Thin film lithium niobate end-coupler and method of making same
By spin-coating photoresist onto the surface of a thin-film lithium niobate chip and fabricating a three-dimensional polymer waveguide using femtosecond laser two-photon polymerization technology, the mode field mismatch problem of the thin-film lithium niobate end-face coupler was solved, achieving low-loss, high-efficiency fiber optic connection and broadening the operating bandwidth.
Patent Information
- Application Number
- CN202611550132.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to achieve high-efficiency coupling performance in thin-film lithium niobate end-face couplers, resulting in issues such as mode-field mismatch, high coupling loss, and complex processes.
A negative photoresist layer with a thickness of not less than 12 μm is spin-coated on the surface of a thin-film lithium niobate chip using femtosecond laser two-photon polymerization technology. The layer is then directly written onto the lithium niobate waveguide to form a three-dimensional polymer waveguide, which undergoes mode field thermal evolution. Finally, the waveguide is developed, cured, and cut and polished to achieve docking with a standard single-mode fiber.
The coupling performance of the thin-film lithium niobate end coupler was improved, the coupling loss was reduced, the operating bandwidth was broadened, the fiber alignment tolerance was improved, and the packaging difficulty was reduced.
Smart Images

Figure CN123066918A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of optical communication technology, and in particular to a thin-film lithium niobate end-face coupler and its fabrication method. Background Technology
[0002] Thin-film lithium niobate materials possess advantages such as wide transparency windows, strong electro-optic effects, and high nonlinear coefficients, making them an important integrated photonic platform for fabricating high-performance electro-optic modulators and quantum light sources. To achieve high-density integration of photonic devices, thin-film lithium niobate waveguides are typically fabricated to sub-micron cross-sectional dimensions. The mode field size of these waveguides is much smaller than that of standard single-mode optical fibers, resulting in a severe mode field mismatch that leads to significant coupling losses and limits the practical application of these devices.
[0003] Existing technologies have developed various coupling schemes, such as grating couplers and edge coupling. Among them, grating couplers, although supporting wafer-level testing, suffer from drawbacks such as narrow operating bandwidth and polarization sensitivity; traditional edge coupling relies solely on lithium niobate reverse cones to extend modes, making it difficult to evolve large-size mode spots that match single-mode fibers; and multilayer polymer stacking processes require multiple spin coatings and step-by-step photolithography, resulting in complex procedures, poor interlayer alignment accuracy, and a tendency to generate scattering interfaces, making it impossible to achieve ideal adiabatic mode transitions. All existing schemes have different shortcomings, making it difficult to obtain end-face coupling devices with excellent coupling performance.
[0004] Therefore, how to improve the coupling performance of thin-film lithium niobate end couplers is a problem that urgently needs to be solved by those skilled in the art. Summary of the Invention
[0005] To address the aforementioned issues, this application provides a thin-film lithium niobate end-face coupler and its fabrication method. By integrally forming a layered interface, scattering loss is reduced, the operating bandwidth is broadened, and the coupling performance of the thin-film lithium niobate end-face coupler is improved.
[0006] In a first aspect, embodiments of this application provide a method for fabricating a thin-film lithium niobate end-face coupler, comprising: A thin-film lithium niobate chip is provided; the surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide with an inverted cone structure; the tip of the inverted cone structure points to the coupling end face of the thin-film lithium niobate chip; A negative photoresist is spin-coated onto the surface of the thin-film lithium niobate chip to form a photoresist layer with a thickness of not less than 12 μm; The photoresist layer is three-dimensionally written using femtosecond laser two-photon polymerization technology to integrally form a three-dimensional polymer waveguide with continuously changing morphology above the lithium niobate waveguide. The transverse cross-sectional dimensions and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face. This is used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode pattern that matches a standard single-mode fiber. The first dimension is smaller than the second dimension. The photoresist layer is developed, and the three-dimensional polymer waveguide is cured. The coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with the standard single-mode optical fiber.
[0007] Optionally, the three-dimensional direct writing of the photoresist layer using femtosecond laser two-photon polymerization technology includes: As the scanning position moves toward the coupling end face, the output power of the laser is increased linearly or nonlinearly, and the Z-axis focusing depth of the femtosecond laser is adjusted simultaneously.
[0008] Optionally, the first size is 2 μm to 6 μm, and the second size is 8 μm to 16 μm.
[0009] Optionally, the length of the transition section of the three-dimensional polymer waveguide is not less than 300 μm.
[0010] Optionally, the width of the tip of the inverted cone structure is 80 nm to 150 nm.
