A molding process for pulp molded products
By using a multi-stage progressive extrusion and hot-pressing process to gradually reduce the wall thickness of the wet blank and by using differentiated mold draft angles, the problem of uneven fiber distribution in pulp molding products during hot-pressing was solved, achieving high-yield molding of thick-walled products.
Patent Information
- Application Number
- CN202611270991.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-10
Smart Images

Figure CN123064064A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pulp molding technology, and in particular to a molding process for pulp molded products. Background Technology
[0002] Pulp molding products are a type of environmentally friendly packaging products made from waste paper or plant fibers. They are formed by vacuum adsorption in pulp using molds and then hot-pressed to set the shape. They are widely used for cushioning packaging in the fields of electronics, home appliances, and auto parts.
[0003] Currently, the conventional molding process for pulp molding products is a two-step process: first, the molding mold is immersed in the pulp, and paper fibers are deposited on the surface of the mold by vacuum suction to form a wet blank with a certain moisture content; then the wet blank is transferred to a hot press mold, and the lignin in the fibers is softened and cross-linked by high temperature and high pressure to complete the product shaping.
[0004] However, the above two-step process has the following technical problems: For products with small draft angles (steep sidewalls) and large wall thickness, the wall thickness of the wet blank adsorbed on the forming mold is usually 2.5-3.0 mm, while the final product wall thickness after the hot press mold is closed is only about 1.0-1.5 mm. Since the thickness of the wet blank is much larger than the gap of the hot press mold cavity, when the wet blank directly enters the hot press mold for one-time mold closing and shaping, the mold cavity wall will exert a violent lateral pushing force on the wet blank during the mold closing process. This forces a large number of paper fibers to flow and accumulate laterally in the mold gap, resulting in uneven fiber distribution and local accumulation on the sidewall of the product (commonly known as "pulping"), which can lead to product scrap in severe cases. This problem cannot be effectively solved in the existing process that relies on only one hot press shaping.
[0005] To address the aforementioned issues, there is currently no existing technology that employs multi-pass progressive extrusion to gradually reduce the wall thickness of the wet billet while simultaneously coordinating angle transitions. Summary of the Invention
[0006] The purpose of this invention is to provide a molding process for pulp molded products to solve the problems mentioned in the background art.
[0007] The above-mentioned technical objective of the present invention is achieved through the following technical solution: A molding process for pulp molded products. It provides an extrusion upper die, a first hot pressing upper die, a second hot pressing upper die, a forming die, a first hot pressing lower die, and a second hot pressing lower die; The forming mold is disposed between the first hot pressing lower mold and the second hot pressing lower mold, the extrusion upper mold is disposed on the Y-axis side of the forming mold, and the first hot pressing upper mold and the second hot pressing upper mold are respectively disposed on both sides of the forming mold in the X-axis direction; The extrusion die is configured to reciprocate horizontally along the Y-axis; The first hot-pressing upper die and the second hot-pressing upper die are respectively configured to reciprocate horizontally along the X-axis; The forming mold, the first hot press lower mold, and the second hot press lower mold are respectively configured to move up and down along the Z-axis; In the process, when the first hot pressing upper die or the second hot pressing upper die moves along the X-axis to above the forming die, the extrusion upper die moves along the Y-axis to make way. The process includes the following steps: S1: The forming mold is immersed in the pulp slurry, and paper fibers are deposited on the surface of the forming mold by vacuum suction to form a wet blank; S2: First extrusion: The extrusion die moves along the Y-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the extrusion die, performing the first extrusion on the wet blank to initially reduce the wall thickness of the wet blank and change its draft angle. During the mold closing process, the extrusion die blows air and the forming die draws air. When the mold is separated, the forming die moves downward along the Z-axis, and the wet blank remains on the forming die. Subsequently, the extrusion die moves backward along the Y-axis to make way. S3: Second extrusion: The second hot press upper die moves along the X-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the second hot press upper die, performing a second extrusion on the wet blank. During the mold closing process, the second hot press upper die is selectively heated to cause at least partial cross-linking and pre-curing of the surface of the wet blank. During the mold closing process, the second hot press upper die blows air and the forming die evacuates air. When the mold is separated, the forming die moves downward along the Z-axis, and the wet blank remains on the forming die. S4: Third extrusion: The first hot press upper die moves along the X-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the first hot press upper die, performing a third extrusion on the wet blank to further change the wall thickness and draft angle of the wet blank. During the mold closing process, the first hot press upper die blows air and the forming die draws air. During the mold separation, the forming die moves downward along the Z-axis, and the forming die blows air and the first hot press upper die draws air, so that the wet blank is adsorbed onto the first hot press upper die and moves away from the forming die along the X-axis with the first hot press upper die. S5: Final Hot Press Shaping: The first hot press upper mold carries the wet blank along the X-axis to above the first hot press lower mold. The first hot press lower mold moves upward along the Z-axis and closes with the first hot press upper mold to perform hot press cross-linking and curing on the wet blank, completing the final shaping of the product. When separating the molds, the first hot press upper mold keeps evacuating air, and the first hot press lower mold moves downward along the Z-axis and blows air, so that the product remains in the first hot press upper mold; or, when separating the molds, the first hot press upper mold keeps blowing air, and the first hot press lower mold moves downward along the Z-axis and sucks air, so that the product remains in the first hot press lower mold.
