Methods to improve the magnetic properties of NdFeB sheet magnets
By employing multi-frequency eddy current scanning and differentiated processing, the problem of insufficient compensation on one side or excessive compensation on the other side during the diffusion process of neodymium iron boron thin sheet magnets was solved, achieving uniformity and controllability of magnetic properties.
Patent Information
- Application Number
- CN202611344428.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-10
AI Technical Summary
Existing technologies struggle to balance the coercivity and remanence on both sides of neodymium iron boron sheet magnets, leading to magnetic moment dispersion. Furthermore, during the diffusion process, insufficient compensation on one side or excessive compensation on the other can easily occur.
The equivalent damage depth on both sides of the NdFeB thin sheet magnet was determined by multi-frequency eddy current scanning, the amount of material removed was allocated differently, and the Tb-Cu diffusion source surface density and diffusion time were adjusted according to the residual damage depth to ensure the uniformity of treatment on both sides and the controllability of the thickness direction.
This method achieves a balance in the damage depth on both sides of the neodymium iron boron thin-film magnet, avoiding excessive or insufficient diffusion and improving the uniformity and controllability of magnetic properties.
Smart Images

Figure CN123072912A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of rare earth permanent magnet material processing technology, specifically to a method for improving the magnetic properties of neodymium iron boron thin-film magnets. Background Technology
[0002] After wire cutting and grinding, the surface of neodymium iron boron (NdFeB) thin-film magnets is prone to grain breakage, exposed grain boundaries, and localized oxidation areas. In actual production, heavy rare earth grain boundary diffusion is usually used to improve coercivity. Existing diffusion processes generally set the surface treatment amount, diffusion source coating amount, and diffusion time uniformly according to the magnet thickness.
[0003] However, for thin-film magnets, especially in machining scenarios where the two sides of the same thin film undergo grinding wheel entry and exit facets respectively, the surface damage depths on both sides are not consistent. If equal-volume grinding and double-sided equal-volume diffusion are still used, the damaged grain boundaries on one side may not be adequately compensated, while the heavy rare earth elements on the other side may diffuse excessively. At the same time, due to the small thickness of the magnet, the diffusion fronts on both sides tend to approach or overlap in the middle of the thickness, causing local heavy rare earth enrichment. This makes it difficult to simultaneously improve coercivity and maintain remanence, thus leading to magnetic moment dispersion in the thin-film magnet. Summary of the Invention
[0004] The purpose of this invention is to provide a method for improving the magnetic properties of neodymium iron boron sheet magnets, thereby overcoming the shortcomings in the prior art.
[0005] To achieve the above objectives, the present invention provides the following technical solution: a method for improving the magnetic properties of neodymium iron boron sheet magnets, comprising: Multi-frequency eddy current scanning was performed on the first and second surfaces of the sliced NdFeB thin sheet magnet, and the equivalent damage depth of the two surfaces was determined based on the impedance amplitude and phase change at different frequencies. Based on the equivalent damage depth, the initial thickness of the sheet and the target thickness, a double-sided material removal constraint is constructed. The first removal amount and the second removal amount that minimize the difference in residual damage depth between the two surfaces are obtained, and the two surfaces are quantitatively polished accordingly. The Tb-Cu diffusion source surface density of the two surfaces is determined based on the residual damage depth of the two surfaces obtained after polishing and the target thickness of the sheet. The side with a larger residual damage depth corresponds to a higher diffusion source surface density. The diffusion time is determined based on the target thickness and the pre-calibrated diffusion depth-time relationship, so that the sum of the predicted diffusion depths on both sides is less than the target thickness. The two surfaces are coated according to the diffusion source surface density, and vacuum diffusion and low-temperature aging treatment are performed according to the diffusion time to obtain neodymium iron boron thin sheet magnets.
[0006] Preferably, the eddy current detection probe is scanned relative to the detection areas of the first surface and the second surface, respectively, and the complex impedance response of the corresponding surface is collected at multiple detection frequencies. For any detection frequency, the corresponding impedance amplitude and impedance phase are obtained according to the complex impedance response, and the impedance amplitude and impedance phase are compared with the corresponding reference response to obtain the impedance amplitude change and phase change at the corresponding detection frequency. The impedance amplitude change and phase change of the first surface are combined according to the detection frequency to obtain the multi-frequency impedance change data of the first surface, and the multi-frequency impedance change data of the second surface is obtained in the same way.