[0011] Optionally, the curing temperature is between 150°C and 250°C.
[0012] Optionally, the cutting and polishing of the coupling end face of the thin-film lithium niobate chip includes: The coupling end face of the thin-film lithium niobate chip is cut using a diamond cutting wheel, and the coupling end face is polished using an abrasive medium with a particle size of 0.1μm to 1μm.
[0013] Secondly, embodiments of this application provide a thin-film lithium niobate end-face coupler, comprising: Thin-film lithium niobate chip and three-dimensional polymer waveguide; The surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide with an inverted cone structure, the tip of which points towards the coupling end face of the thin-film lithium niobate chip. The three-dimensional polymer waveguide is integrally formed on top of the lithium niobate waveguide. The transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face. This is used to perform adiabatic evolution of the mode field of the lithium niobate waveguide to obtain a mode pattern that matches that of a standard single-mode fiber. The first dimension is smaller than the second dimension. The end section of the three-dimensional polymer waveguide is exposed on the coupling end face to interface with the standard single-mode fiber.
[0014] Optionally, the first size is 2 μm to 6 μm, and the second size is 8 μm to 16 μm.
[0015] Optionally, the length of the transition section of the three-dimensional polymer waveguide is not less than 300 μm.
[0016] As can be seen from the above technical solutions, compared with the prior art, this application has the following advantages: This application provides a method for fabricating a thin-film lithium niobate end-face coupler. First, a thin-film lithium niobate chip is provided, and a negative photoresist is spin-coated onto the surface of the thin-film lithium niobate chip to form a photoresist layer with a thickness of not less than 12 μm. A lithium niobate waveguide with an inverted cone structure is disposed on the surface of the thin-film lithium niobate chip; the tip of the inverted cone structure points towards the coupling end face of the thin-film lithium niobate chip. Then, femtosecond laser two-photon polymerization technology is used to perform three-dimensional direct writing on the photoresist layer, integrally forming a three-dimensional polymer waveguide with continuously changing morphology above the lithium niobate waveguide. The transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the lithium niobate waveguide end along the propagation direction to a second dimension near the coupling end face, used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode spot matching a standard single-mode fiber; the first dimension is smaller than the second dimension. Finally, the photoresist layer is developed, and the three-dimensional polymer waveguide is cured. Finally, the coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with a standard single-mode fiber. Thus, by spin-coating a negative photoresist layer with a thickness of not less than 12 μm onto the surface of the thin-film lithium niobate chip, and using femtosecond laser two-photon polymerization technology to directly write and integrally form a three-dimensional polymer waveguide with continuously changing morphology, the mode field of the lithium niobate waveguide can be adiabatically evolved using this waveguide, resulting in a mode pattern matching that of a standard single-mode fiber. After development, curing, and cutting and polishing of the coupling end face, fiber docking is achieved, improving the coupling performance of the thin-film lithium niobate end face coupler. Attached Figure Description
[0017] Figure 1 A flowchart illustrating a method for fabricating a thin-film lithium niobate end-face coupler provided in this application embodiment; Figure 2 A process flow diagram for fabricating a thin-film lithium niobate end-face coupler provided in this application embodiment; Figure 3 This is a schematic diagram of a thin-film lithium niobate end-face coupler provided in an embodiment of this application. Detailed Implementation
[0018] As mentioned earlier, existing technologies struggle to produce thin-film lithium niobate end-face couplers with excellent coupling performance. Specifically, existing technologies have developed various coupling schemes, such as grating couplers and edge coupling. While grating couplers support wafer-level testing, they suffer from narrow operating bandwidth and polarization sensitivity. Traditional edge coupling relies solely on the reverse cone of lithium niobate to extend modes, making it difficult to evolve large-size mode spots that match single-mode fibers. Furthermore, multilayer polymer stacking processes require multiple spin coatings and step-by-step photolithography, resulting in complex procedures, poor interlayer alignment accuracy, and a tendency to generate scattering interfaces, making it impossible to achieve ideal adiabatic mode transitions. Each existing solution has its own shortcomings, making it difficult to obtain thin-film lithium niobate end-face couplers with excellent coupling performance.