[0008] A further setting is that, in step S2, the extrusion upper die is a concave die, the forming die is a convex die, and the wall thickness of the wet blank formed after the two are closed is 2.1-2.8mm. The draft angle of the inner wall of the extrusion upper die is 1.5°-2.0°, and the draft angle of the outer wall of the forming die is 0.5°-1.0°.
[0009] A further setting is that, in step S3, the second hot-pressing upper mold is a concave mold, the forming mold is a convex mold, and the wall thickness of the wet blank formed after the two are closed is 1.7-2.2mm. The draft angle of the inner wall of the second hot-pressing upper mold is 1.0°-1.6°, and the draft angle of the outer wall of the forming mold is 0.5°-1.0°.
[0010] A further setting is that, in step S4, the first hot-pressing upper mold is a concave mold, the forming mold is a convex mold, and the wall thickness of the wet blank formed after the two are closed is 1.2-1.6mm. The draft angle of the inner wall of the first hot-pressing upper mold is 0.2°-0.3°, and the draft angle of the outer wall of the forming mold is 0.5°-1.0°.
[0011] A further setting is that, in step S5, after the first hot-pressing upper mold and the first hot-pressing lower mold are closed, the product wall thickness formed between them is 1mm, and the draft angle of the inner wall of the first hot-pressing upper mold and the draft angle of the outer wall of the first hot-pressing lower mold are both 0.2°-0.3°.
[0012] A further setting is that, in step S3, when the top surface of the wet blank is smooth, the second hot press upper die is heated and the extrusion time is extended; when the top surface of the wet blank is mesh-like, the second hot press upper die is kept at room temperature.
[0013] A further setting is that, after step S5 is completed, the receiving tray is moved to the bottom of the first hot press upper mold, and the first hot press upper mold blows air to make the product fall into the receiving tray.
[0014] In summary, the beneficial effects of this invention are as follows: Compared with the existing two-step method in pulp molding process where wet blanks are directly shaped by a single hot pressing, this invention is based on a compact equipment layout with "forming mold in the center, extrusion upper mold on the Y-axis side, and two sets of hot pressing upper molds on both sides of the X-axis". With the coordinated action sequence of each mold moving independently along the X-axis, Y-axis and Z-axis, the extrusion upper mold and the hot pressing upper mold can automatically yield to each other without interference when working alternately, providing space and action guarantee for multi-pass continuous production. Based on this, the present invention employs a four-stage deformation process—three progressive extrusions and one final hot pressing—to gradually reduce the wall thickness of the wet blank from 2.1-2.8 mm to 1.0 mm. Simultaneously, the invention utilizes differentiated draft angles for each stage (extrusion die 1.5°-2.0° → second hot pressing die 1.0°-1.6° → first hot pressing die 0.2°-0.3°). This ensures gradual moisture removal while preventing lateral fiber flow and accumulation caused by large single-stage deformation. This effectively solves the problem of slurry pushing during mold closing for thick-walled products with small draft angles due to a severe mismatch between the mold clearance and the wet blank wall thickness. Furthermore, the second hot pressing die can be heated to either a smooth or mesh surface during the second extrusion, allowing the wet blank surface to undergo preliminary cross-linking and pre-curing before the third extrusion. This further improves the shape retention of the wet blank in subsequent large deformation processes, reduces the probability of internal bubbles and delamination defects, and ultimately achieves high-yield and stable molding of thin-walled wallpaper products with small draft angles. Attached Figure Description
[0015] Figure 1 This is a partial structural schematic diagram of the pulp molding product forming equipment of the present invention; Figure 2 This is a schematic diagram of the structure of a single extrusion of the present invention; Figure 3 This is a schematic diagram of the secondary extrusion structure of the present invention; Figure 4 This is a schematic diagram of the three-stage extrusion structure of the present invention; Figure 5 This is a schematic diagram of the hot-pressing structure of the present invention; Figure 6 This is a diagram showing the state changes of the wet blank of the present invention.
