-copper crystals, thus obtaining copper-carbon nanofiber filter nonwoven fabric.
[0027] Test case The nonwoven fabric samples prepared in Examples 1-3 and Comparative Examples 1-4 were placed under the same environmental conditions (temperature 25±2℃, relative humidity 50±5%) for 24 hours and then the performance was tested. Ten samples were taken from each group of samples, and the test results were taken as the arithmetic mean. (1) Antibacterial performance: Referring to standard GB / T20944.3-2008, the antibacterial rate of non-woven fabric samples against Staphylococcus aureus was determined by shaking flask method (each non-woven fabric sample was shaken and contacted with bacterial solution for 24h, and the number of viable colonies before and after contact was measured, and the antibacterial rate was calculated: initial antibacterial rate = (initial number of viable bacteria - number of viable bacteria after contact) / initial number of viable bacteria × 100%), antibacterial rate after 20 washes (the samples were washed 20 times (each time soaked in deionized water and shaken for 10min, and the deionized water was changed and repeated 20 times) and air-dried naturally, and the antibacterial efficiency retention rate was measured under the same conditions) and antibacterial efficiency retention rate (antibacterial efficiency retention rate = antibacterial rate after 20 washes / initial antibacterial rate × 100%). (2) Filtration performance: Referring to standard GB / T14295-2019, the filter material comprehensive performance test bench was used to measure the filtration resistance (the pressure difference between the two sides of the sample was measured under an air volume of 32L / min), initial filtration efficiency (the filtration efficiency for 0.3μm NaCl aerosol particles was measured under an air volume of 32L / min), filtration efficiency after 20 water washes (the sample was washed 20 times (each time soaked in deionized water and shaken for 10min, and the deionized water was replaced and repeated 20 times) and air-dried naturally, and the filtration efficiency retention rate was measured under the same conditions) and filtration efficiency retention rate (filtration efficiency retention rate = filtration efficiency after 20 water washes / initial filtration efficiency × 100%). The performance test results are shown in Table 1: Table 1
[0028] As shown in Table 1, the nonwoven fabric prepared by this invention has excellent antibacterial and filtration properties, and its performance retention rate is high after 20 washes. Compared with Example 1, the initial antibacterial rate of Comparative Example 1 was significantly lower than that of all copper-containing examples, indicating that the main antibacterial function of the nonwoven fabric of the present invention comes from the nano-copper crystals. The initial antibacterial rate of 15.0% can be attributed to the physical interception and adsorption of bacteria by the nonwoven fabric matrix, but its antibacterial level is far lower than the chemical bactericidal effect of the nano-copper crystals, verifying that copper is the core component for achieving efficient antibacterial function. The initial filtration efficiency of Comparative Example 2 was far lower than that of Example 1, indicating that carbon nanoparticles are the core component for providing physical interception and fiber surface roughening. Although its initial antibacterial rate was close to that of Example 1, due to the lack of carbon nanoparticles, the nano-copper crystals generated by the decomposition of copper salt precursor lacked carrying sites inside the fiber and were prone to agglomeration, resulting in a reduction in the effective exposure area of copper. At the same time, its filtration efficiency retention rate after 20 washes was also lower than that of the Example group, further illustrating the necessity of carbon nanoparticles for maintaining the dispersion state of functional components and filtration performance. The initial antibacterial rate, antibacterial rate after 20 washes, and antibacterial efficiency retention rate of Comparative Example 3 were all lower than those of Example 1. The initial filtration efficiency, filtration efficiency after 20 washes, and filtration efficiency retention rate were all significantly lower than those of Example 1, indicating that the decomposition products of the copper salt precursor under air atmosphere were mainly copper oxide, the carbothermic reduction reaction was insufficient, the binding force between the nano-copper crystals and carbon nanoparticles was weak, some functional components were lost during the washing process, and both antibacterial and filtration performance deteriorated, verifying the necessity of nitrogen atmosphere for achieving in-situ carbothermic reduction reaction. Comparative Example 4 had the highest filtration resistance, and the initial filtration efficiency, filtration efficiency after 20 washes, filtration efficiency retention rate, initial antibacterial rate, antibacterial rate after 20 washes, and antibacterial efficiency retention rate all decreased significantly, indicating that the surface coating / impregnation loading method not only blocked the pores of the nonwoven fabric surface, leading to a significant increase in air resistance, but also that the functional components only adhered to the fiber surface and were largely detached during the washing process, resulting in serious deterioration of both antibacterial and filtration performance, verifying the superiority of the technical solution of "directly blending the functional components with the polymer melt and then melt-blowing to embed the functional components inside the fiber" in this invention compared with the existing post-treatment loading route.
