Preparation method and application of bio-based self-repairing cashmere fabric anti-pilling finishing agent

By using a bio-based self-healing waterborne polyurethane finishing agent, combined with dynamic covalent bonds and POSS nanoparticles, the problem of pilling in cashmere fabrics has been solved, achieving a balance of self-healing, wear resistance, and soft hand feel, making it suitable for high-end cashmere products.

CN123064015APending Publication Date: 2026-11-10嘉兴欧美斯羊绒制品股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611128496.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing waterborne polyurethane anti-pilling finishing agents rely on petrochemical resources, lack self-healing capabilities, and have insufficient mechanical properties, affecting the wearing comfort and appearance of cashmere fabrics.

Method used

Using a bio-based self-healing waterborne polyurethane finishing agent, dynamic covalent bonds and POSS nanoparticles are introduced to form a film layer with self-healing, wear resistance and soft feel. Combined with ultraviolet light or thermal crosslinking technology, the self-healing and wear resistance properties are improved.

Benefits of technology

It achieves durable anti-pilling and anti-fuzzing properties for cashmere fabrics, multiple self-repair capabilities, unchanged softness, and high breathability retention, making it suitable for high-end environmentally friendly cashmere products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123064015A_ABST
    Figure CN123064015A_ABST
Patent Text Reader

Abstract

The application discloses a preparation method and application of a bio-based self-repairing cashmere fabric anti-pilling finishing agent, and the preparation method comprises the following steps: adding unsaturated polyester diol, polyethylene glycol monoether ester and a chain extender into a reaction container, heating and melting, and cooling; adding diisocyanate and an organic catalyst, and carrying out heat preservation reaction; adding a solvent to adjust viscosity, and stopping the reaction when the value of -NCO reaches a theoretical value; then adding POSS-isocyanate adduct into the reaction system to obtain a prepolymer; cooling the prepolymer, and then adding a neutralizing agent, stirring, and adding deionized water to carry out phase inversion emulsification, so as to obtain a water-based polyurethane dispersion; and removing the solvent through reduced pressure distillation, and filtering the discharge. By embedding a dynamic covalent bond into a polyurethane main chain, the finishing agent is endowed with a self-repairing capability. When a resin film generates microcracks due to friction, the dynamic bond reversibly exchanges at room temperature, automatically heals the cracks, and restores the film layer integrity and anti-pilling function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the preparation method and application of a bio-based self-healing anti-pilling finishing agent for cashmere fabrics, belonging to the technical field of functional finishing agents for cashmere fabrics. Background Technology

[0002] Cashmere, as a natural protein fiber, is soft to the touch, warm, highly absorbent, and comfortable to wear, making it highly valuable in the apparel industry, and fabrics made from it are very popular with consumers. However, cashmere fibers are relatively fine, and their surface scale structure is significant, making them prone to pilling and fuzzing during wear and friction, which severely affects the appearance and feel of the fabric. Anti-pilling finishing has always been a technical challenge in cashmere product processing. Currently, waterborne polyurethane (WPU) finishing agents are widely used in anti-pilling finishing of textiles due to their good film-forming properties, soft feel, and environmental friendliness. However, existing waterborne polyurethane anti-pilling finishing agents still have the following technical shortcomings: The monomers rely on petrochemical resources. Conventional waterborne polyurethanes often use polyether polyols (such as polypropylene glycol PPG) or polyester polyols (such as polybutylene adipate PBA) for the soft segments, and isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), or hexamethylene diisocyanate (HDI) for the hard segments. These monomers are all derived from non-renewable petrochemical raw materials, which is inconsistent with current policies promoting green, low-carbon, and sustainable development.

[0003] Finishing agents lack self-healing capabilities after film formation. Conventional waterborne polyurethane resin films formed on cashmere fiber surfaces rapidly lose their anti-pilling properties and cannot self-repair once micro-cracks or damage occur during wear and friction.

[0004] The mechanical properties and abrasion resistance of resin films need improvement. Conventional waterborne polyurethanes have limited mechanical strength, and the film layer formed on the surface of cashmere fibers is insufficient to resist repeated friction. To enhance the film layer performance, existing technologies typically employ methods to increase the degree of crosslinking, but this often results in a stiff feel and reduced breathability, affecting the wearing comfort of cashmere products.

