Modified fibrous material, method for its production and use thereof

By modifying the fiber material, its hydrophilic, oleophobic, and antifouling properties are improved, solving the problem of insufficient oleophobic properties of the fiber material in oil-water separation applications and achieving better oil-water separation results.

CN123064010APending Publication Date: 2026-11-10CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510583865.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-07
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The application of existing fiber materials in oil-water separation is limited, especially due to insufficient oleophobic properties, resulting in poor separation performance.

Method used

By mixing monomeric compounds with specific structural formulas, alcohols, polyenols, and initiators with water solvents to form a modified solution, and then subjecting it to contact treatment with fiber materials, including immersion and light or heat treatment, the hydrophilic and oleophobic properties and antifouling properties of the fiber materials are improved.

Benefits of technology

The prepared modified fiber material exhibits excellent oleophobic properties underwater and oil-bearing capacity under wetting conditions, significantly improving the oil-water separation effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064010A_ABST
    Figure CN123064010A_ABST
Patent Text Reader

Abstract

The application relates to the technical field of fiber materials, in particular to a modified fiber material and a preparation method and application thereof. The method comprises the following steps: (1) mixing a monomer compound with a structure shown in formula (I), alcohol, polyalkylene glycol, an initiator and optionally an aqueous solvent to obtain a modified solution; (2) performing contact treatment on fibers and the modified solution; wherein R1 and R2 are each independently hydrogen, C1-C8 alkyl; and R3 is amino, hydroxyl, substituted or unsubstituted alkoxy. The method can improve the hydrophilic and oleophobic properties and the antifouling property of the fiber material, and meanwhile, the method is simple in process, mild in conditions, low in cost and suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fiber materials technology, specifically to a modified fiber material, its preparation method, and its application. Background Technology

[0002] Nylon, the world's first synthetic fiber, is composed of polyamide, a general term for thermoplastic resins containing repeating amide groups —[NHCO]— in their molecular backbone. Nylon possesses excellent comprehensive properties, including good tensile strength, heat resistance, and abrasion resistance, and is widely used in various fields such as automobiles, home appliances, machinery, and the medical industry. Furthermore, with continuous development of industrial technology, the downstream market is gradually expanding, offering broad development prospects. However, when used as filter cloth, nylon's amphiphilic nature limits its application to conventional solid-liquid separation processes, restricting its deeper applications. Improving nylon's oleophobic properties could expand its applications in oil-water separation, thereby increasing its application value. Currently, the main modification methods for nylon include copolymerization modification, filler modification, blending modification, and direct addition of additives, aiming to improve its flame retardant properties. Modification methods for improving oleophobic properties are extremely rare.

[0003] Polyester is a synthetic fiber made from organic diacids and diols through chemical polycondensation; it belongs to the category of polymer compounds. Polyester has many advantages. First, it has excellent wrinkle resistance and shape retention, making garments less prone to wrinkling and maintaining their original shape during wear. Second, polyester fibers have high strength and elastic recovery, making woven fabrics durable and able to quickly return to their original shape. Furthermore, polyester fibers are abrasion-resistant and lint-free, resulting in cleaner-looking fabrics. However, polyester also has disadvantages such as low moisture content, poor breathability, poor dyeability, a tendency to pill and fuzz, and easy staining. Summary of the Invention

[0004] The purpose of this invention is to overcome the problem that existing fiber materials cannot achieve oil-water separation or have poor separation effect, and to provide a modified fiber material, its preparation method and application. The method has the characteristics of simple process, mild conditions and low cost. The modified fiber material prepared by this method has good hydrophilic and oleophobic properties and strong antifouling properties.

[0005] To achieve the above objectives, the first aspect of the present invention provides a method for preparing a modified fiber material, the method comprising: (1) mixing a monomer compound having the structural formula shown in formula (I), an alcohol, a polyenol, an initiator and optionally an aqueous solvent to obtain a modified solution; and (2) subjecting the fiber to a contact treatment with the modified solution. In this configuration, R1 and R2 are each independently hydrogen or C1-C8 alkyl groups; R3 is an amino group, a hydroxyl group, or a substituted or unsubstituted alkoxy group.

[0006] A second aspect of the present invention provides a modified fiber material prepared by the method described in the present invention.

[0007] A third aspect of the present invention provides an application of the modified fiber material described herein in oil-water separation.