[0019] To address the aforementioned issues, this application provides a method for fabricating a thin-film lithium niobate end-face coupler. First, a thin-film lithium niobate chip is provided, and a negative photoresist is spin-coated onto the surface of the chip to form a photoresist layer with a thickness of not less than 12 μm. A lithium niobate waveguide with an inverted cone structure is disposed on the surface of the thin-film lithium niobate chip; the tip of the inverted cone structure points towards the coupling end face of the chip. Then, femtosecond laser two-photon polymerization technology is used to perform three-dimensional direct writing on the photoresist layer, integrally forming a three-dimensional polymer waveguide with continuously varying morphology above the lithium niobate waveguide. The lateral cross-sectional dimensions and vertical height of the three-dimensional polymer waveguide smoothly transition from a first dimension near the lithium niobate waveguide end along the propagation direction to a second dimension near the coupling end face, used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode pattern matching a standard single-mode fiber; the first dimension is smaller than the second dimension. Finally, the photoresist layer is developed, and the three-dimensional polymer waveguide is cured. Finally, the coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with standard single-mode optical fiber.
[0020] Thus, by spin-coating a negative photoresist layer with a thickness of not less than 12 μm onto the surface of a thin-film lithium niobate chip, and using femtosecond laser two-photon polymerization technology to directly write and integrally form a three-dimensional polymer waveguide with continuously changing morphology, the mode field of the lithium niobate waveguide can be adiabatically evolved by relying on this waveguide, and a mode spot matching the standard single-mode fiber can be obtained. After development, curing, and cutting and polishing of the coupling end face, fiber docking is achieved, which improves the coupling performance of the thin-film lithium niobate end face coupler.
[0021] It should be noted that the thin-film lithium niobate end-face coupler and its fabrication method provided in this application can be applied to the field of optical communication technology. The above are merely examples and do not limit the application field of the thin-film lithium niobate end-face coupler and its fabrication method provided in this application.
[0022] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0023] Figure 1 This is a flowchart illustrating a method for fabricating a thin-film lithium niobate end-face coupler, as provided in an embodiment of this application. (Combined with...) Figure 1 As shown in the embodiments of this application, a method for fabricating a thin-film lithium niobate end-face coupler may include: S101: Provides a thin-film lithium niobate chip; the surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide with an inverted cone structure; the tip of the inverted cone structure points to the coupling end face of the thin-film lithium niobate chip.
[0024] Furthermore, the width of the tip of the inverted cone structure is 80 nm to 150 nm.
[0025] In practical applications, thin-film lithium niobate chips are provided first. Figure 2 This document provides a process flow diagram for the fabrication of a thin-film lithium niobate end-face coupler, as illustrated in an embodiment of this application. Figure 2 As shown, this thin-film lithium niobate chip is fabricated based on a lithium niobate on insulator (LNOI) wafer, which consists of a silicon substrate 100, a silicon dioxide buried oxide layer 200, and a thin-film lithium niobate layer 300 from bottom to top. Figure 2 As shown in Figure a, the thin-film lithium niobate layer 300 is first processed by electron beam lithography or deep ultraviolet lithography to form a patterned photoresist mask 400 on the surface of the thin-film lithium niobate layer 300, defining the lithium niobate waveguide and the inverted cone pattern. Then, an etching process is performed to remove the portion of the thin-film lithium niobate layer 300 not covered by the photoresist mask 400, thereby fabricating a lithium niobate (ridge) waveguide 310 with an inverted cone structure on the thin-film lithium niobate layer 300, as shown in Figure a. Figure 2As shown in b, the tip of the inverted cone structure faces the coupling end face formed by the subsequent cutting and polishing of the chip. Furthermore, the tip width of the inverted cone structure is set to 80nm to 150nm. Because the waveguide core of this inverted cone structure continuously narrows along the light propagation direction, the confinement effect on the light field gradually weakens, and the light transmitted inside the lithium niobate waveguide 310 diffuses outward to form an evanescent light field. Limiting the cone tip width to the range of 80nm-150nm allows the light field in the lithium niobate waveguide 310 to fully diffuse outward, facilitating efficient coupling of light into the subsequently formed three-dimensional polymer waveguide 510, and reducing mode coupling loss during the transition of light from the lithium niobate waveguide 310 to the polymer waveguide. If the tip width is designed to be too large, the waveguide's ability to confine light will remain very strong, making it difficult for the light field to escape and efficiently enter the upper-layer 3D polymer waveguide 510. If the tip width is designed to be too small, it will significantly increase the difficulty of photolithography patterning and etching, making the tip prone to breakage and morphological defects, thus reducing device yield. Therefore, a tip width of 80nm to 150nm ensures both high optical field coupling efficiency and feasibility for practical micro-nano fabrication, guaranteeing the stable progress of the subsequent mode field adiabatic evolution process.
[0026] S102: Spin-coat a negative photoresist onto the surface of the thin-film lithium niobate chip to form a photoresist layer with a thickness of not less than 12 μm.
