A method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values.
By using four-point bending loading and electrochemical impedance spectroscopy, the stress corrosion performance of sulfur-resistant pipes was quantified, solving the problem of evaluating stress corrosion performance in high-temperature, high-pressure sulfur-containing environments and achieving rapid and accurate assessment of stress corrosion contribution rate.
Patent Information
- Application Number
- CN202611196857.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies are insufficient to accurately evaluate the stress corrosion performance of sulfur-resistant pipes in high-temperature, high-pressure sulfur-containing environments. Furthermore, traditional methods require stringent testing conditions and cannot quickly quantify the contribution rate of stress corrosion performance.
By using a four-point bending load specimen and combining it with electrochemical AC impedance testing, the impedance values of the tensile and compressive stress loading surfaces are calculated, the stress corrosion performance index is quantified, and the contribution rate of stress to corrosion performance is evaluated.
This provides a simple and accurate method to quickly evaluate the stress corrosion performance of sulfur-resistant pipes, quantify the contribution rate of stress corrosion, and assist in early corrosion prevention and life assessment.
Smart Images

Figure CN123065882A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of stress corrosion performance detection for sulfur-resistant pipes, in particular, to a method for calculating the influence degree of applied stress on the corrosion performance of sulfur-resistant pipes based on impedance values. Background Art
[0002] Stress Corrosion Cracking (SCC) refers to the phenomenon that a metal material under tensile stress undergoes delayed fracture in certain specific media due to the synergistic effect of the corrosive medium and stress, which is one of the most common and most harmful corrosion failure modes. Even materials with excellent corrosion resistance, such as stainless steel or nickel-based alloys, cannot easily avoid stress corrosion cracking in specific service environments.
[0003] In recent years, with the exploration and development of oil and gas wells in harsh environments with ultra-depth, ultra-high temperature and ultra-high corrosion, the working conditions of oil and gas wells generally feature "high temperature, high pressure, high , high , high salinity". Due to the complex and harsh working conditions combined with special operation processes, steels for downhole and surface transmission pipelines are facing severe challenges. Especially during long-distance, high-temperature and high-pressure transmission, and in acidic well conditions containing hydrogen sulfide, steels for different transmission pipes need to withstand the combined effects of tensile stress, compressive stress, corrosion and other factors. For example, when serving in an oil field downhole, the pipe string is subjected to a certain stress due to its own weight, and the swing and vibration of the tubing cause the inclination and bending of the pipe body, which may lead to sudden stress corrosion cracking in severe cases and cause major accidents, thus affecting the normal production and operation of oil and gas fields.
[0004] At present, the four-point bending loading test in the ASTM G39 standard is generally referenced to evaluate the stress corrosion performance of sulfur-resistant pipes. The standard solution of Method A is adopted, products that do not fracture within 720 hours are qualified, and products that fracture within 720 hours are unqualified. A 10x magnifying glass is used to observe whether there are cracks on the surface of the unbroken sample. The test results can only provide information on failure and non-failure, and the test conditions are relatively harsh. For non-failed samples, further analysis combined with other additional tests is required to quantitatively evaluate the stress corrosion resistance of the non-failed samples. For example, the weight loss method is used to calculate the corrosion rate or corrosion weight loss of the bending loaded sample to assist in evaluating the stress corrosion resistance of the pipes.
[0005] Normally, when the corrosion sample is not loaded, the corrosion degree of the upper surface and the lower surface is the same, and it is approximately considered that the upper surface and the lower surface have the same contribution rate to the corrosion rate. After the corrosion sample is loaded by bending, the upper surface bears tensile stress, the lower surface bears compressive stress, and the stress states of the upper surface and the lower surface have different degrees of influence on their corrosion rates.
[0006] Electrochemistry is a commonly used method for testing the corrosion rate and corrosion resistance of materials, characterized by its simplicity, speed, and accuracy. Examples include potentiodynamic polarization curves, Tafel curves, linear polarization curves, and electrochemical impedance spectroscopy (EIS). Among these, EIS involves applying a variable-frequency, small-amplitude (typically 5mV~10mV) sinusoidal AC voltage (or current) signal as a disturbance to an electrochemical system in equilibrium or steady state, while simultaneously measuring the system's output current (or voltage) response signal. By calculating the relationship between the system's impedance value and frequency (i.e., impedance spectrum), the system's impedance value can be determined. It is an important parameter in electrochemical testing and is frequently used to evaluate the corrosion resistance of materials.
