A highly stable carbon nanotube conductive paste and its preparation method

By combining functionalized modified intermediates with gallium indium tin alloy, the problems of layering and gelation in carbon nanotube conductive paste were solved, achieving high stability and uniformity, and improving battery performance.

CN123072808APending Publication Date: 2026-11-10湖北冠毓新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611548821.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-08
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing carbon nanotube conductive pastes are prone to stratification, sedimentation, and gelation during storage and processing. Traditional dispersants have weak binding force, and functionalized dispersants may trigger side reactions, affecting electrode consistency and battery performance.

Method used

By using functionalized modified intermediates, pyrene groups are firmly anchored to the surface of carbon nanotubes through π-π stacking. Combined with sulfonate betaine structure, electrostatic repulsion and steric hindrance are provided. In conjunction with gallium indium tin alloy, conductive bridging is formed, which improves dispersion stability and reduces contact resistance.

Benefits of technology

The prepared conductive slurry exhibits no stratification or sedimentation during long-term storage, has a low viscosity change rate, and good uniformity of electrode sheet resistance, thereby improving the rate performance and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123072808A_ABST
    Figure CN123072808A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of conductive materials technology, specifically relating to a highly stable carbon nanotube conductive slurry and its preparation method. The conductive slurry comprises the following raw materials in parts by weight: 3-8 parts carbon nanotubes, 0.1-1 parts modified intermediate, 2 parts gallium indium tin alloy, 0.1-0.5 parts dispersant, 0.5-2 parts binder, and 88.5-96.5 parts organic solvent. The modified intermediate is mainly prepared from PAMAM, pyrene formaldehyde, 1,3-propanesulfonate lactone, and sodium borohydride. First, pyrene groups are grafted onto PAMAM through Schiff base reaction and reduction. Then, sulfonate betaine structure is introduced by ring opening with propanesulfonate lactone to block free amino groups. The pyrene groups are non-covalently coupled to carbon nanotubes through π-π coupling. At the same time, the zwitterionic structure provides electrostatic repulsion and steric hindrance, avoiding amino side reactions. This results in a slurry that does not stratify or harden during long-term storage, has a low viscosity change rate, and good sheet resistance uniformity of the electrode, which is beneficial to improving battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of conductive materials technology, specifically relating to a highly stable carbon nanotube conductive paste and its preparation method. Background Technology

[0002] Carbon nanotubes, due to their excellent electrical conductivity, high aspect ratio, and good mechanical properties, have broad application prospects in the field of conductive agents for electrochemical energy storage devices such as lithium-ion batteries and supercapacitors. In practical applications, carbon nanotubes are usually made into conductive slurries, which are then coated and dried to form a conductive network to reduce electrode internal resistance and improve rate performance. However, due to their large specific surface area and strong intertube van der Waals forces, carbon nanotubes are prone to agglomeration and entanglement in organic solvents, leading to increased slurry viscosity and poor dispersion uniformity, which in turn affects the uniformity of electrode resistance and battery cycle performance.

[0003] To address the aforementioned issues, existing technologies typically employ the addition of dispersants to improve the dispersion of carbon nanotubes in solvents. Common dispersants primarily rely on steric hindrance or electrostatic repulsion to inhibit aggregation; however, their binding force to the carbon nanotube surface is weak, and they often exist in a physical adsorption form. Under long-term storage, temperature fluctuations, or high-shear processing conditions, they are prone to desorption, leading to stratification, sedimentation, or even gelation of the slurry. Some existing technologies attempt to introduce anchoring effects through surface chemical modification of carbon nanotubes, but covalent modification often disrupts the graphitic structure of carbon nanotubes, impairing conductivity, while non-covalent coating may still lead to desorption in polar solvents. Furthermore, while some functionalized dispersants can provide strong anchoring capabilities, the active groups in their molecular structure may react with solvents, binders, or other components in the slurry, causing abnormally high viscosity or gelation, thus limiting practical applications. Therefore, developing a conductive slurry system that can effectively improve the dispersion stability of carbon nanotubes while avoiding the introduction of adverse side reactions remains a pressing technical problem in this field. Summary of the Invention

