A fiber optic communication MT plug with low-reflection AR coating and its coating preparation method
By setting an annular junction area with a high refractive index layer and a low refractive index covering layer and a membrane-free isolation ring in the optical fiber communication MT plug, the problems of high reflectivity and large propagation loss in the optical fiber communication MT plug are solved, and the effect of low reflectivity and low propagation loss is achieved.
Patent Information
- Application Number
- CN202611473796.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies make it difficult to effectively control the edge position and adhesive interface of the antireflective film in optical fiber communication MT plugs, resulting in high reflectivity and large propagation loss. Furthermore, the design of the coating window is prone to introducing shadow areas and positioning errors.
By setting a high refractive index layer and a low refractive index capping layer on the fiber end face, a closed annular bonding area is formed, and a film-free isolation ring is retained on the cladding end face to prevent the antireflection film from crossing the adhesive interface. Channel-by-channel detection is combined to ensure the accuracy of film thickness and position.
It achieves low reflectivity and low propagation loss, stably controls the edge position of the film, avoids the impact of adhesive deformation and interface contamination on optical performance, and improves the reliability of optical fiber communication.
Smart Images

Figure CN123066931A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to multi-fiber connectors and optical thin film fabrication technology, specifically to an optical fiber communication MT plug with low-reflection AR coating and its coating fabrication method. Background Technology
[0002] The MT connector uses a multi-hole ferrule to hold the positions of multiple fiber end faces and two guide holes for mating alignment. The fiber core transmits signals, and the surrounding glass cladding constrains the guided mode; at the point where the quartz end face contacts the air, the abrupt change in refractive index causes Fresnel reflection. Physical contact mating ensures the relative glass surfaces are in contact, while non-contact mating requires simultaneous control of end face reflections and propagation losses caused by air gaps.
[0003] In non-contact structures, the fiber end face can be recessed and a dielectric antireflection coating deposited, utilizing the interference of thin films with different refractive indices to reduce reflection. The fiber is typically fixed within the ferrule with adhesive, thus the end face comprises glass, adhesive, and ferrule material. If the antireflection coating continuously spans these heterogeneous interfaces, adhesive deformation or interface contamination may affect the coating edge; simply obscuring the ferrule bearing surface does not clearly define the relationship between the coating boundary and the adhesive interface on a single fiber.
[0004] On the other hand, simply reducing the size of the coating window introduces shadow areas and positioning errors, which may result in insufficient film thickness in the effective light area or failure of the upper layer to cover the edge of the lower layer. The shadow effect of the window, combined with the positioning deviation, makes it difficult to stably control the film edge position and interlayer coverage on the single fiber end face. Summary of the Invention
[0005] To address the aforementioned issues, this invention provides an optical fiber communication MT plug with low-reflection AR coating and its coating preparation method. By preparing the nested film boundaries and corresponding windows on each fiber end face, the anti-reflection film is separated from the adhesive interface, while maintaining non-contact mating.
[0006] The above-mentioned technical objective of the present invention is achieved through the following technical solution: an optical fiber communication MT plug with low-reflection AR coating, comprising an MT ferrule having two guide holes and a bearing end face, and a plurality of optical fibers arranged in an array and each consisting of a fiber core and a cladding surrounding the fiber core, wherein the cladding is fixed to the MT ferrule by an adhesive layer; each optical fiber end face is provided with a high refractive index layer covering the fiber core and extending to the cladding, and a low refractive index cover layer covering the high refractive index layer; the low refractive index cover layer extends beyond the entire periphery of the high refractive index layer and directly joins with the end face of the cladding to form a closed annular joint area; the outer periphery of the low refractive index cover layer is located within the end face of the cladding, and a continuous membrane-free isolation ring is maintained between the low refractive index cover layer and the interface between the cladding and the adhesive layer; the bearing end face does not cover the high refractive index layer and the low refractive index cover layer, and the coating surface on each optical fiber end face is recessed behind the bearing end face, so that an air gap is maintained between the opposing coating surfaces when the bearing end faces of the same type plug abut against each other.