[0027] In practical applications, after fabricating the thin-film lithium niobate chip and the reverse cone-shaped lithium niobate waveguide 310, a negative photoresist needs to be spin-coated onto the surface of the thin-film lithium niobate chip at a low speed (e.g., 1000–2000 rpm) to form a photoresist layer 500 with a thickness of not less than 12 μm. Figure 2 As shown in c in the figure. Figure 2Figures a, b, and c in the diagram are side cross-sectional views of the structure perpendicular to the light propagation direction. This embodiment uses SU-8 series negative photoresist. It is understood that subsequent femtosecond laser two-photon polymerization 3D direct writing requires the fabrication of a continuously changing morphology 3D polymer waveguide 510 within the photoresist layer 500. If the photoresist layer thickness is less than 12 μm, the longitudinal space of the layer will be limited, failing to provide sufficient height, making it difficult to fabricate a polymer waveguide with a sufficiently large vertical end dimension, and thus failing to obtain a mode spot matching the standard single-mode fiber. The standard single-mode fiber referred to in this embodiment can be SMF-28, with a mode field diameter of approximately 10.4 μm at a wavelength of 1550 nm. Setting the photoresist layer 500 thickness to not less than 12 μm provides sufficient longitudinal processing space for the subsequently formed 3D gradient structure of the polymer waveguide 510, ensuring that the lateral cross-sectional dimensions and vertical height of the 3D polymer waveguide 510 can smoothly grow from the first dimension to the second dimension, meeting the structural requirements for adiabatic evolution of the mode field and ensuring that the light field can fully complete mode conversion. Meanwhile, by using negative photoresist such as SU-8, the resulting polymer structure, after subsequent development and curing, exhibits high mechanical strength and good anti-aging properties, which helps improve the overall structural reliability of the end-face coupler.
[0028] After this, before performing three-dimensional direct writing on the photoresist layer 500 using femtosecond laser two-photon polymerization technology, the photoresist layer 500 can be pre-baked with a multi-level temperature gradient, such as holding at 65 degrees Celsius for 5 minutes and gradually increasing the temperature to 95 degrees Celsius for 10 minutes, to ensure the release of internal stress in the photoresist layer.
[0029] S103: Using femtosecond laser two-photon polymerization technology, the photoresist layer is three-dimensionally written directly to integrally form a three-dimensional polymer waveguide with continuously changing morphology above the lithium niobate waveguide; the transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face, which is used to perform adiabatic evolution of the mode field of the lithium niobate waveguide to obtain a mode spot that matches a standard single-mode fiber; the first dimension is smaller than the second dimension.
[0030] Furthermore, the first size is 2μm to 6μm, and the second size is 8μm to 16μm; The length of the transition section of the three-dimensional polymer waveguide is not less than 300 μm.
[0031] In practical applications, after preparing a negative photoresist layer 500 with a thickness of not less than 12 μm, three-dimensional direct writing processing of the photoresist layer 500 is performed using femtosecond laser two-photon polymerization technology. This results in the integral formation of a three-dimensional polymer waveguide 510 with continuously varying morphology above the lithium niobate waveguide 310, such as... Figure 2 As shown in d and e. Figure 2In the diagram, d and e represent side cross-sectional views of the structure along the light propagation direction. The transverse cross-sectional dimensions and vertical height of the three-dimensional polymer waveguide 510 smoothly and gradually increase from a first dimension near the end of the lithium niobate waveguide 310 along the light propagation direction, transitioning to a second dimension near the coupling end face M, where the first dimension is smaller than the second dimension. This gradient structure allows for adiabatic evolution of the mode field of the lithium niobate waveguide 310, ultimately yielding a mode pattern that matches that of a standard single-mode fiber. Furthermore, the first dimension is set to 2μm to 6μm, the second dimension to 8μm to 16μm, and the length of the transition section L of the three-dimensional polymer waveguide 510 is set to be no less than 300μm. In other words, the lateral cross-sectional dimension and vertical height of the three-dimensional polymer waveguide 510 located near the lithium niobate waveguide 310 in this application are both 2μm to 6μm, and they can be equal or unequal, but are usually equal. Similarly, the lateral cross-sectional dimension and vertical height of the three-dimensional polymer waveguide 510 located near the coupling end face M are both 8μm to 16μm, and they can also be equal or unequal, but are usually equal. Thus, based on the three-dimensional direct-write process using femtosecond laser two-photon