[0004] To address the above issues, this invention provides a highly stable carbon nanotube conductive slurry and its preparation method. By functionalizing and modifying the dispersant molecules, it enables them to have specific anchoring ability to the carbon nanotube surface and chemical inertness to the slurry components. This dispersant is then used in the preparation of the carbon nanotube conductive slurry, solving the problems of easy stratification, sedimentation, and gelation in existing slurries during storage and processing.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 3-8 parts carbon nanotubes, 0.1-1 parts modified intermediate, 2 parts gallium indium tin alloy, 0.1-0.5 parts dispersant, 0.5-2 parts binder, and 88.5-96.5 parts organic solvent.

[0006] Furthermore, the gallium-indium-tin alloy has the following composition by mass percentage: 68.5% gallium, 21.5% indium, and 10% tin.

[0007] Furthermore, the dispersant is selected from any one of PVP (polyvinylpyrrolidone), PAN (polyacrylonitrile), and PVB (polyvinyl butyral).

[0008] Furthermore, the adhesive is selected from any one of PVDF (polyvinylidene fluoride), PI (polyimide), and PMMA (polymethyl methacrylate).

[0009] Furthermore, the organic solvent is NMP (N-methylpyrrolidone) or DMF (N,N-dimethylformamide).

[0010] Further, the modified intermediate comprises the following raw materials: PAMAM (polyamide-amine dendritic polymer), PCA (pyrene formaldehyde), 1,3-propanesulfonate lactone, and NaBH4 (sodium borohydride), wherein the mass ratio of PAMAM, PCA, 1,3-propanesulfonate lactone, and NaBH4 is 10:0.67:10.6:0.22.

[0011] Furthermore, the method for preparing the modified intermediate is as follows: S1: Under a nitrogen atmosphere, PAMAM and PCA were dissolved separately to obtain PAMAM solution and PCA solution. The PCA solution was slowly added to the PAMAM solution and stirred at room temperature in the dark for 12 h. The solution gradually turned yellow-brown and a Schiff base reaction occurred to generate an imine, thus obtaining the reaction solution. S2: Cool the reaction solution to 4°C, add NaBH4 and stir to reduce. After the reaction is complete, transfer to diethyl ether for precipitation, filter, collect the precipitate and wash and dry to obtain Py-PAMAM (pyrene-modified intermediate). S3: After dissolving Py-PAMAM, 1,3-propanesulfonic acid lactone was added under a nitrogen atmosphere. The mixture was heated and stirred for 24 h. The lactone underwent ring opening under the action of primary, secondary or tertiary amines to generate a zwitterionic structure of sulfonate betaine, which was used to consume exposed and unreacted amino groups, block PAMAM, and prevent subsequent gelation in the conductive slurry, thus obtaining a sulfonated intermediate. The sulfonated intermediate was cooled and transferred to diethyl ether to precipitate, filtered, and the precipitate was collected, washed, purified by dialysis and dried to obtain the modified intermediate.

[0012] This invention also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve the modified intermediate in 20 parts of organic solvent to obtain an intermediate solution. Disperse the carbon nanotubes in the remaining organic solvent to obtain a dispersion. Heat the gallium indium tin alloy until it is completely melted, sonicate it, and then quickly add it to the dispersion. Stir it evenly to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min. The pyrene group in the modified intermediate is adsorbed on the surface of carbon nanotubes through π-π interaction. The sulfonate betaine structure provides steric hindrance and electrostatic repulsion, thus obtaining a pre-dispersed slurry. Step 3: After adding dispersant and binder to the pre-dispersed slurry, homogenize for 2 hours to allow the carbon nanotubes to fully deflocculate and disperse evenly, obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it, obtaining a highly stable carbon nanotube conductive slurry.