[0005] In summary, developing a novel anti-pilling finishing agent that combines bio-based origin, self-healing function, excellent mechanical properties, and functional scalability has significant industrial value and technological innovation implications. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a bio-based self-healing waterborne polyurethane anti-pilling finishing agent. Through molecular structure design, the finishing agent is endowed with self-healing properties, high abrasion resistance, biodegradability and post-crosslinking ability, and achieves the unity of durable anti-pilling and soft hand feel for cashmere fabrics.

[0007] To solve the above-mentioned technical problems, the objective of this invention is achieved as follows: The present invention relates to a method for preparing a bio-based self-healing anti-pilling finishing agent for cashmere fabrics, comprising the following steps: Unsaturated polyester glycol, polyethylene glycol monoether ester, and chain extender are added to a reaction vessel and heated to 90-110℃ to melt and mix evenly. The mixture is then cooled to 70-85℃. Diisocyanate and a tin-containing organic catalyst are added under stirring, and the reaction is maintained at this temperature for 2-4 hours. During the reaction, an organic solvent is added to adjust the viscosity, and the reaction is stopped when -NCO reaches the theoretical value. The POSS-isocyanate adduct is then added to the above reaction system, and the reaction continues for 0.5-1 hour to obtain the prepolymer. The prepared prepolymer was cooled to 40-50℃, and then a neutralizing agent was added to neutralize the carboxyl groups and stirred. Under the stirring of an emulsifier, deionized water was slowly added to perform reverse emulsification, and stirring was continued to obtain an aqueous polyurethane dispersion with a solid content of 30-40%. The solvent is removed by vacuum distillation, and the product is filtered out to obtain the finished finishing agent; The chain extender is an aromatic diol containing dynamic covalent bonds.

[0008] Furthermore, the unsaturated polyester glycol is itaconic acid-based unsaturated polyester glycol or rosin-based unsaturated polyester glycol; the chain extender is 4,4-dihydroxydiphenyl disulfide or bis(4-hydroxyphenyl)diselenoether; the tin-containing organic catalyst is dibutyltin dilaurate or stannous octoate; the diisocyanate is bio-based diisocyanate or petroleum-based diisocyanate; the neutralizing agent is triethylamine; and the organic solvent is acetone or butanone. Bio-based diisocyanate: preferably lysine diisocyanate (LDI) or dimer fatty acid diisocyanate (DDI), partially or completely replacing petroleum-based IPDI / HDI, further increasing the bio-based content of the finishing agent and reducing its carbon footprint.

[0009] The aromatic diol containing dynamic covalent bonds is preferably 4,4-dihydroxydiphenyl disulfide (DHPDS) or bis(4-hydroxyphenyl)diselenoether. The phenolic hydroxyl group of this chain extender reacts with the isocyanate to covalently embed the disulfide bond (-SS-) or diselenoether bond (-Se-Se-) into the polyurethane backbone. When microcracks develop in the resin film due to wear, the disulfide / diselenoether bonds undergo a reversible exchange reaction at room temperature, achieving self-repair of the cracks and significantly extending the effective lifespan of the anti-pilling finishing process. Introducing dynamic covalent bonds through backbone embedding offers advantages over externally compounded crosslinking agents, including higher self-repair efficiency and stronger multiple repair capabilities.

[0010] Furthermore, the synthesis process of the itaconic acid-based unsaturated polyester glycol is as follows: itaconic acid and diol are added to a reaction vessel at a molar ratio of 1:1.05-1:1.2, and p-toluenesulfonic acid is added as a catalyst. The mixture is heated to 160-200℃ under a protective gas atmosphere for melt polycondensation. During the reaction, the generated water is continuously removed until the acid value drops below 10 mg KOH / g. The temperature is then lowered to 80-100℃, and low-boiling substances are removed by vacuum distillation to obtain itaconic acid-based unsaturated polyester glycol with a number average molecular weight of 1000-4000. The amount of p-toluenesulfonic acid catalyst used is 0.1-0.5% of the total weight of itaconic acid and diol. The itaconic acid-based unsaturated polyester glycol is synthesized by melt polycondensation of bio-based itaconic acid obtained from sugar fermentation and diol, and its main chain contains carbon-carbon double bonds. The beneficial effects of this soft segment are: first, the raw materials are renewable, which aligns with the concept of green chemistry; second, the double bonds in the main chain can undergo free radical cross-linking after finishing through ultraviolet light or thermal initiation to form a secondary network, thereby improving the cross-linking density and abrasion resistance of the film layer; and third, the residual carboxyl groups of itaconic acid can regulate the hydrophilicity of the polymer and improve the stability of the emulsion.

[0011] Furthermore, the diol is 1,4-butanediol, neopentyl glycol, or ethylene glycol.