[0007] Preferably, the multi-frequency impedance change data of the first surface and the second surface are matched or inverted with the pre-obtained equivalent damage depth correspondence, and the depth value corresponding to the corresponding multi-frequency impedance change data is determined as the equivalent damage depth of the corresponding surface, so as to obtain the equivalent damage depth of the first surface and the equivalent damage depth of the second surface.
[0008] Preferably, the total material removal amount on both sides is determined based on the initial thickness and target thickness of the sheet.
[0009] Preferably, the residual damage depth of the first surface is determined based on the equivalent damage depth of the first surface and the first removal amount, and the residual damage depth of the second surface is determined based on the equivalent damage depth of the second surface and the second removal amount. Under the condition of satisfying the double-sided material removal constraint, the first removal amount and the second removal amount are determined.
[0010] Preferably, when the total material removal amount on both sides is insufficient to make the residual damage depth of both the first surface and the second surface zero, the first removal amount and the second removal amount are allocated according to the relationship between the equivalent damage depth of the first surface and the equivalent damage depth of the second surface, so that the side with the larger equivalent damage depth corresponds to a larger material removal amount, and the first removal amount and the second removal amount are used as the quantitative polishing control amount for the first surface and the second surface, respectively, to remove material so that the thickness of the sheet after quantitative polishing reaches the target thickness.
[0011] Preferably, the residual damage depth of the first surface and the residual damage depth of the second surface are set after polishing; the residual damage depth of the first surface and the residual damage depth of the second surface are compared, and the Tb-Cu diffusion source surface density of the first surface and the Tb-Cu diffusion source surface density of the second surface are determined in a manner in which the Tb-Cu diffusion source surface density and the residual damage depth are configured in the same direction.
[0012] Preferably, based on a pre-defined relationship between diffusion depth and time, a first predicted diffusion depth extending from the first surface into the interior of the sheet and a second predicted diffusion depth extending from the second surface into the interior of the sheet are obtained at the candidate diffusion time; the first predicted diffusion depth and the second predicted diffusion depth are superimposed and compared with the target thickness to determine the diffusion time that meets the requirements from the candidate diffusion times.
[0013] Preferably, the first and second surfaces after quantitative polishing are cleaned; a corresponding amount of Tb-Cu diffusion source is placed on the first surface according to the Tb-Cu diffusion source areal density of the first surface, and a corresponding amount of Tb-Cu diffusion source is placed on the second surface according to the Tb-Cu diffusion source areal density of the second surface, so as to control the amount of Tb-Cu diffusion source on the two surfaces respectively; the double-sided coated NdFeB thin sheet magnet is placed in a vacuum heat treatment environment and vacuum diffusion is performed according to the diffusion time.
[0014] Preferably, during the vacuum diffusion process, the Tb-Cu diffusion source disposed on the first surface diffuses from the first surface into the interior of the magnet, and the Tb-Cu diffusion source disposed on the second surface diffuses from the second surface into the interior of the magnet. The diffusion duration on both sides is limited by the diffusion time. After the vacuum diffusion is completed, the NdFeB thin sheet magnet is subjected to low-temperature aging treatment, and then cooled after the low-temperature aging treatment is completed to obtain the NdFeB thin sheet magnet.
[0015] The technical effects and advantages provided by the present invention in the above technical solution are as follows: Compared to existing methods for processing NdFeB sheet magnets, which typically involves removing equal amounts from both surfaces based on a uniform processing allowance, the core technical approach of this invention lies in: separately obtaining the equivalent damage depth of the first and second surfaces; and, under the constraints of the initial and target thickness of the sheet, allocating the first and second removal amounts based on the difference in damage levels on both sides, so that the material removal process directly corresponds to the actual damage state of each surface. This reduces the possibility of insufficient removal on the deeper damaged side and excessive removal on the shallower damaged side, resulting in a more balanced residual damage depth on both surfaces after polishing. This provides a more consistent and quantifiable surface foundation for subsequent double-sided diffusion and avoids mismatches in double-sided processing caused by using only the total thickness as the processing basis.