[0007] Based on the above, in order to accurately calculate the influence of bending loading stress on the corrosion resistance of sulfur-resistant pipes, and to quantify and quickly evaluate the stress corrosion resistance of sulfur-resistant pipes, this invention is proposed to evaluate the contribution ratio of stress to the corrosion resistance of sulfur-resistant pipes based on impedance values. Summary of the Invention
[0008] To address the aforementioned technical issues, a method is provided to calculate the impact of applied stress on the corrosion performance of sulfur-resistant pipes based on impedance values. This method aims to accurately evaluate the stress corrosion performance of sulfur-resistant pipes, further quantify the contribution of bending stress in a hydrogen sulfide environment to corrosion performance, analyze the influence of stress on stress corrosion fracture of pipes, solve the corrosion risk rating problem of pipe sections at bends in oil and gas pipelines, and assist in early corrosion prevention and pipeline life assessment.
[0009] A method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values includes the following steps: S1: Process the specimen to the set size, and grind and degrease the surface of the specimen; according to the nominal yield strength, use a fixture to apply a four-point bending load to the specimen at the set loading ratio; S2: Place the fixture and sample as a whole into a sealed storage tank for stress corrosion resistance test, and simultaneously conduct the first electrochemical test on the upper and lower surfaces of the sample, and record the first electrochemical data; after completing the set test cycle, conduct the second electrochemical test on the upper and lower surfaces of the unfailed sample, and record the second electrochemical data; both the first and second electrochemical tests use constant potential AC impedance testing. S3: Calculate the impedance value of the tensile stress-loaded surface in the first electrochemical test using the first electrochemical data. And the impedance value of the compressive stress-loaded surface in the first electrochemical test. The impedance value of the tensile stress-loaded surface in the second electrochemical test was calculated using the second electrochemical data. And the impedance value of the compressive stress-loaded surface in the second electrochemical test. The stress corrosion performance index, the contribution rate of bending loading tensile stress to the corrosion resistance of sulfur-containing pipes, and the contribution rate of bending loading compressive stress to the corrosion resistance of sulfur-containing pipes were calculated. The stress corrosion performance index The calculation formula is:
[0010]
[0011] in, The value of is related to the polarization resistance of the sample surface, and the range is 0.5~1. The contribution rate of the bending loading tensile stress to the corrosion resistance of sulfur pipes The calculation formula is:
[0012] in, For loading ratio, The stress corrosion resistance index for sulfur-resistant pipes; The contribution rate of the bending loading compressive stress to the corrosion resistance of sulfur pipes The calculation formula is:
[0013] in, For loading ratio, The stress corrosion resistance index is used for sulfur-resistant pipe materials.
[0014] Furthermore, the dimensions set in S1 are 100~120mm in length, 10~20mm in width, and 3~6mm in thickness.
[0015] Furthermore, the polishing and degreasing process in S1 includes the following steps: First, remove the burrs from the edge of the sample and polish the sample evenly with sandpaper; then clean the sample twice in acetone using an ultrasonic cleaner; finally, clean the sample once with anhydrous ethanol.
[0016] Furthermore, the protruding part between the two inner supports on the specimen is defined as the upper surface of the specimen, and the concave part corresponding to the upper surface of the specimen is defined as the lower surface of the specimen; the four-point bending loading ensures that uniform longitudinal tensile stress and compressive stress are generated on the upper and lower surfaces of the specimen, respectively, and the stress linearly decreases to zero from the inner support to the outer support on the specimen.
[0017] Furthermore, the loading ratio set in S1 is 50% to 80% of the nominal yield strength; the test period set in S2 is 360 to 720 hours.
[0018] Furthermore, the test solutions for both the first and second electrochemical tests are 5% sodium chloride solutions containing sulfur, with a pH value of 2 ≤ pH ≤ 6; the sulfur is in a gaseous state. and Any one of them, or any one of solid sodium sulfide and thiourea, or and The mixture of any one of the following is a mixture of sodium sulfide and thiourea; the first and second electrochemical tests both use a three-electrode system, with applied potentials of ±10mV and scanning frequencies ranging from 0.1Hz to 10KHz.