[0012] Furthermore, the polyethylene glycol monoether ester is itaconic acid polyethylene glycol monoether ester; the synthesis process of the itaconic acid polyethylene glycol monoether ester is as follows: itaconic acid and polyethylene glycol monomethyl ether are fed in a set molar ratio, p-toluenesulfonic acid catalyst and hydroquinone polymerization inhibitor are added, and the reaction is carried out at 120-150℃ for 4-6 hours, and then the acid value is adjusted to below 5 mg KOH / g to obtain itaconic acid polyethylene glycol monoether ester; the amount of p-toluenesulfonic acid catalyst is 0.2-0.5 wt%; the amount of hydroquinone polymerization inhibitor is 0.1-0.3 wt%.

[0013] Itaconic acid polyethylene glycol monoether ester (IM): Synthesized by esterification of itaconic acid and polyethylene glycol monomethyl ether (MPEG), the molecule contains both carboxyl groups (providing hydrophilicity) and carbon-carbon double bonds (providing post-crosslinking sites). IM replaces conventional DMPA or DMBA, serving both as a hydrophilic monomer to achieve self-emulsification of waterborne polyurethanes and introducing crosslinkable double bonds for subsequent UV curing, thus achieving a unity of hydrophilic and crosslinking functions.

[0014] Furthermore, the POSS-isocyanate adduct is prepared by reacting polyhedral oligomeric silsesquioxane with diisocyanate in a protective gas environment at 60-70°C.

[0015] Furthermore, the polyhedral oligomeric silsesquioxane is an amino polyhedral oligomeric silsesquioxane or a polyhedral oligomeric silsesquioxane modified with fluorinated alkyl groups. The amino polyhedral oligomeric silsesquioxane (NH2-POSS) has a cage-like structure of approximately 1.5 nm, and the amino groups at its apex can react with isocyanates to covalently link to the polyurethane network. The introduction of POSS significantly improves the hardness, abrasion resistance, and heat resistance of the resin film, while maintaining the original soft feel of cashmere due to the nanoscale effect. The organic groups (such as isobutyl groups) on the surface of POSS also impart hydrophobic and antifouling properties to the coating.

[0016] Furthermore, vacuum distillation is carried out at 50-60℃ and -0.9MPa.

[0017] The present invention also relates to the application of the prepared finishing agent in the finishing process of cashmere fabrics.

[0018] Furthermore, the cashmere fabric finishing process includes the following steps: (1) Impregnation: Impregnate the cashmere fabric in the finishing agent dispersion at a bath ratio of 1:20-1:30. The amount of finishing agent is 2-6% (owf) of the fabric weight. Impregnate at room temperature for 20-40 minutes. (2) Dehydration: residual rate 70-85%; (3) Pre-baking: Pre-baking at 50-60℃ for 3-5 minutes; (4) UV curing / thermal crosslinking: Irradiate under 365nm UV light for 2-5 minutes to initiate free radical crosslinking reaction of carbon-carbon double bonds in the main chain of polyethylene glycol monoether ester and unsaturated polyester diol to form a secondary network; (5) Baking: Baking at 70-90℃ for 1-3 minutes to complete the finishing.

[0019] The beneficial effects of this invention are as follows: The preparation method and application of the bio-based self-healing anti-pilling finishing agent for cashmere fabrics involved in this invention endow the finishing agent with self-healing capabilities by embedding dynamic covalent bonds into the polyurethane backbone. When microcracks are generated in the resin film due to friction, the dynamic bonds undergo reversible exchange at room temperature, automatically healing the cracks and restoring the integrity of the film layer and its anti-pilling function. Compared with traditional external microcapsule self-healing systems, the self-healing mechanism of this invention has the significant advantages of being able to repair multiple times and without the depletion of the repair agent.

[0020] POSS is covalently grafted onto a polyurethane network. Its rigid cage-like structure hinders crack propagation at the nanoscale, significantly improving the hardness and abrasion resistance of the resin film. At the same time, the nanoscale effect of POSS does not damage the original soft feel of cashmere, achieving "enhancement without hardening".

[0021] By utilizing the carbon-carbon double bonds in itaconic acid residues and itaconic acid polyethylene glycol monoether ester monomers, secondary crosslinking can be initiated by ultraviolet light or heat after finishing, allowing for flexible control of the crosslinking density and mechanical properties of the film. This post-crosslinking process also avoids the gelation risk inherent in the synthesis process.