[0007] Preferably, the periphery of the high refractive index layer has a transition region that gradually thins from the inside to the outside, and the low refractive index capping layer continuously covers the transition region and extends to the annular bonding region; the minimum radial width of the membrane-free isolation ring is not less than 10 μm.
[0008] Preferably, the optical fiber is a quartz single-mode optical fiber with a diameter of 125 μm, and the end face of the optical fiber is perpendicular to the optical axis; the high refractive index layer is a tantalum oxide layer, and the low refractive index capping layer is a silicon dioxide layer, with nominal thicknesses of 50 nm and 300 nm respectively covering the central region of the fiber core, for use in the 1260-1360 nm band.
[0009] Preferably, the MT ferrule is a zirconia component, the glass end face of each optical fiber is recessed 2.5-3.5 μm relative to the bearing end face, and the coated surface is recessed 2.1-3.2 μm relative to the bearing end face.
[0010] A method for preparing a coating on an optical fiber communication MT plug with a low-reflection AR coating includes the following steps: Step 1: Fix multiple optical fibers consisting of fiber core and cladding to the MT ferrule with two guide holes using an adhesive layer. Flatten the end face of each optical fiber and form a receding amount relative to the bearing end face. After cleaning, establish a coating positioning reference with the two guide holes. Step 2: While keeping the bearing end face and the adhesive layer shielded, align each small window of the first shield with the fiber core, and deposit a high refractive index layer through the small windows to cover the fiber core and terminate in the cladding end face. Step 3: Maintain the positioning reference of the MT ferrule, remove the first shield and align the large window of the second shield with the optical fiber corresponding to the small window respectively; based on the window size, the distance between the shield and the end face, the angle range of the deposition bundle and the positioning deviation, limit the maximum deposition envelope of the high refractive index layer to be surrounded by the full illumination area of the large window, and the maximum deposition envelope of the large window is separated from the boundary between the cladding and the adhesive layer. Step 4: Deposit a low-refractive-index capping layer through the large window, so that it continuously covers the periphery of the high-refractive-index layer and forms a closed direct bonding area on the end face of the cladding layer. Remove the second mask, leaving the film-free isolation ring on the outer periphery of the low-refractive-index capping layer. Step 5: Detect the receding amount of the membrane-free isolation ring, the direct bonding area, and each membrane surface relative to the bearing end face, and detect the end face reflection spectrum of the target band channel by channel. Remove plugs that have the membrane crossing the boundary between the cladding and the adhesive layer, the direct bonding area not closed, the receding amount insufficient, or the reflection spectrum not meeting the set upper limit.
[0011] Preferably, the small window has a diameter of 65±1μm, the large window has a diameter of 92±1μm, the mask thickness is 15μm, the distance between the glass end face and the near side of the mask is 10μm, the angle between the deposition beam and the optical axis does not exceed 5°, the deviation of each window from the fiber core does not exceed 2μm, and the measured minimum width of the membrane-free isolation ring is not less than 10μm.
[0012] Preferably, the high refractive index layer of tantalum oxide and the low refractive index coating layer of silicon dioxide are formed sequentially by ion-assisted electron beam evaporation, and the MT ferrule is held on a cooling fixture at a temperature not exceeding 80°C; when switching the mask, the mask is first removed from the formed film layer along the optical axis, and then switched laterally, while maintaining the position of the MT ferrule in the vacuum fixture during the switching.
[0013] Preferably, a fused silica witness plate with the same frame as the MT ferrule is used to measure the refractive index and deposition rate of each material, and the film thickness in the central region is determined by the measured values; the end face power reflectivity measured channel by channel in the 1260-1360nm band is set with an upper limit of no more than 0.2%, and the insertion loss is tested separately after mating with the same type of plug.
[0014] In summary, the present invention has the following advantages: by using a low refractive index coating layer to pass over the periphery of the high refractive index layer and directly bond to the glass, the edge of the lower film is covered under the outer layer, and then a continuous film-free isolation ring is used to disconnect the connection between the film layer and the glass-adhesive interface, thereby reducing the path of heterogeneous interface deformation to the optically effective area through the continuous film.