polymerization, a complete three-dimensional polymer waveguide 510 can be integrally formed within the photoresist layer 500 without multiple photolithography stacking and overlay processes. The formed three-dimensional polymer waveguide 510 is continuous as a whole, without any layered interfaces, thus avoiding light scattering loss caused by multi-layer processing. The first dimension is set to 2μm-6μm, which can adapt to the light field output by the lithium niobate reverse cone, allowing light to efficiently couple from the lithium niobate waveguide 310 into the three-dimensional polymer waveguide 510. If the first dimension is too small, it will reduce the efficiency of optical coupling into the polymer waveguide; if the first dimension is too large, it will easily excite higher-order hybrid modes, interfering with the normal transmission of the fundamental mode light. The second dimension at the end is controlled between 8μm and 16μm, allowing the mode spot size at the output end of the 3D polymer waveguide 510 to match the mode spot size of a standard single-mode fiber, improving the overlap of their optical fields, reducing coupling loss during fiber splicing, increasing alignment tolerance during fiber assembly, reducing device packaging difficulty, and enabling the overlap integral between the fundamental mode of the 3D polymer waveguide 510 and the SMF-28 fiber to reach over 98%. Furthermore, setting the length L of the transition section to no less than 300μm ensures that the width and height changes of the 3D polymer waveguide 510 are sufficiently gradual, meeting the conditions for adiabatic evolution of the mode field, suppressing the generation of higher-order modes and light leakage loss, and ensuring stable forward transmission of light in the fundamental mode. If the length L of the transition section is too short, the waveguide morphology changes too rapidly, disrupting the adiabatic evolution conditions, exciting higher-order modes, and introducing additional coupling loss.As can be seen, by reasonably setting the first dimension, the second dimension, and the length of the transition section L, this application allows the three to work together to ensure that light can be efficiently transferred from the lithium niobate waveguide to the polymer waveguide, and to achieve stable mode field adiabatic evolution, outputting a mode spot that is compatible with standard single-mode fiber, thus obtaining a low-loss, broadband-operable end-coupled device.
[0032] Furthermore, since there are different ways to perform three-dimensional direct writing, this application embodiment can describe one possible three-dimensional direct writing method.
[0033] In one instance, the three-dimensional direct writing of the photoresist layer using femtosecond laser two-photon polymerization technology includes: As the scanning position moves toward the coupling end face, the output power of the laser is increased linearly or nonlinearly, and the Z-axis focusing depth of the femtosecond laser is adjusted simultaneously.
[0034] In practical applications, when using femtosecond laser two-photon polymerization technology for 3D direct writing, a microscopic imaging system can be used to locate the tip of the lithium niobate reverse cone. As the laser scanning position moves towards the coupling end face M, the output power of the laser needs to be increased linearly or nonlinearly, while simultaneously adjusting the Z-axis focusing depth of the femtosecond laser. Specifically, the size of the area where the femtosecond laser irradiates the photoresist layer 500 to produce polymerization is affected by both the laser output power and the Z-axis focusing depth: the laser power determines the lateral polymerization range of the photoresist layer 500; the Z-axis focusing depth controls the polymerization position of the photoresist layer 500 in the thickness direction. By adjusting the laser output power and the Z-axis focusing depth in a linked manner, the curing cross-sectional size of the polymer at various locations can be changed in real time during laser scanning, thereby directly fabricating a 3D polymer waveguide 510 with smooth lateral and vertical height variations, without the need for masks or multi-layer step-by-step photolithography. Thus, by introducing femtosecond laser two-photon polymerization as a processing method, linear or nonlinear gradient profiles can be flexibly achieved, ensuring the continuous morphology of the three-dimensional polymer waveguide 510 without steps or abrupt changes. If only the laser power is adjusted without adjusting the Z-axis focusing depth, a continuous gradient in the waveguide's vertical height cannot be achieved, making it difficult to obtain a qualified three-dimensional gradient waveguide. This solution, by introducing femtosecond laser two-photon polymerization technology, ensures that the fabricated three-dimensional polymer waveguide 510 meets the adiabatic evolution conditions of the mode field, suppresses the generation of higher-order modes, and reduces coupling loss.
[0035] S104: The photoresist layer is developed and the three-dimensional polymer waveguide is cured.
[0036] Furthermore, the curing temperature is between 150°C and 250°C.