[0013] The beneficial effects achieved by this invention are as follows: The carbon nanotube conductive slurry provided by this invention incorporates pyrene and sulfonate betaine groups into a dendritic macromolecular framework through molecular design, constructing a modified intermediate with both strong anchoring and zwitterionic dispersion functions. Utilizing the strong π-π stacking interaction between the pyrene groups and the π-electron cloud on the carbon nanotube surface, the intermediate is firmly anchored to the carbon nanotube surface, overcoming the shortcomings of traditional dispersants that rely solely on physical adsorption and are prone to desorption. Simultaneously, sulfonate betaine alkalization transforms the highly reactive primary and secondary amines in PAMAM into chemically inert internal salt structures, shielding against side reactions between the amines and solvents / binders, and inhibiting carbon nanotube aggregation through electrostatic repulsion and steric hindrance. This "anchoring-dispersion-shielding" functional structure effectively solves the problems of slurry gelation and sedimentation. Furthermore, gallium indium tin alloy fills the gaps in the carbon nanotube network in the form of micron-sized droplets, forming conductive bridges between the tubes, reducing contact resistance, and endowing the conductive film with a certain degree of self-healing capability. In the conductive slurry, the modified intermediate works synergistically with the dispersant and binder. The stable coating layer on the surface of carbon nanotubes reduces competitive adsorption, allowing the dispersant to more effectively regulate the slurry viscosity. The binder, during film formation, works with the coating layer to construct a continuous conductive network. The conductive slurry prepared in this way exhibits no stratification or hard sedimentation during long-term storage, low viscosity change rate, and significantly improved sheet resistance uniformity of coated electrodes. This is beneficial for enhancing the rate performance and cycle stability of batteries, and shows promising prospects for industrial application. Attached Figure Description

[0014] Figure 1 The results of scanning electron microscopy examination of the conductive pastes prepared in Example 1 and Comparative Example 1; Figure 2The results of the particle size dispersibility study of the conductive pastes prepared in Examples 1-3 and Comparative Examples 1-2 are shown. Figure 3 The resistivity results are for the conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2. Figure 4 The results of viscosity variation investigation for the conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2 are shown. Figure 5 The deposition of the conductive pastes prepared in Example 1 and Comparative Example 2 after 3 months of storage; Figure 6 The results show the uniformity of sheet resistance of the conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2. Detailed Implementation

[0015] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0016] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.

[0017] Unless otherwise specified, all methods used in the following examples are conventional. Unless otherwise specified, all materials used in the following examples are new materials purchased from the market, and all parts are parts by weight. In the following examples and comparative examples, the carbon nanotubes used are multi-walled carbon nanotubes with a size of 9.5 nm × 1.5 μm, carbon purity > 95%, and metal oxide impurities < 5%. The PVP used is PVP K30. The PAN used has a molecular weight of approximately 150 kDa. The PVDF used is HSV900. The PAMAM used is PAMAM-G3, which is a third-generation polyamide-amine dendritic polymer containing 32 terminal amino active sites.