[0019] Compared with the prior art, the present invention has the following advantages: This invention conducts electrochemical tests on bending-loaded specimens. By measuring the impedance values of the tensile stress-loaded surface and the compressive stress-loaded surface, the stress corrosion performance index of sulfur-resistant pipes is calculated. By analyzing the correlation between impedance values and corrosion rates, the influence and contribution rate of the loading stress in the hydrogen sulfide environment on the corrosion performance of the loaded specimens are quantified. This provides a theoretical basis for elucidating the control mechanism of stress corrosion cracking in sulfur-resistant pipes and improving their SCC resistance. This invention is simple to operate and produces accurate measurement results. Attached Figure Description
[0020] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0021] Figure 1 This is an overall flowchart of the method of the present invention for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values; Figure 2 This is a structural diagram of the fixture and sample in this invention under four-point bending loading. Figure 3 This is the first AC impedance curve of the loaded sample in Example 1 of the present invention; Figure 4 This is the second AC impedance curve of the loaded sample in Example 1 of the present invention; Reference numerals: 1-sample; 2-clamp; 101-inner fulcrum; 102-outer fulcrum. Detailed Implementation
[0022] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.
[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0024] Example 1: like Figures 1 to 4 As shown, the method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values includes the following steps: S1: Process the specimen 1 to the set size, and grind and degrease the surface of the specimen 1; according to the nominal yield strength, use the fixture 2 to apply a four-point bending load to the specimen 1 at the set loading ratio. S2: Place the fixture 2 and the sample 1 into a sealed storage tank for stress corrosion resistance test, and simultaneously conduct the first electrochemical test on the upper and lower surfaces of the sample 1, and record the first electrochemical data; after completing the set test cycle, conduct the second electrochemical test on the upper and lower surfaces of the unfailed sample 1, and record the second electrochemical data; both the first and second electrochemical tests use constant potential AC impedance testing. S3: Calculate the impedance value of the tensile stress-loaded surface in the first electrochemical test using the first electrochemical data. And the impedance value of the compressive stress-loaded surface in the first electrochemical test. The impedance value of the tensile stress-loaded surface in the second electrochemical test was calculated using the second electrochemical data. And the impedance value of the compressive stress-loaded surface in the second electrochemical test. ; Calculate the stress corrosion performance index and the contribution rate of bending loading tensile stress to the corrosion resistance of sulfur pipes; The stress corrosion performance index The calculation formula is:
[0025]
[0026] in, The value of is related to the polarization resistance of the surface of sample 1, and the value range is 0.5~1; The contribution rate of the bending loading tensile stress to the corrosion resistance of sulfur pipes The calculation formula is:
[0027] in, For loading ratio, The stress corrosion resistance index is used for sulfur-resistant pipe materials.
[0028] The contribution rate of the bending loading compressive stress to the corrosion resistance of sulfur pipes The calculation formula is:
[0029] in, For loading ratio, The stress corrosion resistance index is used for sulfur-resistant pipe materials.
[0030] Specifically, the test period set in S2 is 360~720h to ensure that sample 1 does not fail within the test period.
[0031] In this embodiment, the dimensions set in S1 are 100~120mm in length, 10~20mm in width, and 3~6mm in thickness.
[0032] In this embodiment, the polishing and degreasing process in S1 includes the following steps: First, remove the burrs from the edge of sample 1 and polish sample 1 evenly with sandpaper; then clean sample 1 twice in acetone using an ultrasonic cleaner; finally, clean sample 1 once with anhydrous ethanol.
[0033] In this embodiment, the protruding part between the two inner support points 101 on the sample 1 is defined as the upper surface of the sample 1, and the concave part corresponding to the upper surface of the sample 1 is defined as the lower surface of the sample 1. The four-point bending loading ensures that the upper and lower surfaces of the sample 1 generate uniform longitudinal tensile stress and compressive stress, respectively. From the inner support point 101 to the outer support point 102 on the sample 1, the stress linearly decreases to zero.
[0034] In this embodiment, the loading ratio set in S1 is 50% to 80% of the nominal yield strength.