[0008] Through the above technical solution, the present invention has the following advantages:

[0009] The method of this invention can improve the hydrophilic and oleophobic properties and antifouling properties of fiber materials. At the same time, the process is simple, the conditions are mild, and the cost is low, making it suitable for industrial applications.

[0010] The fiber material prepared by the method of this invention has excellent underwater oleophobic properties and superior oil-bearing capacity under wetting conditions. Attached Figure Description

[0011] Figure 1 This is a schematic diagram of the surface of the nylon filter cloth before modification according to the present invention;

[0012] Figure 2 This is a schematic diagram of the surface of the modified nylon filter cloth of the present invention. Detailed Implementation

[0013] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0014] The present invention provides a method for preparing a modified fiber material, the method comprising: (1) mixing a monomer compound having the structural formula shown in formula (I), an alcohol, a polyenol, an initiator and optionally an aqueous solvent to obtain a modified solution; (2) subjecting the fiber to contact treatment with the modified solution;

[0015]

[0016] Formula (I); wherein R1 and R2 are each independently hydrogen or C1-C8 alkyl; and R3 is amino, hydroxyl, substituted or unsubstituted alkoxy.

[0017] The method of this invention can improve the hydrophilic and oleophobic properties and antifouling properties of fiber materials. At the same time, the process is simple, the conditions are mild, and the cost is low, making it suitable for industrial applications.

[0018] According to a preferred embodiment of the present invention, the mass ratio of the alcohol to the polyenol is 0.2-10:1, for example, it can be 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1 and 9:1, preferably 1-5:1. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and stain-resistant properties of the fiber material can be further improved.

[0019] In this invention, the degree of polymerization of the polyenol can be selected from a wide range. Commonly used degrees of polymerization of polyenols in the art can be applied to this invention. The following is an illustrative description, but it does not limit the scope of this invention. For example, the degree of polymerization of the polyenol is 1500-2000.

[0020] In this invention, the range of types of polyenols is relatively wide, and various polyenols can be used in this invention, with the olefin being, for example, a C2-C4 olefin.

[0021] According to a preferred embodiment of the present invention, the polyol is selected from polyvinyl alcohol and / or polyacryl alcohol, preferably the polyol is a mixture of polyvinyl alcohol and polyacryl alcohol, wherein the mass ratio of polyvinyl alcohol to polyacryl alcohol in the mixture is 0.5-2:1, for example, 0.6:1, 0.8:1, 1:1, 1.2:1, 1.4:1, 1.6:1 and 1.8:1. The advantages of the present invention are illustrated by taking a 1:1 mass ratio of polyvinyl alcohol to polyacryl alcohol in the mixture as an example. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0022] In this invention, the type of alcohol can be a conventional choice in the art as long as the purpose of this invention can be achieved. The following is an illustrative description, but it does not limit the scope of this invention. According to a preferred embodiment of this invention, the alcohol is a C1-C5 alcohol, preferably selected from ethanol and / or isopropanol.

[0023] According to a preferred embodiment of the present invention, R1 and R2 are each independently hydrogen or a C1-C4 alkyl group; preferably, R1 is hydrogen and R2 is hydrogen or methyl. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0024] According to a preferred embodiment of the present invention, the substituent of the alkoxy group is a halogen and / or a hydroxyl group.

[0025] According to a preferred embodiment of the present invention, R3 is an amino group, a hydroxyl group, a C1-C8 alkoxy group, or a C1-C4 alkoxy group substituted with a halogen and / or hydroxyl group. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0026] According to a preferred embodiment of the present invention, the monomeric compound is selected from one or more of acrylamide, methyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and 3-chloro-2-hydroxypropyl methacrylate, preferably one or more of acrylamide, methacrylic acid, methyl methacrylate, ethyl methacrylate, and 3-chloro-2-hydroxypropyl methacrylate, more preferably a mixture of acrylamide and 3-chloro-2-hydroxypropyl methacrylate, wherein the mass ratio of acrylamide to 3-chloro-2-hydroxypropyl methacrylate in the mixture is 0.5-2:1, for example, 0.6:1, 0.8:1, 1:1, 1.2:1, 1.4:1, 1.6:1, and 1.8:1. The advantages of the present invention are illustrated by using a mass ratio of 1:1 for acrylamide to 3-chloro-2-hydroxypropyl methacrylate in the mixture. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0027] In this invention, as long as the purpose of this invention can be achieved, there are no special requirements for the type of initiator. Commonly used initiators in the art can be applied to this invention. The following is an illustrative description, but it does not limit the scope of this invention. According to a preferred embodiment of this invention, the initiator is one or more of peroxy acid salts, peroxides, and aryl ketones, preferably one or more of lauroyl peroxide, dicyclohexyl percarbonate, tert-butyl hydroperoxide, cyclohexanone peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, benzophenone, and xanthones.