[0018] In the following examples and comparative examples, the modified intermediate comprises the following raw materials in parts by weight: 5 parts PAMAM, 0.335 parts PCA, 5.3 parts 1,3-propanesulfonic acid lactone, and 0.11 parts NaBH4. The preparation method is as follows: S1: Under a nitrogen atmosphere, 5 parts of PAMAM were dissolved in DMF to prepare a 20% PAMAM solution, and 0.335 parts of PCA were dissolved in DMF to prepare a 13.4% PCA solution. The PCA solution was slowly added to the PAMAM solution at a rate of 1 mL / min. The mixture was stirred at room temperature in the dark for 12 h at a stirring speed of 300 rpm to obtain the reaction solution. S2: Cool the reaction solution to 4℃, add 0.11 parts of NaBH4 in 3 portions under stirring at 200 rpm, and stir to reduce the solution. The addition is 5 min apart. Stir the reaction at room temperature for 4 h. After the reaction is complete, transfer the solution to 8 volumes of pre-cooled anhydrous diethyl ether at 4℃ for precipitation, filter, collect the precipitate, wash it 3 times with anhydrous diethyl ether, and dry it at 60℃ for 12 h to obtain Py-PAMAM. S3: Py-PAMAM was dissolved in DMF to prepare a 15% (w / v) solution. 5.3 parts of 1,3-propanesulfonic acid lactone were added to the solution under a nitrogen atmosphere. The mixture was heated to 70°C and stirred at 200 rpm for 24 h to obtain a sulfonated intermediate. After cooling, the sulfonated intermediate was transferred to pre-cooled anhydrous diethyl ether to precipitate and filtered. The precipitate was collected and washed. The washed precipitate was redissolved in purified water at a 5% (w / v) concentration and purified by dialyzing in a dialysis bag with a molecular weight cutoff of 500 Da for 24 h, with the water changed every 8 h. After dialysis, the retentate was freeze-dried to obtain the modified intermediate.

[0019] Example 1: This example provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 5 parts carbon nanotubes, 0.5 parts modified intermediate, 2 parts gallium indium tin alloy, 0.3 parts PVP K30, 1 part PVDF and 93.2 parts NMP.

[0020] This embodiment also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve 0.5 parts of the modified intermediate in 20 parts of NMP to obtain an intermediate solution. Disperse 5 parts of carbon nanotubes in the remaining 73.2 parts of NMP using ultrasonication at 400 W for 15 min to obtain a dispersion. Heat 2 parts of gallium indium tin alloy to 30°C until completely melted, sonicate for 3 min, and then quickly add it to the dispersion. Stir until homogeneous to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min, and the temperature is controlled below 30℃ to obtain the pre-dispersed slurry. Step 3: Add 0.3 parts of PVP K30 and 1 part of PVDF to the pre-dispersed slurry, and homogenize for 2 hours at a speed of 3000 rpm while controlling the temperature at 45℃ to fully deflocculate and uniformly disperse the carbon nanotubes, thus obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it at a speed of 50 rpm to obtain a highly stable conductive carbon nanotube slurry.

[0021] Example 2: This example provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 4 parts carbon nanotubes, 0.8 parts modified intermediate, 2 parts gallium indium tin alloy, 0.2 parts PAN, 1.5 parts PI and 93.5 parts DMF.

[0022] This embodiment also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve 0.8 parts of the modified intermediate in 20 parts of DMF to obtain an intermediate solution. Disperse 4 parts of carbon nanotubes in the remaining 73.5 parts of NMP using ultrasonication at 400 W for 15 min to obtain a dispersion. Heat 2 parts of gallium indium tin alloy to 30°C until completely melted, sonicate for 3 min, and then quickly add it to the dispersion. Stir evenly to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min, and the temperature is controlled below 30℃ to obtain the pre-dispersed slurry. Step 3: Add 0.2 parts of PAN and 1.5 parts of PI to the pre-dispersed slurry, and homogenize for 2 hours at a speed of 3000 rpm and a temperature of 45℃ to fully deflocculate and uniformly disperse the carbon nanotubes, thus obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it at a speed of 50 rpm to obtain a highly stable carbon nanotube conductive slurry.

[0023] Example 3: This example provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 6 parts carbon nanotubes, 0.2 parts modified intermediate, 2 parts gallium indium tin alloy, 0.4 parts PVB, 1.2 parts PMMA and 92.2 parts NMP.

[0024] This embodiment also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve 0.2 parts of the modified intermediate in 20 parts of NMP to obtain an intermediate solution. Disperse 6 parts of carbon nanotubes in the remaining 72.2 parts of NMP using ultrasonication at 400 W for 15 min to obtain a dispersion. Heat 2 parts of gallium indium tin alloy to 30°C until completely melted, sonicate for 3 min, and then quickly add it to the dispersion. Stir until homogeneous to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min, and the temperature is controlled below 30℃ to obtain the pre-dispersed slurry. Step 3: Add 0.4 parts PVB and 1.2 parts PMMA to the pre-dispersed slurry, then homogenize for 2 hours at a speed of 3000 rpm and control the temperature at 45℃ to fully deflocculate and uniformly disperse the carbon nanotubes, thus obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it at a speed of 50 rpm to obtain a highly stable conductive carbon nanotube slurry.