[0016] In the diagram: 1. Extrusion upper die; 2. Forming die; 3. First hot press upper die; 4. First hot press lower die; 5. Second hot press upper die; 6. Second hot press lower die; 7. Receiving tray; 8. Slurry pool. Detailed Implementation
[0017] To make the technical means, creative features, achieved objectives, and effects of this invention easier to understand, the invention is further described below with reference to specific embodiments and accompanying drawings. However, the following embodiments are merely preferred embodiments of this invention and not all embodiments. Other embodiments obtained by those skilled in the art based on the embodiments described herein without creative effort are all within the protection scope of this invention.
[0018] Specific embodiments of the present invention are described below with reference to the accompanying drawings.
[0019] like Figures 1 to 6 The above describes a molding process for a pulp molded product. It provides an extrusion upper die 1, a first hot pressing upper die 3, a second hot pressing upper die 5, a forming die 2, a first hot pressing lower die 4, and a second hot pressing lower die 6; The forming mold 2 is disposed between the first hot pressing lower mold 4 and the second hot pressing lower mold 6, the extrusion upper mold 1 is disposed on the Y-axis side of the forming mold 2, and the first hot pressing upper mold 3 and the second hot pressing upper mold 5 are respectively disposed on both sides of the X-axis direction of the forming mold 2; The extrusion die 1 is configured to reciprocate horizontally along the Y-axis; The first hot-pressing upper mold 3 and the second hot-pressing upper mold 5 are respectively configured to reciprocate horizontally along the X-axis; The forming mold 2, the first hot pressing lower mold 4 and the second hot pressing lower mold 6 are respectively configured to move up and down along the Z-axis; In the process, when the first hot pressing upper die 3 or the second hot pressing upper die 5 moves along the X-axis to above the forming die 2, the extrusion upper die 1 moves along the Y-axis to make way. The process includes the following steps: S1: The forming mold 2 is immersed in the pulp slurry of the pulp tank 8, and paper fibers are deposited on the surface of the forming mold 2 by vacuum suction to form a wet blank; S2: First extrusion: The extrusion die 1 moves along the Y-axis to above the forming die 2. The forming die 2 moves upward along the Z-axis and closes with the extrusion die 1 to perform the first extrusion on the wet blank, so as to initially reduce the wall thickness of the wet blank and change its draft angle. During the mold closing process, the extrusion die 1 blows air and the forming die 2 evacuates air. When the mold is separated, the forming die 2 moves downward along the Z-axis, and the wet blank remains on the forming die 2. Subsequently, the extrusion die 1 moves backward along the Y-axis to make way. S3: Second extrusion: The second hot press upper die 5 moves along the X-axis to above the forming die 2, and the forming die 2 moves upward along the Z-axis to close with the second hot press upper die 5, performing a second extrusion on the wet blank. During the mold closing process, the second hot press upper die 5 is selectively heated to cause at least partial cross-linking and pre-curing of the surface of the wet blank. During the mold closing process, the second hot press upper die 5 blows air and the forming die 2 extracts air. When the mold is separated, the forming die 2 moves downward along the Z-axis, and the wet blank remains on the forming die 2. S4: Third extrusion: The first hot-pressing upper die 3 moves along the X-axis to above the forming die 2, and the forming die 2 moves upward along the Z-axis to close with the first hot-pressing upper die 3, performing a third extrusion on the wet blank to further change the wall thickness and draft angle of the wet blank. During the mold closing process, the first hot-pressing upper die 3 blows air and the forming die 2 extracts air. During the mold separation, the forming die 2 moves downward along the Z-axis, and the forming die 2 blows air and the first hot-pressing upper die 3 extracts air, so that the wet blank is adsorbed onto the first hot-pressing upper die 3 and moves away from the forming die 2 along the X-axis with the first hot-pressing upper die 3. S5: Final Hot Press Shaping: The first hot press upper mold 3 carries the wet blank and moves along the X-axis to above the first hot press lower mold 4. The first hot press lower mold 4 moves upward along the Z-axis and closes with the first hot press upper mold 3 to perform hot press cross-linking and curing on the wet blank, completing the final shaping of the product. When separating the molds, the first hot press upper mold 3 keeps evacuating air, and the first hot press lower mold 4 moves downward along the Z-axis and blows air, so that the product remains in the first hot press upper mold 3; or, when separating the molds, the first hot press upper mold 3 keeps blowing air, and the first hot press lower mold 4 moves downward along the Z-axis and sucks air, so that the product remains in the first hot press lower mold 4.