[0028] According to a preferred embodiment of the present invention, the fiber is selected from one or more of nylon, polyester, and PTFE, preferably nylon. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0029] In this invention, there are no special requirements for the pore size of the fiber. Commonly used pore sizes of fibers in the art can be applied to this invention. The following is an illustrative description, but it does not limit the scope of this invention. For example, the pore size of the fiber is 300-4500 mesh.

[0030] In this invention, the composition of the modified solution can be selected from a wide range. The following is an illustrative description, but it does not limit the scope of the invention. According to a preferred embodiment of the invention, based on the total weight of the modified solution, the content of the monomer compound is 4-20 wt%, for example, it can be 5 wt%, 8 wt%, 10 wt%, 12 wt%, 14 wt%, 15 wt%, 16 wt%, and 18 wt%, preferably 5-15 wt%. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0031] In this invention, the range of alcohol content is relatively wide. The following is an illustrative description, but it does not limit the scope of the invention. According to a preferred embodiment of the invention, the alcohol content is 15-80 wt%, preferably 40-60 wt%, based on the total weight of the modified solution.

[0032] According to a preferred embodiment of the present invention, the polyenol content is 2-20 wt% based on the total weight of the modified solution, for example, it can be 3 wt%, 6 wt%, 8 wt%, 12 wt%, 16 wt%, 18 wt%, and 19 wt%, preferably 5-10 wt%. By adopting the aforementioned preferred embodiment, the hydrophilic and oleophobic properties and antifouling properties of the fiber material can be further improved.

[0033] In this invention, as long as the purpose of this invention can be achieved, the content of the initiator is not particularly required. The following is an illustrative description, but it does not limit the scope of this invention. According to a preferred embodiment of this invention, the content of the initiator is 0.5-3 wt%, preferably 1-2 wt%, based on the total weight of the modified solution.

[0034] In this invention, as long as the purpose of this invention can be achieved, there are no special requirements for the content of the water solvent. The following is an illustrative description, but it does not limit the scope of this invention. According to a preferred embodiment of this invention, the content of the water solvent is 0-75 wt%, preferably 30-70 wt%, based on the total weight of the modified solution.

[0035] In this invention, as long as the purpose of this invention can be achieved, the contact method in step (2) can be a conventional choice in the art. The following is an illustrative example, but it does not limit the scope of this invention. For example, in step (2), the contact is an immersion contact and / or a coating contact.

[0036] In this invention, as long as the objective of this invention can be achieved, the amount of fiber and modified solution used in step (2) can be selected within a wide range, specifically determined based on the contact method and the target product. For example, during the soaking process, it is sufficient to ensure that the modified solution covers the fiber; generally, the volume ratio of fiber to modified solution is 1:1-5, preferably 1:2-4. For example, during the coating process, it is sufficient to ensure that the modified solution is uniformly coated on the fiber; the specific amount is determined based on the target product.

[0037] In this invention, as long as the purpose of this invention can be achieved, the processing method in step (2) is a conventional technical means in the field, such as light processing and / or heat processing.

[0038] In this invention, the range of selectable light processing conditions is relatively wide, and commonly used light processing conditions in the art can all be applied to this invention. For example, light processing conditions include: ultraviolet irradiation, irradiation time of 0.5-12h, and irradiation intensity of 15-60W.

[0039] In this invention, as long as the purpose of this invention can be achieved, there are no special requirements for the heat treatment method. For example, the heat treatment method can be one or more of water bath, microwave, and ultrasonic.

[0040] In this invention, the range of selectable heat treatment conditions is relatively wide, and commonly used heat treatment conditions in the art can be applied to this invention. For example, the heat treatment conditions include: a heating temperature of 70-120°C, and a heating time selected and determined according to the temperature, for example, a heating time of 2-12 hours.