[0035] In this embodiment, the test solutions for the first and second electrochemical tests are both 5% sodium chloride solutions containing sulfur, with a pH value of 2 ≤ 6.
[0036] Specifically, sulfur can be in a gaseous state. , It may be a solid form such as sodium sulfide or thiourea, or a mixture of a gaseous and a solid substance.
[0037] In this embodiment, both the first and second electrochemical experiments used a three-electrode system, with applied potentials of ±10mV and scanning frequencies ranging from 0.1Hz to 10KHz.
[0038] Specifically, the impedance value is the impedance modulus corresponding to the minimum frequency, indicating the reaction resistance of the corrosion system. It is inversely proportional to the corrosion current (i.e., the corrosion rate) and directly proportional to the corrosion resistance. > , > .
[0039] In this embodiment, the method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values consists of four steps: sample preparation (step a), surface treatment (step b), bending loading and electrochemical testing (step c), and calculation of test results (step d).
[0040] In step a, sample 1 is processed to a size of 115mm. 15mm 5mm; In step b, first remove the edge burrs, then polish with 2000# sandpaper to achieve a surface finish of 0.3μm, and then clean with acetone twice and anhydrous ethanol once in the ultrasonic process. In step c, the bending loading test employs a four-point bending loading method, applying a load of 50% of the nominal yield strength of the well pipe. After loading, sample 1 and fixture 2 are placed as a whole into a sealed storage tank for stress corrosion resistance testing. The test solution is solution A (NACE standard) containing 1000 ppm hydrogen sulfide, pH=3. The first electrochemical test is also conducted simultaneously on both the upper and lower surfaces, and the first electrochemical data is recorded. The AC impedance curve is shown in [reference needed]. Figure 3 When the minimum frequency is 0.1Hz, the impedance value of the tensile stress-loaded surface is obtained. =2436Ω.cm 2 The impedance value of the compressive stress loading surface =2538Ω·cm², after 720h of testing, a second electrochemical test was conducted simultaneously on the upper and lower surfaces of the unfailed sample 1, and the second electrochemical data were recorded. The AC impedance curve is shown in [reference needed]. Figure 4 When the minimum frequency is 0.1Hz, the impedance value of the tensile stress-loaded surface is obtained. =2143Ω.cm 2 The impedance value of the compressive stress loading surface =2298Ω.cm2; In the calculation of the test results in step d, the K value is taken as 0.90, based on the stress corrosion performance index. The calculation formula and the contribution rate of bending loading tensile stress to the corrosion resistance of sulfur-containing pipes. The calculation formula and the contribution rate of bending loading compressive stress to the corrosion resistance of sulfur pipes. The calculation formula yields a stress corrosion performance index r = 0.73, indicating the contribution rate of tensile stress under bending load to the corrosion resistance of sulfur-resistant pipes. =35.29%, the contribution rate of bending loading compressive stress to the corrosion resistance of sulfur-resistant pipes =32.91%.
[0041] Therefore, it can be seen that when the loading ratio is 50%, the stress corrosion performance index of the sulfur-resistant pipe is 0.73, and the stress performance against hydrogen sulfide is good. The contribution rate of bending loading tensile stress to the corrosion performance of the sulfur-resistant pipe is 35.29%, and the contribution rate of bending loading compressive stress to the corrosion performance of the sulfur-resistant pipe is 32.91%.
[0042] Example 2: The data results under the test environment of 5% NaCl containing sodium sulfide and pH=3 are shown in the table below:
[0043] The above test results show that when the loading ratio is 80% and the test period is 720h, the stress corrosion performance index of the sulfur-resistant pipe is 0.68, the contribution rate of bending loading tensile stress to the corrosion performance of the sulfur-resistant pipe is 61.56%, and the contribution rate of bending loading compressive stress to the corrosion performance of the sulfur-resistant pipe is 56.38%.
[0044] Example 3: The data results under the test environment of thiourea-containing 5% NaCl pH=6 are shown in the table below:
[0045] The above test results show that when the loading ratio is 80% and the test period is 720h, the stress corrosion performance index of the sulfur-resistant pipe is 0.72, the contribution rate of bending loading tensile stress to the corrosion performance of the sulfur-resistant pipe is 58.08%, and the contribution rate of bending loading compressive stress to the corrosion performance of the sulfur-resistant pipe is 52.87%.