[0015] The mating position is defined by the uncoated bearing end face, keeping the effective film surface recessed to avoid the antireflective film bearing the mating contact load. The coverage margin is determined by combining the outer envelope of the window and the full illumination area, simultaneously considering film edge bonding and the uncoated isolation ring. Channel-by-channel reflection detection avoids judging the antireflective effect solely based on the nominal deposition thickness. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the end structure of the MT ferrule.
[0017] Figure 2 This is a partial front view of a single-channel end face.
[0018] Figure 3 This is a partial cross-sectional view of the periphery of the high refractive index layer.
[0019] Figure 4 This is a partial longitudinal section of the end of a single-sided MT ferrule.
[0020] Figure 5 This is a flowchart of the coating preparation process.
[0021] Explanation of reference numerals in the attached drawings: 110, MT ferrule; 111, bearing end face; 112, guide hole; 121, fiber core; 122, cladding; 123, membrane-free isolation ring; 130, adhesive layer; 140, high refractive index layer; 150, low refractive index cover layer. Detailed Implementation
[0022] The following is combined Figures 1 to 5 This invention is described below. Here, AR stands for anti-reflective coating, and MT represents an interface form that utilizes rectangular multi-fiber ferrules and dual guide holes to achieve multi-channel alignment. This embodiment uses customized zirconia porous components and matching connectors, suitable for quartz single-mode optical fibers in the 1260-1360nm band. Its front end uses normal, non-contact optical splicing, and the rear can be fitted with a conventional housing with axial elastic preload and locking structure; the housing's function is to keep the two bearing end faces 111 in contact, and the optical film does not bear this preload.
[0023] like Figure 1 and Figure 4 As shown, the MT ferrule 110 has a row of eight fiber optic holes, with a guide hole 112 on each side. The fiber pitch is 250μm, the nominal diameter of the cladding 122 is 125μm, and the nominal diameter of the fiber optic holes is 126μm. A cured epoxy adhesive layer 130 is formed between them. The MT ferrule 110 can have dimensions of 6.4mm × 2.5mm × 3mm, and the center distance between the two guide holes 112 is 4.6mm, with a hole diameter of 0.700mm. During mating, a 0.699mm diameter guide pin is inserted into the corresponding holes on both sides. The actual selection and fit of the guide pin and holes must also meet the lateral alignment requirements of the channel.
[0024] The key structure of this embodiment can be understood from a single end face: the high-refractive-index layer 140 covers the fiber core 121 and a portion of the surrounding cladding 122, but does not reach the interface between the glass and the adhesive; the low-refractive-index capping layer 150 forms an anti-reflection film system with the high-refractive-index layer 140 at the center, and extends outward beyond the periphery of the high-refractive-index layer 140, landing directly on the exposed cladding 122. This direct bonding area closes around the high-refractive-index layer 140, and further outward is the still-exposed, film-free isolation ring 123. Therefore, there is neither a continuous film bridging the glass and the adhesive, nor is the periphery of the high-refractive-index layer 140 directly exposed as the outer boundary of the film system.
[0025] like Figure 2 and Figure 3 As shown, the high-refractive-index layer 140 has a center thickness of 50 nm and a center plateau radius of 31 μm, terminating at a radius of 34 μm after thinning transition. The low-refractive-index capping layer 150 has a center thickness of 300 nm, its lower surface extends along the upper surface of the high-refractive-index layer 140 and the thinning perimeter, and then directly bonds to the glass; its outer plateau can extend to a radius of 43 μm, then thins outward and terminates at a radius of 47 μm. Thus, the nominal radial width of the unfilmed isolation ring 123 is 15.5 μm, and the total central film thickness is 350 nm. The above edge dimensions are nominal designs for process tuning; the actual shadow transition zone is formed by the beam angle distribution and mask spacing, and its contour should be confirmed through sample cross-section or contour measurement.