[0041] In this invention, depending on the source and cleanliness of the fiber, the fiber can be pretreated to remove impurities before step (1).

[0042] In this invention, as long as the purpose of this invention can be achieved, the pretreatment method can be a conventional technique in the field, and the specific method is selected and determined according to the type of impurities. For example, it can be alkaline treatment. The pretreatment method includes: contacting the fiber with an aqueous solution containing an alkaline substance, and then washing it with acetone solvent.

[0043] In this invention, as long as impurities in the fiber can be removed, the volume ratio of the fiber to the aqueous solution containing the alkaline substance can be a conventional choice in the art. For example, the volume ratio of the fiber to the aqueous solution containing the alkaline substance is 1:1-5, preferably 1:2-4.

[0044] In this invention, the concentration of the treatment agent in the aqueous solution containing the alkaline substance is 0.1-1 wt%.

[0045] In this invention, the type of alkaline substance can be a conventional choice in the art. The following is an illustrative description, but it does not limit the scope of the invention. According to a preferred embodiment of the invention, the alkaline substance is selected from one or more of MOH, MCO3, and MHCO3, wherein M is an alkali metal element and / or an alkaline earth metal element, such as sodium hydroxide, sodium carbonate, sodium bicarbonate, etc.

[0046] In this invention, the range of possible pretreatment conditions is relatively wide. The following is an illustrative example, but it does not limit the scope of this invention. For example, the pretreatment conditions include: a temperature of 90-150°C; and the time can be adjusted accordingly as the temperature changes, for example, a time of 0.5-2 hours.

[0047] According to a preferred embodiment of the present invention, the method further includes: washing the fibers after contact treatment. The washing method can be any conventional technique in the art, such as centrifugation, as long as it achieves the purpose of the present invention.

[0048] This invention provides a modified fiber material prepared by the method described above.

[0049] The fiber material prepared by the method of the present invention has excellent underwater oleophobic properties and superior oil-bearing capacity under wetting conditions. Accordingly, the present invention provides an application of the modified fiber material in oil-water separation.

[0050] The present invention will be described in detail below through embodiments.

[0051] In the following embodiments,

[0052] The underwater oil contact angle was measured using a DCAT21 dynamic contact angle and surface tension meter from DataPhysics, Germany.

[0053] The oil holding height under wetting conditions was measured by fixing the filter cloth to the bottom of the glass tube, adding the oil phase (cyclohexane) after wetting, and finally measuring the oil phase height.

[0054] The filter cloth material is a commercially available product from Shanghai Heqi Glass Instrument Co., Ltd. Unless otherwise specified, all other materials are commercially available products.

[0055] In the following examples, unless otherwise specified, the content refers to the weight content.

[0056] Example 1

[0057] (1) Place 400-mesh nylon filter cloth in a 0.4wt% sodium carbonate aqueous solution with a volume ratio of nylon to sodium carbonate aqueous solution of 1:2, boil for 30 minutes, and clean the surface with acetone.

[0058] (2) Soak the filter cloth in a mixture of 5% methacrylic acid, 1% potassium persulfate, 10% polyvinyl alcohol (polymerization degree of 1800), 40% ethanol and 44% water at 80°C for 1 hour. The volume ratio of nylon to the mixture is 1:2. Place the soaked filter cloth in a UV curing instrument and irradiate for 2 hours at an intensity of 40W.

[0059] (3) Modified filter cloth is obtained after centrifugal washing of the filter cloth. A schematic diagram of the surface of the modified filter cloth before modification is shown in the figure. Figure 1 As shown in the schematic diagram of the surface of the modified filter cloth, see below. Figure 2 As shown, an underwater hydrophobicity evaluation experiment was conducted on the modified filter cloth: the underwater oil contact angle increased from 0° before modification to 58°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 31cm, showing significant effects.

[0060] Example 2

[0061] (1) Soak a clean 400-mesh polyester filter cloth in a mixture of 5% methacrylic acid, 1% potassium persulfate, 10% polyvinyl alcohol (polymerization degree of 1800), 40% ethanol and 44% water at 80°C for 1 hour. The volume ratio of polyester to the mixture is 1:2. Place the soaked filter cloth in a UV curing instrument and irradiate for 2 hours at an intensity of 40W.