[0016] Furthermore, compared to existing methods that use the same amount of diffusion source on both sides and perform grain boundary diffusion at a fixed process time, this invention determines the Tb-Cu diffusion source areal density based on the residual damage depth of both surfaces after polishing. This ensures that the side with a larger residual damage depth corresponds to a higher diffusion source areal density. Simultaneously, the diffusion time is limited by combining the target thickness of the sheet and a pre-calibrated diffusion depth-time relationship, ensuring that the sum of the predicted diffusion depths on both sides is less than the target thickness. This invention enables the diffusion source allocation to match the actual residual damage state on both sides and constrains the diffusion fronts on both sides in the thickness direction. This reduces the possibility of insufficient diffusion compensation on one side, excessive diffusion on the other side, and excessive proximity or overlap of the diffusion regions on both sides. This provides a direct technical basis for balancing the processing balance on both sides of the sheet magnet and the controllability of diffusion in the thickness direction. Attached Figure Description
[0017] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this invention. For those skilled in the art, other drawings can be obtained based on these drawings.
[0018] Figure 1 This is a flowchart of the method of the present invention.
[0019] Figure 2 This is a schematic diagram of the double-sided multi-frequency eddy current scanning of the present invention.
[0020] Figure 3 This is a schematic diagram illustrating the determination of the equivalent damage depth on both surfaces according to the present invention. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0022] Example 1, please refer to Figure 1 , Figure 2 and Figure 3 As shown in this embodiment, the method for improving the magnetic properties of NdFeB thin-film magnets includes: Step S1 involves performing multi-frequency eddy current scanning on the first and second surfaces of the sliced NdFeB thin-film magnet, respectively, to determine the equivalent damage depth of the two surfaces based on the impedance amplitude and phase changes at different frequencies. Here, the first and second surfaces refer to the two surfaces of the NdFeB thin-film magnet positioned opposite each other along the thickness direction after slicing. Multi-frequency eddy current scanning refers to using alternating electromagnetic fields of two or more different frequencies to detect the corresponding surfaces and obtaining the eddy current impedance response corresponding to each detection frequency. Since the eddy current fields corresponding to different detection frequencies have different response sensitivities to different depths near the material's surface, using multi-frequency information can obtain a more complete near-surface state characterization compared to using a single frequency.
[0023] It is important to understand that the equivalent damage depth described in this embodiment is not limited to the actual geometric depth of a specific crack, a broken grain, or a localized oxidation region. Rather, it is a depth quantity used to characterize the comprehensive impact of the damaged surface area on the multi-frequency eddy current response after slicing. In other words, for the surface grain breakage, grain boundary exposure, and localized oxidation states formed during the slicing process, the changes they cause to the near-surface electromagnetic response of the magnet are converted into depth parameters that can be used for subsequent calculations of the amount of material removed from both sides. For conductive materials, the amplitude and phase of the eddy current impedance can change with the state of the object being detected and the detection frequency. The amplitude and phase information under multi-frequency conditions can be used to characterize the material state at different depth locations.
[0024] Considering that the first and second surfaces of the NdFeB thin-film magnet may be in different entry and exit states during the slicing process, and the surface damage levels of the two surfaces may not be consistent, it is necessary to obtain the equivalent damage depth of each surface before determining the subsequent first and second removal amounts. If equal amounts of material are removed from both surfaces directly according to the total thickness of the thin film, it is impossible to provide an input quantity that reflects the actual differences in the two sides for the subsequent double-sided material removal constraints, making it difficult to separately constrain the residual damage of the two surfaces in subsequent calculations. Therefore, this step first transforms the surface states that cannot be directly used for quantitative material removal into two comparable equivalent damage depths.
[0025] Specifically, when detecting the first surface, the eddy current detection probe scans the area to be detected relative to the first surface, and the complex impedance response of the probe is acquired at multiple detection frequencies during the scanning process. After the detection of the first surface is completed, the second surface is scanned under the same detection method to obtain the complex impedance response of the second surface at the corresponding detection frequency. The scanning of the first and second surfaces is independent of each other, but they use corresponding detection frequencies and impedance data expression methods to make the data obtained from the two surfaces comparable. Multi-frequency eddy current scanning can be performed by sequentially changing the excitation frequency and acquiring impedance data frequency by frequency, or by using an excitation signal containing multiple frequency components and extracting the corresponding frequency impedance data from the obtained response. Both of these methods are optional implementations of multi-frequency eddy current scanning in this embodiment. Multi-frequency measurement and extraction of material or geometric state information from different frequency responses are existing implementation ideas in eddy current detection.