[0022] The POSS and dynamic bond sites in the molecular structure of finishing agents can serve as anchoring points for functional groups, making it easy to introduce functional units such as antibacterial, anti-UV, and hydrophobic properties, thereby achieving synergy between anti-pilling and multiple functions.

[0023] The finishing agent of this invention forms a thin and flexible film on the surface of cashmere fibers. Combined with the nano-reinforcement method of POSS, it does not affect the natural curl and fluffiness of cashmere fibers. The softness of the finished cashmere fabric can reach 3.5-4.0 (out of 5), and the air permeability retention rate is ≥90%. Attached Figure Description

[0024] Figure 1 This describes the microstructure of the cashmere fabric after processing according to the present invention. Detailed Implementation

[0025] The present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0026] Example 1 The raw materials and reagents used in this embodiment are as follows: Itaconic acid: purity ≥99%, Shandong Zhongke Biotechnology Co., Ltd.; 1,4-Butanediol (BDO): analytical grade, Sinopharm Group; Polyethylene glycol monomethyl ether (MPEG-500): Mn=500, Sigma-Aldrich; Lysine diisocyanate (LDI): purity ≥98%, Shanghai Maclean Biochemical Technology; Isophorone diisocyanate (IPDI): industrial grade, Wanhua Chemical; 4,4-Dihydroxydiphenyl disulfide (DHPDS): purity ≥98%, Sigma-Aldrich; Aminopropyl isobutyl POSS (NH2-POSS): purity ≥95%, Hybrid Plastics, USA; Dibutyltin dilaurate (DBTDL): analytical grade, Sinopharm Group; Triethylamine (TEA): analytical grade, Sinopharm Group; Acetone: analytical grade, Sinopharm Group; Deionized water.

[0027] Synthesis of Itaconic Acid-Based Unsaturated Polyester Diol (PBI) In a 500 mL four-necked flask equipped with a stirrer, thermometer, nitrogen inlet, and water separator, itaconic acid (130.1 g, 1.0 mol), 1,4-butanediol (99.1 g, 1.1 mol), and p-toluenesulfonic acid (0.58 g) were added. Under nitrogen protection, the mixture was heated to 170 °C and stirred until melted. Water generated during the reaction was continuously drained through the water separator. When the acid value of the reaction system dropped below 15 mg KOH / g, the temperature was raised to 190 °C, the pressure was reduced to 20 mmHg, and the reaction continued for 1 hour. The mixture was then cooled to 80 °C and discharged, yielding a light yellow viscous liquid, PBI. The measured acid value was 8.5 mg KOH / g, the hydroxyl value was 56.2 mg KOH / g, and the number-average molecular weight (GPC) was approximately 2000.

[0028] Synthesis of itaconic acid polyethylene glycol monoether ester (IM) In a 250 mL three-necked flask, itaconic acid (65.0 g, 0.5 mol), MPEG-500 (275 g, 0.55 mol), p-toluenesulfonic acid (0.85 g), and hydroquinone (0.34 g) were added. Nitrogen gas was introduced, and the mixture was heated to 140 °C and stirred for 5 hours until the acid value dropped below 5 mg KOH / g. The mixture was then cooled to room temperature to obtain a pale yellow viscous liquid IM (acid value 4.2 mg KOH / g).

[0029] Preparation of finishing agent Prepolymerization reaction: In a dry 500 mL four-necked flask, add PBI (80.0 g, 0.04 mol), IM (15.0 g, 0.03 mol), and DHPDS (4.0 g, 0.016 mol), heat to 100 °C to melt and mix evenly, then cool to 80 °C. Add LDI (21.0 g, 0.10 mol), IPDI (8.8 g, 0.04 mol), and catalyst DBTDL (0.12 g), and maintain the reaction temperature for 3 hours. During the reaction, add acetone (50 mL) to adjust the viscosity. Determine the -NCO content using the di-n-butylamine method; stop the reaction when the -NCO content reaches the theoretical value (approximately 2.8%).

[0030] POSS grafting: In another small reaction flask, NH2-POSS (3.0 g, about 0.003 mol) and IPDI (1.5 g, 0.0067 mol) were reacted at 60 °C under nitrogen for 1 hour to prepare the POSS-isocyanate adduct. This adduct was added to the above prepolymer, and the reaction was continued for 40 minutes.