[0026] Figure 2 This is a partial front view of an optical fiber end face and surrounding ferrule. The annular outline in the figure includes the contour formed by the undulation of the outer film surface following the lower edge. Figure 3 Only a partial longitudinal section near the periphery of the high-rise is shown to represent the joint relationship after the overburden layer crosses the termination edge of the lower layer; the vertical direction corresponds to the observation direction of the section and does not represent the direction of gravity. Figure 4 A partial longitudinal section of the central thin sheet on one side of an optical channel and surrounding ferrules is taken, and the uncoated bearing end face 111 and the outer surface of the low-refractive-index coating layer 150 receding from this face are marked respectively; the same type of mating parts have the same end face structure. The truncation boundary of each partial figure only defines the observation range and is not the actual outer edge of the ferrule or optical fiber; the film thickness is expressed according to the true scale.
[0027] The reason for setting the aforementioned radial boundaries is that the adhesive layer 130, zirconium oxide, and quartz differ in their elasticity, thermal expansion, and adsorption states. If the antireflective coating crosses these boundaries, the deformation of the adhesive or the localized cleaning load on the end face may be transmitted to the effective light area through the continuous film. The film-free isolation ring 123 interrupts this path on the glass; the annular portion of the low-refractive-index capping layer 150 directly bonded to the glass covers the thin edge of the high-refractive-index layer 140. The residual stress of the film itself can affect edge adhesion, contamination on the glass surface can weaken direct bonding, and foreign particles may alter the non-contact gap or cause localized contact. Therefore, it is necessary to control the deposition stress, end face cleanliness, and particle residue before mating.
[0028] In the axial direction, Figure 4 The bearing end face 111 is at zero position, the glass end face is nominally recessed by 3μm, and the central film surface is recessed by 2.65μm. During mating, the bearing end faces 111 of the two identical plugs abut against each other, and the contact load is borne by the bearing end face 111; the outer surfaces of the low refractive index coating 150 on both sides are recessed to the abutment position, and the nominal air gap between the central film surfaces is 5.30μm. The glass recess is controlled between 2.5 and 3.5μm, and the recess of the film surface after plating is checked and found to be 2.1 to 3.2μm, so the gap between the paired film surfaces is 4.2 to 6.4μm. The recess cannot be replaced by subtracting the thickness of the quartz crystal from the pre-plating dimension; it must be actually measured on the finished end face.
[0029] To achieve the required retraction, the end face of the MT ferrule 110, to which the short bare fiber is fixed, is first leveled with diamond abrasive material of progressively decreasing grit size. Then, a compliant polishing material containing cerium oxide abrasive grains is used to differentially polish the quartz end face, causing a controlled retraction of the quartz relative to the zirconium oxide. An interferometric profilometer is used to measure the height difference between the bearing end face 111 reference and the effective optical area of the fiber channel by channel, controlling end face tilt, scratches, and adhesive residue. The polishing rate is related to the fixture load and abrasive condition; the process is terminated at the measured height, and a micron-level retraction is not guaranteed with a fixed time.
[0030] Zirconia porous components can be obtained through pre-forming with holes, sintering, and precision machining of the hole openings. The positions of the fiber optic holes and guide holes 112 are determined by a common machining datum. Components whose measured channel positions do not meet the alignment requirements are discarded or paired for selection. The nominal dimensions of the aperture and pitch do not represent all permissible positional errors. Taking a single-mode fiber with a mode field diameter of 9.2 μm at 1310 nm as an example, a relative lateral offset of 0.7 μm corresponds to an ideal Gaussian mode coupling loss of approximately 0.10 dB. Therefore, fiber eccentricity, hole position, guide pin gap, and pairing repeatability need to be controlled together.
[0031] like Figure 5As shown, before coating, the adhesive layer 130 is fully cured. A cleaning solution compatible with the selected epoxy is used to remove polishing residue, followed by drying with filtered gas. The area containing the fiber core 121 is checked for the absence of adhesive film and particles. Vacuum treatment uses short bare fibers extending from the rear of the ferrule; the tail coating and outer sheath are left for subsequent splicing processes. Pre-evacuation and low-temperature drying are performed according to the temperature resistance and venting conditions of the adhesive used to prevent the formation of a weak bonding layer on the glass surface by volatile organic compounds.