[0026] Furthermore, for any surface and any detection frequency, the acquired complex impedance is expressed as a complex quantity composed of real and imaginary parts, and the corresponding impedance amplitude and impedance phase are obtained accordingly. To characterize the changes in the surface after slicing relative to the reference state, the impedance amplitude and impedance phase obtained at each detection frequency can be compared with the corresponding reference response to form impedance amplitude changes and phase changes, respectively. As an optional implementation, the reference response can be obtained using a reference response with a material state corresponding to the NdFeB thin-film magnet to be tested; this embodiment does not limit the specific method of obtaining the reference response, its purpose is to provide a unified basis for comparison of response changes at different detection frequencies.
[0027] Furthermore, the impedance amplitude and phase changes of the first surface are combined according to the detection frequency to obtain multi-frequency impedance change data for the first surface; the multi-frequency impedance change data for the second surface is obtained in the same way. Since the eddy current responses at higher and lower frequencies have different depth sensitivity ranges, the impedance change at a single frequency is not directly used as the damage depth. Instead, the range of surface damage along the depth direction is determined by combining the impedance amplitude and phase changes corresponding to multiple detection frequencies. As a specific implementation method, the multi-frequency impedance change data can be matched or inverted with the pre-obtained equivalent damage depth correspondence, and the depth value corresponding to the current multi-frequency response is determined as the equivalent damage depth of the corresponding surface. Parameter inversion using multi-frequency eddy current data combined with frequency-related responses is an existing method for quantitative eddy current analysis.
[0028] Step S2: Based on the equivalent damage depth, the initial thickness of the sheet, and the target thickness, a double-sided material removal constraint is constructed. A first removal amount and a second removal amount that minimize the difference in residual damage depth between the two surfaces are obtained, and quantitative polishing is performed on both surfaces accordingly. The equivalent damage depth includes the equivalent damage depth of the first surface and the equivalent damage depth of the second surface determined in the preceding steps; the initial thickness of the sheet refers to the thickness between the first and second surfaces when the NdFeB magnet sheet has been sliced but before the quantitative polishing in this step has been performed; the target thickness refers to the sheet thickness required after material removal from the first and second surfaces. The first removal amount and the second removal amount respectively characterize the thickness of material removed from the first and second surfaces along the sheet thickness direction.
[0029] The two equivalent damage depths obtained from the aforementioned multi-frequency eddy current scanning reflect the degree to which the first and second surfaces are affected by the slicing. When the equivalent damage depths of the two surfaces are different, if the total material removal amount is evenly distributed to the two surfaces according to the target thickness, the side with the larger equivalent damage depth may retain a relatively deeper damaged area, while the side with the smaller equivalent damage depth may experience unnecessary material removal. Furthermore, subsequent steps require using the residual damage depths of the two surfaces after polishing to determine the extent of damage on both sides. The areal density of the diffusion source is crucial; therefore, if the residual damage state of both surfaces cannot be clearly obtained in this step, the subsequent diffusion source areal density on both sides will lack corresponding surface state input. Based on this, this step does not simply perform equal thinning according to dimensional requirements, but rather, while meeting the target thickness, uses reducing the difference in residual damage depth between the two surfaces as the basis for allocating the amount of material removed.
[0030] Specifically, let the equivalent damage depth of the first surface be... The equivalent damage depth of the second surface is The initial thickness of the thin sheet is The target thickness is The first amount to be removed is The second removal amount is First, the total allowable material removal on both sides is determined based on the initial thickness and target thickness of the sheet, i.e.: ; in, This represents the cumulative material thickness that needs to be removed from the first and second surfaces to achieve the target thickness of the neodymium iron boron sheet magnet from its initial thickness. This establishes a thickness constraint. And satisfy: ; The purpose of the above constraints is to ensure that, regardless of how the first and second removal amounts are allocated, their sum is consistent with the total material removal amount determined by the initial and target thickness of the sheet, thereby avoiding changes to the final sheet thickness in order to reduce surface damage differences.