[0037] In practical applications, after completing femtosecond laser two-photon polymerization 3D direct writing, the photoresist layer 500 is developed, and the 3D polymer waveguide 510 is cured. The curing temperature is between 150℃ and 250℃. It's understandable that after femtosecond laser direct writing exposure, only the areas irradiated by the laser undergo polymerization, forming the initial shape of the 3D polymer waveguide 510; the remaining areas remain unpolymerized photoresist. Developing dissolves and removes this unpolymerized photoresist, fully exposing the formed 3D polymer waveguide 510. Curing is then carried out at a temperature of 150℃-250℃ to further enhance the cross-linking degree between polymer molecules. If the curing temperature is too low, the cross-linking reaction is insufficient, resulting in a soft polymer waveguide with poor mechanical stability; if the curing temperature is too high, the polymer is prone to thermal deformation, altering the original gradient shape of the waveguide. This application limits the curing temperature to 150℃ to 250℃, which can not only fully enhance the hardness and anti-aging ability of the three-dimensional polymer waveguide 510, but also prevent the waveguide from deforming due to heat, preserve the original optical structure of the waveguide, and ensure the normal thermal evolution of the mode field.
[0038] S105: The coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with the standard single-mode optical fiber.
[0039] In practical applications, after development and curing, the coupling end face M of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide 510 on the coupling end face M for docking with standard single-mode optical fiber. Understandably, after the previous processing steps, the end of the three-dimensional polymer waveguide 510 is still obscured by material and cannot be directly docked with the optical fiber. Therefore, it is necessary to first cut the chip at a predetermined position to form the initial coupling end face M; then, polishing is performed on the coupling end face M to remove chips, burrs, and minor surface damage caused by the cutting, allowing the end of the three-dimensional polymer waveguide 510 to be fully exposed on the coupling end face M. If only cutting is performed without polishing, the surface of the coupling end face M will be rough, causing light scattering loss and hindering the tight docking of the optical fiber. After cutting and polishing, the coupling end face M of this application is smooth and flat, and the end of the three-dimensional polymer waveguide 510 is fully exposed. This reduces light scattering loss at the end face and allows the standard single-mode fiber to fit tightly against the chip end face, ensuring efficient coupling of light into the fiber. Furthermore, since the methods for cutting and polishing the coupling end face are not entirely the same, this application embodiment can describe one possible processing method.
[0040] In one case, the cutting and polishing of the coupling end face of the thin-film lithium niobate chip includes: The coupling end face of the thin-film lithium niobate chip is cut using a diamond cutting wheel, and the coupling end face is polished using an abrasive medium with a particle size of 0.1μm to 1μm.
[0041] In practical applications, when processing the coupling end face M, a diamond cutting wheel is used to cut the thin-film lithium niobate chip, and then an abrasive medium with a particle size of 0.1μm-1μm is used to polish the coupling end face M. The diamond cutting wheel has high hardness and can easily cut the multilayer chip composed of lithium niobate, silicon dioxide, and silicon, precisely breaking the chip at a preset position to process the initial coupling end face M. However, after the cutting wheel, the end face will have processing damage such as chipping and micro-cracks, making it unsuitable for direct fiber optic splicing. Therefore, further polishing with an abrasive medium is required. The particle size of the abrasive medium used for polishing must be controlled within the range of 0.1μm-1μm. If the abrasive medium particles are too large, the grinding force is too strong, which can easily scratch the coupling end face M and damage the end of the three-dimensional polymer waveguide 510; if the abrasive medium particles are too small, the material removal speed is very slow, which will prolong the processing time and reduce production efficiency. This application employs polishing media with a particle size of 0.1μm to 1μm to remove chipping and microcracks caused by cutting, resulting in a smooth and flat coupling end face M without scratching the end of the 3D polymer waveguide 510. This approach balances optical quality with processing efficiency, reduces light scattering loss, and ensures effective coupling with standard single-mode optical fibers.
[0042] In summary, this application first provides a thin-film lithium niobate chip, and spin-coates a negative photoresist onto the surface of the thin-film lithium niobate chip to form a photoresist layer with a thickness of not less than 12 μm. A lithium niobate waveguide with an inverted cone structure is disposed on the surface of the thin-film lithium niobate chip; the tip of the inverted cone structure points towards the coupling end face of the thin-film lithium niobate chip. Then, femtosecond laser two-photon polymerization technology is used to perform three-dimensional direct writing on the photoresist layer, integrally forming a three-dimensional polymer waveguide with continuously changing morphology above the lithium niobate waveguide. The transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the lithium niobate waveguide end along the propagation direction to a second dimension near the coupling end face, used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode spot matching a standard single-mode fiber; the first dimension is smaller than the second dimension. Then, the photoresist layer is developed, and the three-dimensional polymer waveguide is cured. Finally, the coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with a standard single-mode fiber. Thus, by spin-coating a negative photoresist layer with a thickness of not less than 12 μm onto the surface of the thin-film lithium niobate chip, and using femtosecond laser two-photon polymerization technology to directly write and integrally form a three-dimensional polymer waveguide with continuously changing morphology, the mode field of the lithium niobate waveguide can be adiabatically evolved using this waveguide, resulting in a mode pattern matching that of a standard single-mode fiber. After development, curing, and cutting and polishing of the coupling end face, fiber docking is achieved, improving the coupling performance of the thin-film lithium niobate end face coupler.