[0020] It should be noted that in each extrusion process, the mold closing position is mechanically limited by a limiting block located on the upper or lower mold. By changing the processing depth and draft angle of each mold cavity, different cavity clearances can be obtained under the same mold closing stroke, thereby achieving a gradual decrease in wall thickness. The operation described in step S1 of this invention, which involves immersing the forming mold in pulp slurry and using vacuum suction to deposit paper fibers onto the surface of the forming mold to form a wet blank, is a conventional forming method in the field of pulp molding. The specific process conditions involved in this step, such as slurry concentration, immersion time, and vacuum degree, can be reasonably determined by those skilled in the art through limited experiments based on factors such as the wall thickness, shape, and fiber type of the target product. This invention does not impose specific limitations on these conditions, as long as a wet blank suitable for subsequent multi-pass progressive extrusion processing can be formed on the surface of the forming mold. In other words, the core improvement of this invention lies in the multi-pass progressive extrusion and hot-pressing shaping process performed after the wet blank is formed. The vacuum adsorption forming of the wet blank is itself a well-known technology in the field and will not be elaborated further.
[0021] The specific process parameters for each step of the present invention, verified by actual production lines, preferably adopt the following ranges: The holding time for the first extrusion in step S2 is 2-8 seconds; the holding time for the second extrusion in step S3 is 1.5-5 seconds; the holding time for the third extrusion in step S4 is 1.5-3 seconds; and the holding time for the final hot pressing and shaping in step S5 is 22-65 seconds. In step S3, when the top surface of the wet blank is smooth, the heating temperature of the second hot pressing upper die is 65-180℃; in step S5, the heating temperature of the first hot pressing upper die is 130-190℃, and the heating temperature of the first hot pressing lower die is 120-180℃. After one extrusion, the moisture content of the wet preform is approximately 60%-70%; after the second extrusion, the moisture content is approximately 50%-65% at room temperature, and can be reduced to 25%-45% under heated conditions; after the third extrusion, the moisture content is further reduced by approximately 2%-5% compared to the second extrusion; and after the final hot pressing, the moisture content is reduced to 5%-8%. The above parameters can be appropriately adjusted within the range given in this invention according to different product specifications, wall thicknesses, and fiber raw materials, all of which can achieve the technical effect of progressively reducing wall thickness and avoiding slurry pushing.
[0022] In step S2, the extrusion die 1 is a concave die, and the forming die 2 is a convex die. The wall thickness of the wet blank formed after the two are closed is 2.1-2.8 mm, preferably 2.5 mm. The draft angle of the inner wall of the extrusion die 1 is 1.5°-2.0°, and the draft angle of the outer wall of the forming die 2 is 0.5°-1.0°.
[0023] In step S3, the second hot-pressing upper mold 5 is a concave mold, and the forming mold 2 is a convex mold. The wall thickness of the wet blank formed after the two are closed is 1.7-2.2mm, preferably 2.0mm. The draft angle of the inner wall of the second hot-pressing upper mold 5 is 1.0°-1.6°, and the draft angle of the outer wall of the forming mold 2 is 0.5°-1.0°.
[0024] In step S4, the first hot-pressing upper mold 3 is a concave mold, and the forming mold 2 is a convex mold. The wall thickness of the wet blank formed after the two are closed is 1.2-1.6 mm, preferably 1.4 mm. The draft angle of the inner wall of the first hot-pressing upper mold 3 is 0.2°-0.3°, and the draft angle of the outer wall of the forming mold 2 is 0.5°-1.0°.