[0031] Furthermore, when determining the first and second removal amounts, the reduction effect of material removal on the corresponding surface equivalent damage area is included in the calculation. The residual damage depth of the first surface after removal can be expressed as: ; The residual damage depth of the second surface after removal can be expressed as: ; in, and These are the residual damage depths of the first and second surfaces, respectively. When the corresponding removal amount is less than the equivalent damage depth of the surface, the difference between the two represents the equivalent damage depth remaining after material removal. When the corresponding removal amount reaches or exceeds the equivalent damage depth, the residual damage depth of the surface is considered zero. It should be noted that the residual damage depth here still uses the technical meaning of the aforementioned equivalent damage depth to describe the depth corresponding to the damage effect of the remaining surface layer after quantitative polishing, and is not limited to the geometric size of a single crack or a single grain defect.
[0032] Based on this, taking the minimum difference in residual damage depth between the two surfaces as the objective for determining the first and second removal amounts, it can be expressed as: ; that is: ; And simultaneously satisfy the aforementioned as well as , The constraint relationship is that neither is less than zero. The purpose of the above calculation is to distribute the finite total material removal amount between the two surfaces in accordance with their respective equivalent damage depths, rather than pre-fixing the two surfaces to have the same removal amount.
[0033] In practice, it is understood that when the total material removal is insufficient to completely remove the equivalent damage areas on both surfaces, the first and second removal amounts are preferentially reduced by solving the above constraints. and The material is allocated according to the direction of the difference. For example, when the equivalent damage depth of the first surface is greater than that of the second surface, the required first removal amount can be correspondingly greater than the second removal amount, under the condition of meeting the target thickness, to reduce the relatively large damage depth of the first surface. Conversely, when the equivalent damage depth of the second surface is larger, the material removal amount of the second surface is increased accordingly. If the total material removal amount is sufficient to make the residual damage depth of both surfaces reach zero, then the target thickness is met. The combination of removal amounts can minimize the difference in residual damage depth, and then the first and second removal amounts are determined within the range that satisfies the constraint of total material removal amount.
[0034] Furthermore, after obtaining the first and second removal amounts, the first and second removal amounts are used as quantitative polishing control amounts for the first and second surfaces, respectively, to remove material from both surfaces. The quantitative polishing can be achieved using existing polishing or grinding methods in the surface finishing of NdFeB magnets that allow control over the material removal thickness. This embodiment does not limit the specific polishing equipment or abrasive type. During implementation, the first surface can be quantitatively polished first according to the first removal amount, and then the second surface can be quantitatively polished according to the second removal amount; alternatively, other sequences can be used while controlling the material removal amounts of the two surfaces separately. Regardless of the specific implementation method, the cumulative actual removal amount of the two surfaces is controlled based on achieving the target thickness of the sheet.
[0035] Step S3: Determine the Tb-Cu diffusion source surface density on both surfaces based on the residual damage depth and the target thickness of the sheet obtained after polishing. The side with a larger residual damage depth corresponds to a higher diffusion source surface density. Determine the diffusion time based on the target thickness and the pre-calibrated diffusion depth-time relationship, so that the sum of the predicted diffusion depths on both sides is less than the target thickness.
[0036] It should be understood that the residual damage depths of the two surfaces are respectively the residual damage depths of the first surface and the second surface after the aforementioned quantitative polishing, used to characterize the equivalent depth of the two surfaces still affected by the slice damage after quantitative polishing. The Tb-Cu diffusion source areal density refers to the amount of Tb-Cu diffusion source per unit area calculated based on the surface area of the corresponding magnet, used to characterize the degree to which Tb-Cu diffusion source is subsequently provided from the corresponding surface to the interior of the magnet. The predicted diffusion depth refers to the expected diffusion distance formed from the corresponding surface to the interior of the thin film, obtained under determined diffusion conditions and diffusion time, based on a pre-calibrated diffusion depth-time relationship, and is not a direct measurement result of the actual diffusion front position after diffusion treatment.