[0043] Figure 3 This is a schematic diagram of a thin-film lithium niobate end-face coupler provided in an embodiment of this application. (Combined with...) Figure 3 As shown, the thin-film lithium niobate end-face coupler includes: a thin-film lithium niobate chip and a three-dimensional polymer waveguide 510; The surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide 310 with an inverted cone structure, the tip of the inverted cone structure pointing towards the coupling end face M of the thin-film lithium niobate chip; The three-dimensional polymer waveguide 510 is integrally formed above the lithium niobate waveguide 310. The transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide 510 smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide 310 along the propagation direction to a second dimension near the coupling end face M. This is used to perform adiabatic evolution of the mode field of the lithium niobate waveguide 310 to obtain a mode pattern that matches that of a standard single-mode fiber. The first dimension is smaller than the second dimension. The end section of the three-dimensional polymer waveguide 510 is exposed on the coupling end face M to interface with the standard single-mode optical fiber.
[0044] Furthermore, the first size is 2μm to 6μm, and the second size is 8μm to 16μm; The length of the transition section L of the three-dimensional polymer waveguide 510 is not less than 300 μm.
[0045] Specifically, this application provides a thin-film lithium niobate end-face coupler, including a thin-film lithium niobate chip and a three-dimensional polymer waveguide 510. The thin-film lithium niobate chip comprises a silicon substrate 100 and a silicon dioxide buried oxide layer 200. An inverted cone structure lithium niobate waveguide 310 is disposed on the upper surface of the silicon dioxide buried oxide layer 200, with the tip of the inverted cone structure facing the coupling end face M of the thin-film lithium niobate chip. The three-dimensional polymer waveguide 510 is integrally formed above the lithium niobate waveguide 310. Its lateral cross-sectional dimensions and vertical height smoothly and gradually increase from a first dimension near the lithium niobate waveguide 310 along the light propagation direction, transitioning to a second dimension near the coupling end face M, where the first dimension is smaller than the second dimension. This gradient structure allows for adiabatic evolution of the mode field of the lithium niobate waveguide 310, outputting a mode pattern matching that of a standard single-mode fiber. Furthermore, the end section of the three-dimensional polymer waveguide 510 is directly exposed on the coupling end face M, facilitating docking with a standard single-mode fiber. Furthermore, the first dimension is set to 2μm to 6μm, the second dimension to 8μm to 16μm, and the length of the transition section L of the three-dimensional polymer waveguide 510 is set to be no less than 300μm. The lithium niobate waveguide 310 with its inverted cone structure can reduce the waveguide's constraint on light, allowing light to diffuse outward and facilitating light coupling into the upper three-dimensional polymer waveguide 510. The first dimension of 2μm-6μm matches the light field output by the lithium niobate waveguide 310, ensuring efficient light entry into the three-dimensional polymer waveguide 510; the second dimension of 8μm-16μm ensures that the output mode pattern matches the mode pattern of a standard single-mode fiber, improving fiber alignment tolerance. The length of the transition section L is no less than 300μm, ensuring that the waveguide size change is sufficiently gradual, meeting the adiabatic evolution conditions, and suppressing the generation of higher-order modes. In summary, this coupler, through the interaction of a lithium niobate reverse cone waveguide and an upper gradient three-dimensional polymer waveguide 510, can achieve low-loss mode field conversion, while also possessing a large fiber alignment tolerance and stable overall optical performance.