[0046] Further analysis of the above experimental results reveals that, under the same loading ratio, the r-value is smaller in the 5% NaCl solution containing sodium sulfide (pH=3), while the r-value is larger in the 5% NaCl solution containing thiourea (pH=6). The lower pH indicates a more demanding testing environment, resulting in a lower stress corrosion performance index and a greater influence and contribution of loading stress on corrosion performance. Under the same pH conditions, as the loading ratio and test period increase, the r-value decreases, the stress corrosion performance of the sulfur-resistant pipe decreases, and the proportion and contribution of loading stress to the corrosion performance of the sulfur-resistant pipe increase.
[0047] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values, characterized in that, Includes the following steps: S1: Process the specimen (1) to the set size, grind and degrease the surface of the specimen (1); according to the nominal yield strength, use the fixture (2) to perform a four-point bending load on the specimen (1) at the set loading ratio; S2: Place the fixture (2) and the sample (1) into a sealed storage tank for stress corrosion resistance test, and conduct the first electrochemical test on the upper and lower surfaces of the sample (1) at the same time, and record the first electrochemical data; after completing the set test cycle, conduct the second electrochemical test on the upper and lower surfaces of the unfailed sample (1) at the same time, and record the second electrochemical data; the first electrochemical test and the second electrochemical test are both conducted using constant potential AC impedance testing; S3: Calculate the impedance value of the tensile stress-loaded surface in the first electrochemical test using the first electrochemical data. And the impedance value of the compressive stress-loaded surface in the first electrochemical test. ; The impedance value of the tensile stress-loaded surface in the second electrochemical test was calculated using the second electrochemical data. And the impedance value of the compressive stress-loaded surface in the second electrochemical test. ; The stress corrosion performance index, the contribution rate of bending loading tensile stress to the corrosion performance of sulfur-containing pipes, and the contribution rate of bending loading compressive stress to the corrosion performance of sulfur-containing pipes were calculated. The stress corrosion performance index The calculation formula is: in, The value of is related to the polarization resistance of the surface of the sample (1), and the value range is 0.5~1; The contribution rate of the bending loading tensile stress to the corrosion resistance of sulfur pipes The calculation formula is: in, For loading ratio, The stress corrosion resistance index for sulfur-resistant pipes; The contribution rate of the bending loading compressive stress to the corrosion resistance of sulfur pipes The calculation formula is: in, For loading ratio, The stress corrosion resistance index is used for sulfur-resistant pipe materials.
2. The method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values according to claim 1, characterized in that, The dimensions set in S1 are 100-120mm in length, 10-20mm in width, and 3-6mm in thickness.
3. The method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values according to claim 1, characterized in that, The polishing and degreasing process in S1 includes the following steps: First, remove the burrs from the edge of the sample (1) and polish the sample (1) evenly with sandpaper; then clean the sample (1) twice in acetone using an ultrasonic cleaner; finally, clean the sample (1) once with anhydrous ethanol.
4. The method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values according to claim 1, characterized in that, The protruding part between the two inner support points (101) on the specimen (1) is defined as the upper surface of the specimen (1), and the concave part corresponding to the upper surface of the specimen (1) is defined as the lower surface of the specimen (1). The four-point bending load ensures that uniform longitudinal tensile stress and compressive stress are generated on the upper and lower surfaces of the specimen (1), respectively, and the stress linearly decreases to zero from the inner support (101) to the outer support (102) on the specimen (1).
5. The method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values according to claim 1, characterized in that, The loading ratio set in S1 is 50% to 80% of the nominal yield strength; the test period set in S2 is 360 to 720 hours.
6. The method for calculating the influence of applied stress on the corrosion resistance of sulfur-resistant pipes based on impedance values according to claim 1, characterized in that, The test solutions for both the first and second electrochemical tests were 5% sodium chloride solutions containing sulfur, with a pH value of 2 ≤ 6; the sulfur was in a gaseous state. and Any one of them, or any one of solid sodium sulfide and thiourea, or and Any one of them can be mixed with any one of sodium sulfide and thiourea; Both the first and second electrochemical experiments used a three-electrode system, with applied potentials of ±10mV and scanning frequencies ranging from 0.1Hz to 10KHz.