[0062] (2) After centrifugation and cleaning of the filter cloth, the modified filter cloth was obtained. The underwater hydrophobicity evaluation experiment of the modified filter cloth was carried out: the underwater oil contact angle increased from 0° before modification to 42°, and the oil bearing height under wetting conditions increased from 30cm before modification to 49cm, which showed significant effect.

[0063] Example 3

[0064] (1) Soak a clean 400-mesh PTFE filter cloth in a mixture of 5% methacrylic acid, 1% potassium persulfate, 10% polyvinyl alcohol (polymerization degree of 1800), 40% ethanol and 44% water at 80°C for 1 hour. The volume ratio of polyester to the mixture is 1:2. Place the soaked filter cloth in a UV curing instrument and irradiate it for 2 hours at an intensity of 40W.

[0065] (2) After centrifugation and cleaning of the filter cloth, the modified filter cloth was obtained. The underwater hydrophobicity evaluation experiment of the modified filter cloth was carried out: the underwater oil contact angle increased from 0° before modification to 126.5°, and the oil holding height under wetting conditions increased from 22cm before modification to 32cm, which showed significant effect.

[0066] Example 4

[0067] Same as Example 1, except that the monomer compound is acrylamide, and all other conditions are the same.

[0068] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 57°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 30cm.

[0069] Example 5

[0070] Same as Example 1, except that the monomer compound is methyl methacrylate, and all other conditions are the same.

[0071] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 58°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 31cm.

[0072] Example 6

[0073] Same as Example 1, except that the monomer compound is 3-chloro-2-hydroxypropyl methacrylate, and all other conditions are the same.

[0074] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 56°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 35cm.

[0075] Example 7

[0076] Same as Example 1, except that the monomer compound is ethyl methacrylate, and all other conditions are the same.

[0077] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 55°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 29cm.

[0078] Example 8

[0079] Same as Example 1, except that the monomer compound is butyl methacrylate, and all other conditions are the same.

[0080] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 52°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 25cm.

[0081] Example 9

[0082] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% 2-ethylhexyl methacrylate, 1% potassium persulfate, 5% polyvinyl alcohol (degree of polymerization 1800), 15% ethanol and 74% water, while other conditions were the same.

[0083] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 55°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 28cm.

[0084] Example 10

[0085] Same as Example 1, except that the polyol is polyacrylol (degree of polymerization is 1800), and all other conditions are the same.

[0086] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 57°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 29cm.

[0087] Example 11

[0088] Same as Example 1, except that isopropanol is used as the alcohol, and all other conditions are the same.

[0089] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 56°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 28cm.

[0090] Example 12

[0091] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% methacrylic acid, 1% potassium persulfate, 20% polyvinyl alcohol (degree of polymerization 1800), 15% ethanol and 59% water, while other conditions were the same.

[0092] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 51°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 20cm.

[0093] Example 13

[0094] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% methacrylic acid, 1% potassium persulfate, 15% polyvinyl alcohol (degree of polymerization 1800), 40% ethanol and 39% water, while other conditions were the same.

[0095] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 51°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 21cm.

[0096] Example 14

[0097] Similar to Example 1, except that the filter cloth was soaked in a mixture of 2.5% acrylamide, 2.5% 3-chloro-2-hydroxypropyl methacrylate, 1% potassium persulfate, 10% polyvinyl alcohol (degree of polymerization 1800), 40% ethanol and 39% water, while other conditions were the same.

[0098] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 60°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 38cm.

[0099] Example 15

[0100] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% methacrylic acid, 1% potassium persulfate, 5% polyvinyl alcohol (degree of polymerization 1800), 5% polyacryl alcohol (degree of polymerization 1800), 40% ethanol and 39% water, while other conditions were the same.

[0101] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 61°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 39cm.

[0102] Comparative Example 1

[0103] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% methacrylic acid, 1% potassium persulfate and 94% water at 80°C for 1 hour, with other conditions remaining the same.

[0104] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 6°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 12cm.

[0105] Comparative Example 2

[0106] Similar to Example 1, except that the filter cloth was soaked in a mixture of 5% methacrylic acid, 1% potassium persulfate, 50% ethanol and 44% water at 80°C for 1 hour, with other conditions remaining the same.