[0032] The first and second shields use the same aperture array and guide reference, with small and large windows respectively. The shields can be made of 15μm thick electroformed nickel sheets and are kept flat by a back frame; initial positioning is done using the guide aperture reference, and then the deviation between each window and the fiber core 121 is measured by microscopic imaging. The near side of the shield is limited by a clamp at a distance of 10μm from the glass end face and does not directly press against the fiber end face. Except for each window, the shield continuously covers the bearing end face 111, the adhesive layer 130, and the aperture reference area.
[0033] The small window diameter is set at 65±1μm, and the large window diameter at 92±1μm. The maximum angle of the deposition beam relative to the optical axis is 5°. This angle limit includes the combined effects of source size, workpiece relative position, and fixture angle error, and should be defined by the source and tooling geometry and the baffle; it is not simply a matter of setting a single workpiece tilt angle. The two positioning deviations should each be controlled within 2μm, and both measurements should be taken relative to the actual fiber center; it is not sufficient to only measure the relative offset between the two shields.
[0034] The process allowance at the window edge is calculated using two different boundaries: the outward expansion envelope of the window is calculated by multiplying the distance from the end face to the near side of the shield by the tangent of the maximum beam angle; the inward reduction of the fully illuminated area is calculated by multiplying the sum of this distance and the shield thickness by the same tangent. Aperture error and positioning deviation are then taken into account. In this embodiment, the maximum deposition radius of the small window is approximately 35.87 μm, and the minimum fully illuminated radius of the large window is approximately 41.31 μm, leaving a coverage allowance of approximately 5.44 μm between them; the maximum deposition radius of the large window is approximately 49.37 μm, leaving approximately 13.13 μm from the outer edge of the glass with a radius of 62.5 μm. Therefore, the minimum width of the finished membrane-free isolation ring 123 can be set to 10 μm, allowing for measurement and edge scattering margins.
[0035] First, a high-refractive-index tantalum oxide layer 140 is deposited through a small window. After reaching the target optical thickness in the central region, the deposition baffle is closed, and the mask is first removed along the optical axis from the formed film layer, then moved to the large window station and the limit is re-measured. During the second deposition of the low-refractive-index silica capping layer 150, the deposition flux from the allowable angle range can reach the entire bevel of the lower layer and the outer exposed glass. Since the thinning slope of the lower layer is relatively gentle, it is not necessary to assume that the vertical sidewalls of the coating are necessarily covered by normal evaporation; if abrupt sidewalls or shadow gaps are formed in the actual measurement, the angle distribution and spacing should be adjusted, and the continuity of the joint should not be judged simply because the large window is large.
[0036] One possible setup is ion-assisted electron beam evaporation with a cooling fixture, where the base pressure is first pumped down to no more than 5 × 10⁻⁶. -4 Pa, then set the oxygen supply and ion-assisted conditions according to the tantalum oxide or silicon dioxide material respectively, and adjust the deposition rate from 0.1 to 0.3 nm / s. The workpiece temperature should not exceed 80℃. Ion assistance is used to improve the density of low-temperature deposition, but it cannot replace cleaning by increasing ion energy; ion bombardment should be avoided to prevent damage to the adhesive or excessive film stress. The first and second masks can be installed on the switching mechanism in the vacuum, and the workpiece is held between the two coatings to reduce interface contamination caused by re-exposure to air.
[0037] The optical setup of the film system uses a planar thin-film model in the central region: tantalum oxide and silicon dioxide sequentially from glass to air. Assuming a glass refractive index of 1.447, tantalum oxide refractive index of 2.10, and silicon dioxide refractive index of 1.45, with each refractive index remaining constant within the used wavelength range and absorption ignored, the single-end power reflectance of the two central films at 50nm and 300nm is approximately 0.0017% at 1310nm, with a maximum value of approximately 0.126% in the 1260–1360nm range. Under the same assumptions, the reflectance at the uncoated glass-air interface is approximately 3.34%. These values are calculated from the characteristic matrix, not from sample measurements.