[0025] In step S5, after the first hot-pressing upper mold 3 and the first hot-pressing lower mold 4 are closed, the product wall thickness formed between them is 1mm, and the draft angle of the inner wall of the first hot-pressing upper mold 3 and the draft angle of the outer wall of the first hot-pressing lower mold 4 are both 0.2°-0.3°.
[0026] In step S3, when the top surface of the wet blank is smooth, the second hot press upper die 5 is heated and the extrusion time is extended; when the top surface of the wet blank is mesh-like, the second hot press upper die 5 is kept at room temperature.
[0027] After step S5 is completed, the receiving tray 7 is moved below the first hot press upper mold 3, and the first hot press upper mold 3 blows air to make the product fall into the receiving tray 7.
[0028] Note: The wall thickness ranges listed in steps S2-S5 (e.g., S2 is 2.1-2.8 mm) are all given proportionally based on the final finished product wall thickness of 1.0 mm. If the actual finished product wall thickness is 0.8 mm, the corresponding wall thickness in S2 should be adjusted proportionally to 1.68-2.24 mm, and so on for other steps.
[0029] Compared to the existing two-step method in pulp molding where wet blanks are directly shaped by a single hot press, this invention is based on a compact equipment layout with the forming die in the center, the extrusion die on the Y-axis side, and two sets of hot pressing dies on both sides of the X-axis. Combined with the coordinated action sequence of each die's independent reciprocating motion along the X, Y, and Z axes, this invention achieves automatic repositioning of the extrusion die and the hot pressing die during alternating operation without interference, providing space and motion assurance for multi-pass continuous production. Based on this, the present invention employs a four-stage deformation process—three progressive extrusions and one final hot pressing—to gradually reduce the wall thickness of the wet blank from 2.1-2.8 mm to 1.0 mm. Simultaneously, the invention utilizes differentiated draft angles for each stage (extrusion die 1.5°-2.0° → second hot pressing die 1.0°-1.6° → first hot pressing die 0.2°-0.3°). This ensures gradual moisture removal while preventing lateral fiber flow and accumulation caused by large single-stage deformation. This effectively solves the problem of slurry pushing during mold closing for thick-walled products with small draft angles due to a severe mismatch between the mold clearance and the wet blank wall thickness. Furthermore, the second hot pressing die can be heated to either a smooth or mesh surface during the second extrusion, allowing the wet blank surface to undergo preliminary cross-linking and pre-curing before the third extrusion. This further improves the shape retention of the wet blank in subsequent large deformation processes, reduces the probability of internal bubbles and delamination defects, and ultimately achieves high-yield and stable molding of thin-walled wallpaper products with small draft angles.
[0030] It should be noted that the reciprocating motion drive structures along the X, Y, and Z axes of the extrusion upper die 1, the first hot-pressing upper die 3, the second hot-pressing upper die 5, the forming die 2, the first hot-pressing lower die 4, and the second hot-pressing lower die 6 involved in this invention, as well as the air blowing and suction channels and their air path control systems provided inside each die, can all be implemented using drive mechanisms (such as cylinders, hydraulic cylinders, linear motors with guide rail slider mechanisms, etc.) and pneumatic control schemes known in the art. Their specific structural configurations and air path connection methods are not the core improvement of this invention, and this invention does not impose specific limitations on them, as long as the translation, lifting, air blowing, and suction switching of each die under the aforementioned spatial motion trajectory can be achieved. In other words, those skilled in the art, knowing the multi-pass progressive extrusion process steps and airflow control sequence provided by this invention, can implement it by selecting suitable known drive and pneumatic components without creative effort.