[0107] The modified filter cloth was subjected to an underwater hydrophobicity evaluation experiment: the underwater oil contact angle increased from 0° before modification to 7°, and the oil-bearing height under wetting conditions increased from 9cm before modification to 13cm.

[0108] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for preparing a modified fiber material, characterized in that, The method includes: (1) A modified solution is obtained by mixing a monomeric compound having the structural formula shown in formula (I), an alcohol, a polyenol, an initiator and optionally an aqueous solvent; (2) The fiber is subjected to contact treatment with the modified solution; In this configuration, R1 and R2 are each independently hydrogen or C1-C8 alkyl groups; R3 is an amino group, a hydroxyl group, or a substituted or unsubstituted alkoxy group.

2. The method according to claim 1, wherein, The mass ratio of the alcohol to the polyenol is 0.2-10:1, preferably 1-5:1; and / or The degree of polymerization of the polyenol is 1500-2000; and / or The polyol is selected from polyvinyl alcohol and / or polyacryl alcohol, preferably the polyol is a mixture of polyvinyl alcohol and polyacryl alcohol, wherein the mass ratio of polyvinyl alcohol to polyacryl alcohol in the mixture is 0.5-2:1; and / or The alcohol is a C1-C5 alcohol, preferably selected from ethanol and / or isopropanol.

3. The method according to claim 1 or 2, wherein, R1 and R2 are each independently hydrogen or a C1-C4 alkyl group; preferably, R1 is hydrogen and R2 is hydrogen or methyl; and / or The alkoxy group is substituented with a halogen and / or a hydroxyl group; and / or The R3 is an amino, hydroxyl, C1-C8 alkoxy, halogen, and / or hydroxy-substituted C1-C4 alkoxy.

4. The method according to any one of claims 1-3, wherein, The monomeric compound is selected from one or more of acrylamide, methyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, and 3-chloro-2-hydroxypropyl methacrylate. Preferably, the monomeric compound is selected from one or more of acrylamide, methacrylic acid, methyl methacrylate, ethyl methacrylate, and 3-chloro-2-hydroxypropyl methacrylate; More preferably, the monomeric compound is selected from a mixture of acrylamide and 3-chloro-2-hydroxypropyl methacrylate, wherein the mass ratio of acrylamide to 3-chloro-2-hydroxypropyl methacrylate in the mixture is 0.5-2:

1.

5. The method according to any one of claims 1-4, wherein, The initiator is one or more of peroxy acid salts, organic peroxides, and aryl ketones. Preferably, the initiator is one or more of lauroyl peroxide, dicyclohexyl percarbonate, tert-butyl hydroperoxide, cyclohexanone peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, benzophenone, and xanthones. and / or The fiber is selected from one or more of nylon, polyester, and PTFE, preferably nylon; and / or The fiber has a pore size of 300-4500 mesh.

6. The method according to any one of claims 1-5, wherein, Based on the total weight of the modified solution, The content of the monomeric compound is 4-20 wt%, preferably 5-15 wt%; and / or The alcohol content is 15-80 wt%, preferably 40-60 wt%; and / or The polyol content is 2-20%, preferably 5-10 wt%; and / or The initiator content is 0.5-3 wt%, preferably 1-2 wt%; and / or The content of the water solvent is 0-75 wt%, preferably 30-70 wt%.

7. The method according to any one of claims 1-4, wherein, In step (2), The contact is an immersion contact and / or a coating contact; and / or When the contact is an immersion contact, the volume ratio of the fiber to the modified solution is 1:1-5, preferably 1:2-4; and / or The treatment is optical treatment and / or thermal treatment; Preferably, The conditions for light treatment include: ultraviolet irradiation, irradiation time of 0.5-12 hours, and irradiation intensity of 15-60W; and / or The conditions for heat treatment include: The heat treatment method is one or more of water bath, microwave, and ultrasonic treatment; and / or The heating temperature is 70-120℃, and the heating time is 2-12 hours.

8. The method according to any one of claims 1-7, wherein, The method also includes: Before step (1), the fibers are pretreated to remove impurities, preferably by alkaline treatment; and / or The fibers after contact treatment in step (2) are cleaned, preferably by centrifugal cleaning.

9. The modified fiber material prepared by the method according to any one of claims 1-8.

10. The application of the modified fiber material according to claim 9 in oil-water separation.