[0029] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a copper-carbon nanofiber filter nonwoven fabric, characterized in that, Includes the following steps: Step 1: Mix polypropylene chips and polyester chips, melt them, and obtain a polymer melt; Step 2: Mix carbon nanoparticles and copper salt precursor, add to the polymer melt, stir and blend to obtain a blended spinning melt; Step 3: The blended spinning melt is extruded through a meltblown die, and nitrogen hot gas is injected into both sides of the die to stretch and draw the extruded melt stream to form continuous fibers. The continuous fibers are then collected. Step 4: The continuous fibers are collected on the web forming device, and the fibers overlap and stack together to form a nonwoven fabric precursor. Step 5: The nonwoven fabric precursor is hot-pressed and shaped using hot rollers, and then cooled to obtain the copper-carbon nanofiber filter nonwoven fabric.
2. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step one, the melting temperature is 240-260℃; the mass ratio of the polypropylene chips to the polyester chips is 1:(0.3-0.8); the polypropylene chips are isotactic polypropylene with a melt index of 20-40 g / 10 min at 230℃ and 2.16 kg load; the polyester chips are polyethylene terephthalate with an intrinsic viscosity of 0.65-0.85 dL / g.
3. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step two, the mass ratio of the carbon nanoparticles to the copper salt precursor is 1:(0.2-0.6), the particle size of the carbon nanoparticles is 20-200 nm, and the carbon nanoparticles are selected from at least one of carbon nanotubes, graphene nanosheets, or conductive carbon black; the copper salt precursor is selected from at least one of copper nitrate trihydrate, copper acetate monohydrate, copper sulfate pentahydrate, or copper chloride dihydrate.
4. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step two, the stirring and mixing conditions are: stirring and mixing at a temperature of 240-260℃ and a speed of 200-600r / min for 15-45min.
5. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step three, the blended spinning melt is metered by a gear pump and then delivered to the inlet of the meltblown die before entering the meltblown die, with a delivery pressure of 1-3 MPa. The temperature of the meltblown die head is 250-270℃.
6. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step three, the meltblown die head is provided with a spinneret orifice with a diameter of 0.2-0.5 mm and a length-to-diameter ratio of (4-10):1; the nitrogen hot gas flow is ejected through slit-type air knives located on both sides of the die head, the width of the slit is 0.5-1.5 mm, and the angle between the direction of the nitrogen hot gas flow and the extrusion direction of the die head is 30-60°.
7. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step three, the temperature of the nitrogen hot gas flow is 260-280℃ and the pressure is 0.3-0.5MPa; the draw ratio of the nitrogen hot gas flow to the extruded melt is 5-20 times; and the average diameter of the continuous fiber is 1-10μm.
8. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step four, the web-forming device is a mobile mesh belt, and the moving speed of the mesh belt is 1-10 m / min; the receiving distance between the spinneret of the meltblown die head and the mobile mesh belt is 10-40 cm; the unit area mass of the nonwoven fabric precursor is 50-200 g / m³. 2 .
9. The method for preparing a copper-carbon nanofiber filter nonwoven fabric according to claim 1, characterized in that, In step five, the hot rolling rolls are a pair of opposing heating rolls, the hot rolling temperature is 130-150℃, the linear pressure is 30-50N / mm, the hot pressing and setting time is 0.5-3s, and the cooling is natural air cooling or wind cooling.
10. A copper-carbon nanofiber filter nonwoven fabric, characterized in that, The copper-carbon nanofiber filter nonwoven fabric is prepared by the preparation method described in any one of claims 1-9.