[0046] In summary, this application provides a thin-film lithium niobate end-face coupler, comprising: a thin-film lithium niobate chip and a three-dimensional polymer waveguide. The surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide of an inverted cone structure, the tip of which points towards the coupling end face of the thin-film lithium niobate chip. The three-dimensional polymer waveguide is integrally formed above the lithium niobate waveguide. The lateral cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face, used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode pattern matching a standard single-mode fiber. The first dimension is smaller than the second dimension. The end cross-section of the three-dimensional polymer waveguide is exposed at the coupling end face for mating with a standard single-mode fiber. Thus, by spin-coating a negative photoresist layer with a thickness of not less than 12 μm onto the surface of a thin-film lithium niobate chip, and using femtosecond laser two-photon polymerization technology to directly write and integrally form a three-dimensional polymer waveguide with continuously changing morphology, the mode field of the lithium niobate waveguide can be adiabatically evolved using this waveguide. This allows for the generation of mode spots that match those of standard single-mode optical fibers. After development, curing, and dicing and polishing of the coupling end face, fiber docking is achieved, improving the coupling performance of the thin-film lithium niobate end face coupler. In addition, the thin-film lithium niobate end face coupler provided in this application can theoretically achieve a single-end coupling loss of less than -0.5 dB and a polarization-dependent loss of less than 0.3 dB. Due to the significant expansion of the end mode field, the 1 dB tolerance of fiber alignment can be increased to more than ±2.4 μm, greatly reducing the packaging difficulty. The continuous geometric gradient avoids the excitation of higher-order modes caused by abrupt mode changes, ensuring stable operation over ultra-wideband (>100 nm).
[0047] The above description of the disclosed embodiments enables those skilled in the art to make or use this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for fabricating a thin-film lithium niobate end-face coupler, characterized in that, The method includes: A thin-film lithium niobate chip is provided; the surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide with an inverted cone structure; the tip of the inverted cone structure points to the coupling end face of the thin-film lithium niobate chip; A negative photoresist is spin-coated onto the surface of the thin-film lithium niobate chip to form a photoresist layer with a thickness of not less than 12 μm; The photoresist layer is three-dimensionally written using femtosecond laser two-photon polymerization technology to integrally form a three-dimensional polymer waveguide with continuously changing morphology above the lithium niobate waveguide. The transverse cross-sectional dimensions and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face. This is used to adiabatically evolve the mode field of the lithium niobate waveguide to obtain a mode pattern that matches a standard single-mode fiber. The first dimension is smaller than the second dimension. The photoresist layer is developed, and the three-dimensional polymer waveguide is cured. The coupling end face of the thin-film lithium niobate chip is cut and polished to expose the end section of the three-dimensional polymer waveguide on the coupling end face for docking with the standard single-mode optical fiber.
2. The method according to claim 1, characterized in that, The method of using femtosecond laser two-photon polymerization technology to perform three-dimensional direct writing on the photoresist layer includes: As the scanning position moves toward the coupling end face, the output power of the laser is increased linearly or nonlinearly, and the Z-axis focusing depth of the femtosecond laser is adjusted simultaneously.
3. The method according to claim 1, characterized in that, The first dimension is 2 μm to 6 μm, and the second dimension is 8 μm to 16 μm.
4. The method according to claim 1, characterized in that, The length of the transition section of the three-dimensional polymer waveguide is not less than 300 μm.
5. The method according to claim 1, characterized in that, The width of the tip of the inverted cone structure is 80 nm to 150 nm.
6. The method according to claim 1, characterized in that, The curing temperature is between 150°C and 250°C.
7. The method according to claim 1, characterized in that, The cutting and polishing of the coupling end face of the thin-film lithium niobate chip includes: The coupling end face of the thin-film lithium niobate chip is cut using a diamond cutting wheel, and the coupling end face is polished using an abrasive medium with a particle size of 0.1μm to 1μm.
8. A thin-film lithium niobate end-face coupler, characterized in that, include: Thin-film lithium niobate chip and three-dimensional polymer waveguide; The surface of the thin-film lithium niobate chip is provided with a lithium niobate waveguide with an inverted cone structure, the tip of which points towards the coupling end face of the thin-film lithium niobate chip. The three-dimensional polymer waveguide is integrally formed on top of the lithium niobate waveguide. The transverse cross-sectional dimension and vertical height of the three-dimensional polymer waveguide smoothly and gradually change from a first dimension near the end of the lithium niobate waveguide along the propagation direction to a second dimension near the coupling end face. This is used to perform adiabatic evolution of the mode field of the lithium niobate waveguide to obtain a mode pattern that matches that of a standard single-mode fiber. The first dimension is smaller than the second dimension. The end section of the three-dimensional polymer waveguide is exposed on the coupling end face to interface with the standard single-mode fiber.
9. The thin-film lithium niobate end-face coupler according to claim 8, characterized in that, The first dimension is 2 μm to 6 μm, and the second dimension is 8 μm to 16 μm.
10. The thin-film lithium niobate end-face coupler according to claim 8, characterized in that, The length of the transition section of the three-dimensional polymer waveguide is not less than 300 μm.