[0031] Neutralization and emulsification: The prepolymer was cooled to 45°C, and triethylamine (calculated based on the total number of carboxyl groups; the total amount of carboxyl groups in IM and PBI is approximately 0.033 mol, so 3.34 g of triethylamine was added) was added, and the mixture was stirred for 20 minutes. Under high-shear emulsifier (3000 rpm) stirring, deionized water (350 mL) was slowly added dropwise. After the addition was complete, emulsification was continued for 40 minutes to obtain a milky white aqueous dispersion with a bluish sheen.

[0032] Solvent removal: Acetone was removed by vacuum distillation at 50℃ and -0.09MPa for 2 hours. After filtration, a finishing agent with a solid content of about 33.5% (labeled as WPU-1) was obtained.

[0033] Cashmere fabric finishing 1. Take 100% pure cashmere knitted fabric (2 / 26Nm double-ply yarn, 10 count, 6cm stretch) and process it according to the following steps: Immerse the fabric in WPU-1 finishing agent (diluted to a solid content of 3.0%) at a liquor ratio of 1:25 for 30 minutes at room temperature. 2. Dehydrated, with a residual rate of 80%, meaning the moisture content is 80%; 3. Pre-bake at 55℃ for 4 minutes; 4. Irradiate with 365nm ultraviolet light for 3 minutes (lamp power 40W, distance 10cm); 5. Bake at 80℃ for 3 minutes.

[0034] The WPU-1 treated cashmere fabric was tested for initial anti-pilling performance, anti-pilling performance after 15 washes, hand softness, tensile strength retention rate, and self-healing efficiency. The results are as follows: Self-healing efficiency test method: The WPU-1 coating was scratched with a blade with a width of about 50 μm and placed in a 60℃ oven for 4 hours. The scratch width was reduced by 82%, indicating that the dynamic exchange of disulfide bonds effectively repaired the film damage.

[0035] SEM observation showed that the surface of the cashmere fibers after treatment was covered with a uniform, transparent, and crack-free film, and the edges of the fiber scales were covered, indicating that the finishing agent had good film-forming properties.

[0036] Example 2 In Example 1, DHPDS (4,4-dihydroxydiphenyl disulfide) was replaced with an equimolar amount of bis(4-hydroxyphenyl)diselenoether, and the remaining components and steps were the same as in Example 1. The resulting finishing agent was labeled WPU-2.

[0037] Test results show that WPU-2 has an initial anti-pilling rating of 4, a rating of 3.5 after 15 washes, and a hand feel score of 4.2. The self-healing efficiency test (60℃, 4h) shows a scratch repair rate of 89%, higher than WPU-1's 82%, proving that the diselenyl bond has a faster dynamic exchange rate and superior self-healing performance.

[0038] Example 3 In Example 1, all the LDI+IPDI hard segments were replaced with LDI (28.0 g, 0.13 mol), while the amount of IPDI was reduced to 0. Diisocyanate (DDI, 3.0 g) was used to partially replace LDI to adjust the compatibility of the soft and hard segments. The remaining steps were the same as in Example 1. The calculated bio-based content of the resulting finishing agent was approximately 68%.

[0039] Test results show that the initial anti-pilling rating is 4.0, which decreases to 3.5 after 15 washes, and the hand feel is rated 4.5 (softer). The all-bio-based solution has a greater advantage in environmental friendliness and is suitable for high-end environmentally friendly cashmere products.

[0040] Example 4 Rosin-based polyester diol was used to replace PBI: rosin acid (302.5 g, 1.0 mol) and ethylene glycol (68.1 g, 1.1 mol) were esterified at 200-240 °C under nitrogen protection until the acid value decreased to below 10 mg KOH / g, yielding rosin-based polyester diol (Mn approximately 1800). The remaining components were synthesized according to Example 1 to obtain the finishing agent (WPU-4).

[0041] Test results: Initial anti-pilling rating: 4; after 15 washes: 3.5; hand feel: 3.8 (slightly stiff). This solution offers better abrasion resistance but a slightly inferior hand feel, suitable for cashmere coat fabrics where a smooth appearance is crucial. All the above embodiments achieved good anti-pilling effects. Embodiment 1, due to its balanced overall performance (excellent anti-pilling, hand feel, and self-healing efficiency), is the optimal implementation. Embodiment 2 excels in self-healing speed, while Embodiment 3 leads in environmental friendliness.

[0042] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.