[0038] Film thickness and material condition must be controlled together. Using tantalum oxide film thicknesses of 49 nm or 51 nm and silicon dioxide film thicknesses of 294 nm or 306 nm, and refractive indices of 2.09 or 2.11 and 1.44 or 1.46 respectively, the reflectance of these combinations can be calculated, with the maximum value reaching approximately 0.324%. Therefore, simply having a thickness within the above range cannot be used to determine if the 0.2% reflectance limit is met. Ellipsometry or spectral fitting is performed using fused silica witness sheets from the same substrate to obtain the batch's refractive index, absorption, and deposition rate, and the deposition endpoint is then redefined accordingly. Crystal monitoring values should also be corrected for geometric tool factors using witness sheets.
[0039] After removing the cover, use microscopic inspection and contour measurement to verify that the uncoated isolation ring 123 is closed and not less than the set width, and that the film does not cross the interface between the glass and the adhesive. For process standardization and batch sampling inspection, cross-sectional observation can be performed on the sacrificial end face of the same process to confirm that the low refractive index capping layer 150 continuously covers the periphery of the high refractive index layer 140 and is bonded to the glass, eliminating shadows, pinholes, and warping. The continuous film on the witness sheet only indicates the corresponding material and thickness status and cannot replace the inspection of the actual fiber end face window position and edge coverage.
[0040] During channel-by-channel testing, the single-end-face reflection spectrum is measured using an optical path with a known reflection reference. Input coupling, fiber optic splicing, and instrument background reflection are subtracted from the calibration. The 1260-1360nm band is scanned, and the maximum power reflectivity within this band is no higher than 0.2% as the acceptance setting for this embodiment. For those that do not meet the requirements, the corresponding channel is recorded, and the reasons for film thickness, refractive index, or window offset are re-analyzed. Unqualified end faces are not directly submitted for pairing. This threshold is the process acceptance condition, and whether it is met is determined by finished product testing.
[0041] After mating, insertion loss and return signal must be measured. Using an ideal Gaussian beam with a mode field radius of 4.6 μm and a wavelength of 1310 nm, the Rayleigh length in air is approximately 50.75 μm. The coupling loss due to axial propagation alone in the 6.4 μm gap is approximately 0.017 dB, but this does not include lateral offset, end-face tilt, contamination, and multiple reflections. Two normally low-reflectivity surfaces can still form a weak Fabry-Perot cavity. Based on the single-sided maximum reflectivity of the aforementioned nominal film system, the worst-case coherent reflection is approximately 0.50%. Therefore, the single-sided anti-reflection rate cannot be directly converted into the return signal performance of the entire plug pair.
[0042] This embodiment is used in pairs with mating parts having the same receding film surface; for physical contact mating parts with protruding end faces, housing keys should be used to distinguish them and avoid mixing, and connection should not be allowed simply because the guide hole can be inserted.
Claims
1. A fiber optic communication MT connector with low-reflection AR coating, characterized in that, It includes an MT ferrule (110) having two guide holes (112) and a bearing end face (111), and a plurality of optical fibers arranged in an array and each consisting of a fiber core (121) and a cladding (122) surrounding the fiber core (121), wherein the cladding (122) is fixed to the MT ferrule (110) by an adhesive layer (130). Each optical fiber has a high refractive index layer (140) covering the fiber core (121) and extending to the cladding (122) on its end face, and a low refractive index capping layer (150) covering the high refractive index layer (140); the low refractive index capping layer (150) extends across the entire periphery of the high refractive index layer (140) and directly joins with the end face of the cladding (122) to form a closed annular joint area; The outer periphery of the low refractive index capping layer (150) is located within the end face of the cladding layer (122), and a continuous membrane-free isolation ring (123) is maintained between the cladding layer (122) and the adhesive layer (130); the bearing end face (111) does not cover the high refractive index layer (140) and the low refractive index capping layer (150), and the film surface on each fiber end face is recessed from the bearing end face (111) so that an air gap is maintained between the opposing film surfaces when the bearing end face (111) of the same type plug abuts.
2. The fiber optic communication MT plug with low-reflection AR coating according to claim 1, characterized in that, The periphery of the high refractive index layer (140) has a transition region that gradually thins from the inside to the outside, and the low refractive index capping layer (150) continuously covers the transition region and extends to the annular bonding region; the minimum radial width of the membrane-free isolation ring (123) is not less than 10 μm.