[0037] Considering that the aforementioned quantitative polishing aims to reduce the difference in residual damage depth between the two surfaces, but constrained by the target thickness of the sheet, the residual damage depth of the two surfaces may still differ. If the same Tb-Cu diffusion source areal density is used for the first and second surfaces in this case, the bifacial distribution of the diffusion source cannot correspond to the actual surface state retained after quantitative polishing. On the other hand, for thin NdFeB sheet magnets, if bifacial diffusion is performed only based on the conventional diffusion time without constraining the diffusion depth on both sides relative to the target thickness of the sheet, the diffusion regions on both sides may become excessively close or even overlap in the thickness direction. Therefore, this step simultaneously uses the residual damage depth of the two surfaces to determine the bifacial distribution relationship of the diffusion source and uses the target thickness of the sheet to limit the diffusion time, thereby providing a definite diffusion source areal density and diffusion time for subsequent actual coating and vacuum diffusion.
[0038] Specifically, let the residual damage depth of the first surface be... The residual damage depth on the second surface is The target thickness of the thin film is The Tb-Cu diffusion source surface density on the first surface is The Tb-Cu diffusion source surface density on the second surface is First, compare. and And determine in combination with the target thickness of the thin film and Among them, under the same corresponding process conditions, the Tb-Cu diffusion source areal density and residual damage depth are configured in the same direction, that is, when At that time, when At that time, When the residual damage depths on both surfaces are the same or in an equivalent state allowed by the predetermined process, the corresponding identical Tb-Cu diffusion source areal density can be used. The specific values for each Tb-Cu diffusion source areal density can be determined within the allowable diffusion source dosage range of the existing Tb-Cu grain boundary diffusion process, based on the residual damage depth and the target thickness of the thin film, through process calibration relationships, established correspondences, or table lookup methods. This embodiment does not impose a unique limitation on specific values. Thus, the side with a larger residual damage depth obtains a relatively high Tb-Cu diffusion source areal density, and the side with a smaller residual damage depth obtains a relatively low Tb-Cu diffusion source areal density, ensuring that the double-sided configuration of the diffusion source corresponds to the residual damage state on both sides formed in the previous step.
[0039] Furthermore, after obtaining the Tb-Cu diffusion source areal density of the first and second surfaces, the diffusion time is determined based on the target thickness and the pre-calibrated diffusion depth-time relationship. The pre-calibrated diffusion depth-time relationship refers to the correspondence between the diffusion time and the diffusion depth formed from the magnet surface inwards, obtained in advance under predetermined process conditions corresponding to subsequent diffusion treatment. This correspondence can be represented by a calibration data table, calibration curve, or a correspondence formed from calibration data. Its purpose is to obtain the corresponding predicted diffusion depth based on the selected diffusion time, without having to reverse-determine the processing time after actual diffusion is completed.
[0040] In practice, for the first surface, candidate diffusion times are obtained based on a pre-defined relationship between diffusion depth and time. The first predicted diffusion depth For the second surface, the second predicted diffusion depth is obtained in the same manner. The first and second predicted diffusion depths are measured along the first and second surfaces inwards from the thin film, respectively. The two predicted diffusion depths are then combined and judged, with the target thickness of the thin film used as a thickness direction constraint, to ensure that the determined diffusion time satisfies: In other words, when selecting a diffusion time from the pre-defined diffusion depth-time relationship, it is not only necessary to determine whether a corresponding diffusion depth can be formed on one side, but also to superimpose the predicted diffusion depths generated by the first surface and the second surface respectively, and compare them with the target thickness of the thin sheet. If the sum of the predicted diffusion depths on both sides corresponding to a candidate diffusion time does not satisfy the above relationship, then the candidate diffusion time is not used as the subsequent diffusion time, and a diffusion time that satisfies the above thickness constraint is selected from the pre-defined diffusion depth-time relationship.
[0041] Step S4: Coat the two surfaces according to the diffusion source surface density, and perform vacuum diffusion and low-temperature aging treatment according to the diffusion time to obtain neodymium iron boron thin sheet magnet.
[0042] In one embodiment of the present invention, after obtaining the Tb-Cu diffusion source surface density corresponding to the first and second surfaces and the diffusion time that satisfies the condition that the sum of the predicted diffusion depths on both sides is less than the target thickness of the sheet, the two surfaces are coated according to the diffusion source surface density, and vacuum diffusion and low-temperature aging treatment are performed according to the diffusion time to obtain a neodymium iron boron sheet magnet.