[0025] Example 4: This example provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 8 parts carbon nanotubes, 1 part modified intermediate, 2 parts gallium indium tin alloy, 0.5 parts PVP K30, 2 parts PMMA and 88.5 parts DMF.

[0026] This embodiment also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve 1 part of the modified intermediate in 20 parts of DMF to obtain an intermediate solution. Disperse 8 parts of carbon nanotubes in the remaining 68.5 parts of NMP by ultrasonication at 400 W for 15 min to obtain a dispersion. Heat 2 parts of gallium indium tin alloy at 30°C until completely melted, sonicate for 3 min, and then quickly add it to the dispersion. Stir evenly to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min, and the temperature is controlled below 30℃ to obtain the pre-dispersed slurry. Step 3: Add 0.5 parts of PVP K30 and 2 parts of PMMA to the pre-dispersed slurry, and homogenize for 2 hours at a speed of 3000 rpm while controlling the temperature at 45℃ to fully deflocculate and uniformly disperse the carbon nanotubes, thus obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it at a speed of 50 rpm to obtain a highly stable conductive carbon nanotube slurry.

[0027] Example 5: This example provides a highly stable carbon nanotube conductive paste, which comprises the following raw materials in parts by weight: 3 parts carbon nanotubes, 0.1 parts modified intermediate, 2 parts gallium indium tin alloy, 0.1 parts PVB, 0.5 parts PI and 96.3 parts NMP.

[0028] This embodiment also provides a method for preparing a highly stable carbon nanotube conductive paste, the specific steps of which are as follows: Step 1: Dissolve 0.1 parts of the modified intermediate in 20 parts of NMP to obtain an intermediate solution. Disperse 3 parts of carbon nanotubes in the remaining 76.3 parts of NMP using ultrasonication at 400 W for 15 min to obtain a dispersion. Heat 2 parts of gallium indium tin alloy to 30°C until completely melted, sonicate for 3 min, and then quickly add it to the dispersion. Stir until homogeneous to obtain a suspension. Step 2: Under stirring conditions, the intermediate solution is slowly added to the suspension. After the addition is complete, ultrasonic dispersion is continued for 30 min, and the temperature is controlled below 30℃ to obtain the pre-dispersed slurry. Step 3: Add 0.1 parts PVB and 0.5 parts PI to the pre-dispersed slurry, then homogenize for 2 hours at a speed of 3000 rpm and control the temperature at 45℃ to fully deflocculate and uniformly disperse the carbon nanotubes, thus obtaining a dispersed slurry. Vacuum stir the dispersed slurry to degas it at a speed of 50 rpm to obtain a highly stable conductive carbon nanotube slurry.

[0029] Comparative Example 1: The difference from Example 1 is that no modified intermediate was added, the amount of PVP K30 was 0.8 parts, and the rest was the same as in Example 1; Comparative Example 2: The difference from Example 1 is that an equal amount of unmodified PAMAM was used instead of the modified intermediate, and the rest is the same as in Example 1.

[0030] Microscopic morphology characterization: The morphology of the conductive pastes prepared in Example 1 and Comparative Example 1 was examined using field emission scanning electron microscopy to evaluate their dispersion uniformity and carbon nanotube aggregation. The results are shown in the figure. Figure 1 .

[0031] Dispersibility study: The dispersibility of the conductive pastes prepared in Examples 1-3 and Comparative Examples 1-2 was analyzed using a nanolaser particle size analyzer. The refractive index Nd of the corresponding solvent was selected as the detection parameter. The particle size results are shown in […]. Figure 2 .