3. The fiber optic communication MT plug with low-reflection AR coating according to claim 2, characterized in that, The optical fiber is a quartz single-mode optical fiber with a diameter of 125 μm, and the end face of the optical fiber is perpendicular to the optical axis; the high refractive index layer (140) is a tantalum oxide layer, and the low refractive index capping layer (150) is a silicon dioxide layer. The nominal thicknesses of the two layers in the central area covering the fiber core (121) are 50 nm and 300 nm, respectively, for the 1260-1360 nm band.
4. The fiber optic communication MT plug with low-reflection AR coating according to claim 1, characterized in that, The MT ferrule (110) is a zirconia component. The glass end face of each optical fiber is recessed by 2.5-3.5 μm relative to the bearing end face (111), and the coated surface is recessed by 2.1-3.2 μm relative to the bearing end face (111).
5. A method for preparing a coating on an optical fiber communication MT plug with a low-reflection AR coating, characterized in that, Includes the following steps: Step 1: Fix multiple optical fibers consisting of fiber core (121) and cladding (122) to MT ferrule (110) with two guide holes (112) using adhesive layer (130). Flatten the end face of each optical fiber and form a receding amount relative to the bearing end face (111). After cleaning, establish the coating positioning reference with the two guide holes (112). Step 2: While keeping the bearing end face (111) and the adhesive layer (130) covered, align each small window of the first shield with the fiber core (121) and deposit a high refractive index layer (140) through the small windows to cover the fiber core (121) and terminate in the end face of the cladding (122). Step 3: Maintain the positioning reference of the MT ferrule (110), remove the first shield and align the large window of the second shield with the optical fiber corresponding to the small window respectively; Based on the window size, the distance between the mask and the end face, the angular range of the deposition beam and the positioning deviation, the maximum deposition envelope of the high refractive index layer (140) is limited to be surrounded by the full illumination area of the large window, and the maximum deposition envelope of the large window is separated from the boundary between the cladding layer (122) and the adhesive layer (130). Step 4: Deposit a low-refractive-index capping layer (150) through the large window, so that it continuously covers the periphery of the high-refractive-index layer (140) and forms a closed direct bonding area on the end face of the cladding layer (122). Remove the second mask and retain the membrane-free isolation ring (123) on the outer periphery of the low-refractive-index capping layer (150). Step 5: Detect the amount of receding of the membrane-free isolation ring (123), the direct bonding area, and each membrane surface relative to the bearing end face (111), and detect the end face reflection spectrum of the target band channel by channel. Remove plugs where the membrane crosses the boundary between the cladding layer (122) and the adhesive layer (130), the direct bonding area is not closed, the receding amount is insufficient, or the reflection spectrum does not meet the set upper limit.
6. The coating preparation method for the fiber optic communication MT plug with low-reflection AR coating according to claim 5, characterized in that, The small window has a diameter of 65±1μm, the large window has a diameter of 92±1μm, the shield thickness is 15μm, the distance between the glass end face and the near side of the shield is 10μm; the angle of the deposition beam relative to the optical axis does not exceed 5°, the deviation of each window from the fiber core (121) does not exceed 2μm, and the measured minimum width of the membrane-free isolation ring (123) is not less than 10μm.
7. The coating preparation method for the fiber optic communication MT plug with low-reflection AR coating according to claim 5, characterized in that, The high refractive index layer (140) of tantalum oxide and the low refractive index capping layer (150) of silicon dioxide are formed sequentially by ion-assisted electron beam evaporation. The MT ferrule (110) is held on a cooling fixture at a temperature not exceeding 80°C. When switching the mask, the mask is first removed from the formed film layer along the optical axis, and then switched laterally. During the switching, the position of the MT ferrule (110) in the vacuum fixture is maintained.
8. The coating preparation method for the fiber optic communication MT plug with low-reflection AR coating according to claim 7, characterized in that, The refractive index and deposition rate of each material were measured using a fused silica witness plate that is on the same frame as the MT ferrule (110), and the film thickness in the central region was determined by the measured values. The end face power reflectivity measured channel by channel in the 1260-1360nm band was set to an upper limit of no more than 0.2%, and the insertion loss was tested separately after the same type of plug was mated.