[0043] Specifically, the first and second surfaces, after quantitative polishing, are first cleaned to remove residual particles, oil, or other surface residues that may affect the adhesion of the diffusion source. Then, based on the Tb-Cu diffusion source areal density of the first surface determined in the previous step, a corresponding amount of Tb-Cu diffusion source is uniformly applied to the first surface; similarly, based on the Tb-Cu diffusion source areal density of the second surface, a corresponding amount of Tb-Cu diffusion source is uniformly applied to the second surface. It should be understood that "separate coating" means that the amount of diffusion source used on the first and second surfaces is controlled by their respective diffusion source areal densities. When the residual damage depths of the two surfaces are different, the Tb-Cu diffusion source areal densities on the two surfaces are correspondingly different, thus maintaining the aforementioned differentiated configuration relationship between the two surfaces during subsequent diffusion treatment.
[0044] Furthermore, the double-sided coated NdFeB thin-film magnet is placed in a vacuum heat treatment environment for vacuum diffusion treatment, and the diffusion treatment time is controlled to the diffusion time determined in the previous step. As an optional implementation, the diffusion temperature, vacuum conditions, and heating / cooling methods used in vacuum diffusion can be set according to the process conditions disclosed in existing Tb-Cu grain boundary diffusion processes, and the present invention does not impose a unique limitation on their specific values. During the diffusion process, the Tb-Cu diffusion sources on the first and second surfaces diffuse from the corresponding surfaces into the interior of the magnet, and their diffusion duration is jointly limited by the diffusion time, so that the actual processing process corresponds to the aforementioned constraint that "the sum of the predicted diffusion depths on both sides is less than the target thickness of the thin film".
[0045] After vacuum diffusion, the NdFeB thin-film magnet undergoes low-temperature aging treatment. This low-temperature aging treatment can employ a low-temperature heat treatment method disclosed in existing sintered NdFeB magnet grain boundary diffusion processes, which further adjusts the state of the diffused grain boundaries and related phases. After low-temperature aging, cooling is performed to obtain the treated NdFeB thin-film magnet.
[0046] This invention addresses the problem of inconsistent surface damage on both sides of a NdFeB thin-film magnet after slicing, and the tendency for diffusion at the grain boundaries on both sides to influence each other in the thickness direction. First, multi-frequency eddy current scanning is used to quantify the equivalent damage depth of the first and second surfaces. Then, under the constraint of the target thickness of the thin film, the amount of material removed from both sides is differentiated to make the residual damage state of the two surfaces after polishing more balanced. Based on this, the Tb-Cu diffusion source areal density is determined according to the difference in residual damage depth on both sides, and the diffusion time is limited by combining the target thickness of the thin film and a pre-calibrated diffusion depth-time relationship. This ensures that the side with greater residual damage receives a higher diffusion source configuration, while avoiding excessive overlap of the diffusion regions on both sides in the thickness direction of the thin film. This forms a continuous closed-loop processing approach of "surface damage detection - differentiated removal - differentiated diffusion source configuration - diffusion depth constraint".
[0047] The above description is merely a specific embodiment of this application, but the scope of protection of this application is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in this application should be included within the scope of protection of this application.
Claims
1. A method for improving the magnetic properties of neodymium iron boron sheet magnets, characterized in that, include: Multi-frequency eddy current scanning was performed on the first and second surfaces of the sliced NdFeB thin sheet magnet, and the equivalent damage depth of the two surfaces was determined based on the impedance amplitude and phase change at different frequencies. Based on the equivalent damage depth, the initial thickness of the sheet and the target thickness, a double-sided material removal constraint is constructed. The first removal amount and the second removal amount that minimize the difference in residual damage depth between the two surfaces are obtained, and the two surfaces are quantitatively polished accordingly. The Tb-Cu diffusion source surface density of the two surfaces is determined based on the residual damage depth of the two surfaces obtained after polishing and the target thickness of the sheet. The side with a larger residual damage depth corresponds to a higher diffusion source surface density. The diffusion time is determined based on the target thickness and the pre-calibrated diffusion depth-time relationship, so that the sum of the predicted diffusion depths on both sides is less than the target thickness. The two surfaces are coated according to the diffusion source surface density, and vacuum diffusion and low-temperature aging treatment are performed according to the diffusion time to obtain neodymium iron boron thin sheet magnets.
2. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 1, characterized in that, The eddy current detection probe is scanned relative to the detection areas of the first and second surfaces, respectively, and the complex impedance responses of the corresponding surfaces are collected at multiple detection frequencies. For any detection frequency, the corresponding impedance amplitude and impedance phase are obtained based on the complex impedance response, and the impedance amplitude and impedance phase are compared with the corresponding reference response to obtain the impedance amplitude change and phase change at the corresponding detection frequency. The impedance amplitude change and phase change of the first surface are combined according to the detection frequency to obtain the multi-frequency impedance change data of the first surface, and the multi-frequency impedance change data of the second surface is obtained in the same way.
3. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 2, characterized in that, The multi-frequency impedance change data of the first surface and the second surface are matched or inverted with the pre-obtained equivalent damage depth correspondence, and the depth value corresponding to the corresponding multi-frequency impedance change data is determined as the equivalent damage depth of the corresponding surface, so as to obtain the equivalent damage depth of the first surface and the equivalent damage depth of the second surface.
4. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 3, characterized in that, The total material removal amount on both sides is determined based on the initial thickness and target thickness of the sheet.
5. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 4, characterized in that, The residual damage depth of the first surface is determined based on the equivalent damage depth of the first surface and the first removal amount. The residual damage depth of the second surface is determined based on the equivalent damage depth of the second surface and the second removal amount. Under the condition of satisfying the double-sided material removal constraint, the first removal amount and the second removal amount are determined.
6. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 5, characterized in that, When the total material removal amount on both sides is insufficient to make the residual damage depth of both the first surface and the second surface zero, the first removal amount and the second removal amount are allocated according to the relationship between the equivalent damage depth of the first surface and the equivalent damage depth of the second surface, so that the side with the larger equivalent damage depth corresponds to the larger material removal amount, and the first removal amount and the second removal amount are used as the quantitative polishing control amount for the first surface and the second surface, respectively, to remove material so that the thickness of the sheet after quantitative polishing reaches the target thickness.
7. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 6, characterized in that, The residual damage depth of the first surface and the residual damage depth of the second surface are set after polishing. The residual damage depth of the first surface and the residual damage depth of the second surface are compared, and the Tb-Cu diffusion source surface density of the first surface and the Tb-Cu diffusion source surface density of the second surface are determined in a manner in which the Tb-Cu diffusion source surface density and the residual damage depth are configured in the same direction.
8. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 7, characterized in that, Based on the pre-defined relationship between diffusion depth and time, a first predicted diffusion depth extending from the first surface into the interior of the thin film and a second predicted diffusion depth extending from the second surface into the interior of the thin film are obtained at the candidate diffusion time. The first predicted diffusion depth and the second predicted diffusion depth are superimposed and compared with the target thickness to determine the diffusion time that meets the requirements from the candidate diffusion times.
9. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 8, characterized in that, After quantitative polishing, the first and second surfaces are cleaned; a corresponding amount of Tb-Cu diffusion source is placed on the first surface according to the Tb-Cu diffusion source areal density of the first surface, and a corresponding amount of Tb-Cu diffusion source is placed on the second surface according to the Tb-Cu diffusion source areal density of the second surface, so as to control the amount of Tb-Cu diffusion source on the two surfaces respectively; the double-sided coated NdFeB thin sheet magnet is placed in a vacuum heat treatment environment and vacuum diffusion is performed according to the diffusion time.
10. The method for improving the magnetic properties of NdFeB thin-film magnets according to claim 9, characterized in that, During the vacuum diffusion process, the Tb-Cu diffusion source disposed on the first surface diffuses from the first surface into the interior of the magnet, and the Tb-Cu diffusion source disposed on the second surface diffuses from the second surface into the interior of the magnet. The diffusion duration on both sides is limited by the diffusion time. After the vacuum diffusion is completed, the NdFeB thin sheet magnet is subjected to low-temperature aging treatment, and then cooled after the low-temperature aging treatment is completed to obtain the NdFeB thin sheet magnet.