Claims

1. A method for preparing a bio-based self-healing anti-pilling finishing agent for cashmere fabrics, characterized in that, Includes the following steps: Unsaturated polyester glycol, polyethylene glycol monoether ester, and chain extender are added to a reaction vessel and heated to 90-110℃ to melt and mix evenly. The mixture is then cooled to 70-85℃. Diisocyanate and a tin-containing organic catalyst are added under stirring, and the reaction is maintained at this temperature for 2-4 hours. During the reaction, an organic solvent is added to adjust the viscosity, and the reaction is stopped when -NCO reaches the theoretical value. The POSS-isocyanate adduct is then added to the above reaction system, and the reaction continues for 0.5-1 hour to obtain the prepolymer. The prepared prepolymer was cooled to 40-50℃, and then a neutralizing agent was added to neutralize the carboxyl groups and stirred. Under the stirring of an emulsifier, deionized water was slowly added to perform reverse emulsification, and stirring was continued to obtain an aqueous polyurethane dispersion with a solid content of 30-40%. The solvent is removed by vacuum distillation, and the product is filtered out to obtain the finished finishing agent; The chain extender is an aromatic diol containing dynamic covalent bonds.

2. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 1, characterized in that, The unsaturated polyester glycol is itaconic acid-based unsaturated polyester glycol or rosin-based unsaturated polyester glycol; the chain extender is 4,4-dihydroxydiphenyl disulfide or bis(4-hydroxyphenyl)diselenoether; the tin-containing organic catalyst is dibutyltin dilaurate or stannous octoate; the diisocyanate is bio-based diisocyanate or petroleum-based diisocyanate; the neutralizing agent is triethylamine; and the organic solvent is acetone or butanone.

3. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 2, characterized in that, The synthesis process of the itaconic acid-based unsaturated polyester glycol is as follows: itaconic acid and diol are added to a reaction vessel at a molar ratio of 1:1.05-1:1.2, and p-toluenesulfonic acid is added as a catalyst. The mixture is heated to 160-200℃ under a protective gas atmosphere to carry out a melt polycondensation reaction. During the reaction, the generated water is continuously removed until the acid value drops below 10 mg KOH / g. The temperature is then lowered to 80-100℃, and low-boiling substances are removed by vacuum distillation to obtain itaconic acid-based unsaturated polyester glycol with a number average molecular weight of 1000-4000. The amount of p-toluenesulfonic acid catalyst used is 0.1-0.5% of the total weight of itaconic acid and diol.

4. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 3, characterized in that, The diol is 1,4-butanediol, neopentyl glycol, or ethylene glycol.

5. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 1, characterized in that, The polyethylene glycol monoether ester is itaconic acid polyethylene glycol monoether ester; the synthesis process of the itaconic acid polyethylene glycol monoether ester is as follows: itaconic acid and polyethylene glycol monomethyl ether are fed in a set molar ratio, p-toluenesulfonic acid catalyst and hydroquinone polymerization inhibitor are added, and the reaction is carried out at 120-150℃ for 4-6 hours, and the acid value is adjusted to below 5mg KOH / g to obtain itaconic acid polyethylene glycol monoether ester; The amount of the catalyst p-toluenesulfonic acid is 0.2-0.5 wt%; the amount of the polymerization inhibitor hydroquinone is 0.1-0.3 wt%.

6. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 1, characterized in that, The POSS-isocyanate adduct is prepared by reacting polyhedral oligomeric silsesquioxane with diisocyanate in a protective gas environment at 60-70°C.

7. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 6, characterized in that, The polyhedral oligomeric silsesquioxane is an amino polyhedral oligomeric silsesquioxane or a polyhedral oligomeric silsesquioxane modified with fluorinated alkyl groups.

8. The method for preparing the bio-based self-healing cashmere fabric anti-pilling finishing agent according to claim 1, characterized in that, Vacuum distillation is carried out at 50-60℃ and -0.9MPa.

9. The application of the finishing agent prepared according to any one of claims 1 to 7 in the finishing process of cashmere fabrics.

10. The application according to claim 9, characterized in that, The cashmere fabric finishing process includes the following steps: (1) Impregnation: Impregnate the cashmere fabric in the finishing agent dispersion at a bath ratio of 1:20-1:

30. The amount of finishing agent is 2-6% (owf) of the fabric weight. Impregnate at room temperature for 20-40 minutes. (2) Dehydration: residual rate 70-85%; (3) Pre-baking: Pre-baking at 50-60℃ for 3-5 minutes; (4) UV curing / thermal crosslinking: Irradiate under 365nm UV light for 2-5 minutes to initiate free radical crosslinking reaction of carbon-carbon double bonds in the main chain of polyethylene glycol monoether ester and unsaturated polyester diol to form a secondary network; (5) Baking: Baking at 70-90℃ for 1-3 minutes to complete the finishing.