[0031] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A molding process for pulp molded products, characterized in that, It provides an extrusion upper die, a first hot pressing upper die, a second hot pressing upper die, a forming die, a first hot pressing lower die, and a second hot pressing lower die; The forming mold is disposed between the first hot pressing lower mold and the second hot pressing lower mold, the extrusion upper mold is disposed on the Y-axis side of the forming mold, and the first hot pressing upper mold and the second hot pressing upper mold are respectively disposed on both sides of the forming mold in the X-axis direction; The extrusion die is configured to reciprocate horizontally along the Y-axis; The first hot-pressing upper die and the second hot-pressing upper die are respectively configured to reciprocate horizontally along the X-axis; The forming mold, the first hot press lower mold, and the second hot press lower mold are respectively configured to move up and down along the Z-axis; In the process, when the first hot pressing upper die or the second hot pressing upper die moves along the X-axis to above the forming die, the extrusion upper die moves along the Y-axis to make way. The process includes the following steps: S1: The forming mold is immersed in the pulp slurry, and paper fibers are deposited on the surface of the forming mold by vacuum suction to form a wet blank; S2: First extrusion: The extrusion die moves along the Y-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the extrusion die, performing the first extrusion on the wet blank to initially reduce the wall thickness of the wet blank and change its draft angle. During the mold closing process, the extrusion die blows air and the forming die draws air. When the mold is separated, the forming die moves downward along the Z-axis, and the wet blank remains on the forming die. Subsequently, the extrusion die moves backward along the Y-axis to make way. S3: Second extrusion: The second hot press upper die moves along the X-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the second hot press upper die, performing a second extrusion on the wet blank. During the mold closing process, the second hot press upper die is selectively heated to cause at least partial cross-linking and pre-curing of the surface of the wet blank. During the mold closing process, the second hot press upper die blows air and the forming die evacuates air. When the mold is separated, the forming die moves downward along the Z-axis, and the wet blank remains on the forming die. S4: Third extrusion: The first hot press upper die moves along the X-axis to above the forming die, and the forming die moves upward along the Z-axis to close with the first hot press upper die, performing a third extrusion on the wet blank to further change the wall thickness and draft angle of the wet blank. During the mold closing process, the first hot press upper die blows air and the forming die draws air. During the mold separation, the forming die moves downward along the Z-axis, and the forming die blows air and the first hot press upper die draws air, so that the wet blank is adsorbed onto the first hot press upper die and moves away from the forming die along the X-axis with the first hot press upper die. S5: Final Hot Press Shaping: The first hot press upper mold carries the wet blank along the X-axis to above the first hot press lower mold. The first hot press lower mold moves upward along the Z-axis and closes with the first hot press upper mold to perform hot press cross-linking and curing on the wet blank, completing the final shaping of the product. When separating the molds, the first hot press upper mold keeps evacuating air, and the first hot press lower mold moves downward along the Z-axis and blows air, so that the product remains in the first hot press upper mold; or, when separating the molds, the first hot press upper mold keeps blowing air, and the first hot press lower mold moves downward along the Z-axis and sucks air, so that the product remains in the first hot press lower mold.
2. The molding process for a pulp molded product according to claim 1, characterized in that: In step S2, the extrusion die is a concave die and the forming die is a convex die. The wet blank formed after the two are closed has a wall thickness of 2.1-2.8 mm. The draft angle of the inner wall of the extrusion die is 1.5°-2.0° and the draft angle of the outer wall of the forming die is 0.5°-1.0°.
3. The molding process for a pulp molded product according to claim 2, characterized in that: In step S3, the second hot-pressing upper mold is a concave mold, and the forming mold is a convex mold. The wet blank formed after the two are closed has a wall thickness of 1.7-2.2 mm. The draft angle of the inner wall of the second hot-pressing upper mold is 1.0°-1.6°, and the draft angle of the outer wall of the forming mold is 0.5°-1.0°.
4. The molding process for a pulp molded product according to claim 3, characterized in that: In step S4, the first hot-pressing upper mold is a concave mold, the forming mold is a convex mold, and the wet blank formed after the two are closed has a wall thickness of 1.2-1.6 mm. The draft angle of the inner wall of the first hot-pressing upper mold is 0.2°-0.3°, and the draft angle of the outer wall of the forming mold is 0.5°-1.0°.
5. The molding process for a pulp molded product according to claim 1, characterized in that: In step S5, after the first hot-pressing upper mold and the first hot-pressing lower mold are closed, the product wall thickness formed between them is 1mm, and the draft angle of the inner wall of the first hot-pressing upper mold and the draft angle of the outer wall of the first hot-pressing lower mold are both 0.2°-0.3°.
6. The molding process for a pulp molded product according to claim 1, characterized in that: In step S3, when the top surface of the wet blank is smooth, the second hot press upper die is heated and the extrusion time is extended; when the top surface of the wet blank is mesh-like, the second hot press upper die is kept at room temperature.
7. The molding process for a pulp molded product according to claim 1, characterized in that: After step S5 is completed, the receiving tray is moved to the bottom of the first hot press upper mold, and the first hot press upper mold blows air to make the product fall into the receiving tray.