[0032] Resistivity investigation: The resistivity characteristics of the conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2 were determined using the four-probe method. The conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2 were dried and pressed into discs with a diameter of 20 mm. The probe spacing was 1 mm, and the resistivity was measured at six different sites on the sample surface. The average value results are shown in [the table below]. Figure 3 .

[0033] Stability study: The conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2 were tested using a rotational viscometer, denoted as η0. The pastes were sealed in glass bottles and kept at a constant temperature of 25°C. The viscosity of the conductive pastes after 3 months was measured and denoted as η1. The viscosity change rate (%) was calculated as (η1-η0) / η0×100%. The results are shown in […]. Figure 4After 3 months, the sedimentation of the conductive paste in Example 1 and Comparative Example 2 is as follows: Figure 5 As shown.

[0034] Electrode sheet resistance uniformity assessment: The conductive pastes prepared in Examples 1-5 and Comparative Examples 1-2 were coated onto aluminum foil using a doctor blade, with a wet film thickness of 100 μm. After drying at 120℃ for 1 h, the sheet resistance was measured at 9 points (3×3 grid) on the electrode using a four-probe sheet resistance meter. The relative standard deviation (RSD) was calculated, and the results are shown below. Figure 6 .

[0035] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0036] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A highly stable carbon nanotube conductive paste, characterized in that, The conductive paste comprises the following raw materials in parts by weight: 3-8 parts carbon nanotubes, 0.1-1 parts modified intermediate, 2 parts gallium indium tin alloy, 0.1-0.5 parts dispersant, 0.5-2 parts binder, and 88.5-96.5 parts organic solvent; The modified intermediate includes the following raw materials: PAMAM, PCA, 1,3-propanesulfonate lactone and NaBH4; The method for preparing the modified intermediate is as follows: S1: Dissolve PAMAM and PCA separately to obtain PAMAM solution and PCA solution. Add PCA solution to PAMAM solution to react and obtain reaction solution; S2: After the reaction solution is cooled, NaBH4 is added to reduce, precipitate, filter, collect the precipitate, wash and dry to obtain Py-PAMAM; S3: After dissolving Py-PAMAM, 1,3-propanesulfonic acid lactone is added to react and a sulfonated intermediate is obtained. The sulfonated intermediate is cooled and precipitated, filtered, and the precipitate is collected, washed, purified, and dried to obtain the modified intermediate.

2. The highly stable carbon nanotube conductive paste according to claim 1, characterized in that, The mass ratio of PAMAM, PCA, 1,3-propanesulfonic acid lactone and NaBH4 is 10:0.67:10.6:0.

22.

3. The highly stable carbon nanotube conductive paste according to claim 1, characterized in that, The dispersant is selected from any one of PVP, PAN and PVB.

4. The highly stable carbon nanotube conductive paste according to claim 3, characterized in that, The adhesive is selected from any one of PVDF, PI and PMMA.

5. The highly stable carbon nanotube conductive paste according to claim 4, characterized in that, The organic solvent is NMP or DMF.

6. The highly stable carbon nanotube conductive paste according to claim 1, characterized in that, The gallium-indium-tin alloy has the following composition by mass percentage: 68.5% gallium, 21.5% indium, and 10% tin.

7. A method for preparing a highly stable carbon nanotube conductive paste according to any one of claims 1-6, characterized in that, The specific steps are as follows: Step 1: Dissolve the modified intermediate in a portion of the organic solvent to obtain an intermediate solution. Disperse the carbon nanotubes in the remaining organic solvent to obtain a dispersion. Heat and sonicate the gallium indium tin alloy and add it to the dispersion to obtain a suspension. Step 2: Slowly add the intermediate solution to the suspension and ultrasonically disperse to obtain a pre-dispersed slurry; Step 3: After adding dispersant and binder to the pre-dispersed slurry, homogenize to obtain a dispersed slurry. Degas the dispersed slurry to obtain a highly stable carbon nanotube conductive slurry.