Zinc anode crystal surface control method, zinc anode and battery

By controlling the zinc anode crystal surface through low-temperature recrystallization and low-temperature annealing, the problem of high cost of controlling the (002) crystal surface in aqueous zinc-ion batteries was solved, achieving efficient and low-cost preferred orientation of the zinc anode crystal surface and improving battery performance.

CN123073006APending Publication Date: 2026-11-10LISHEN (QINGDAO) NEW ENERGY CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611322458.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing aqueous zinc-ion batteries, the (002) crystal plane control method is costly, complex, and time-consuming, making it difficult to achieve large-scale production.

Method used

By employing low-temperature recrystallization and low-temperature annealing methods, the zinc anode is heated to 40°C to 120°C in a reaction furnace, held for 5 min to 240 min, and then cooled to adjust the crystal plane of the zinc anode to achieve preferred orientation of the (002) crystal plane.

Benefits of technology

It achieves the preferred orientation of the (002) crystal plane, increases the ratio of I(002)/I(101) crystal plane by tens or even hundreds of times, has low process cost and short cycle, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073006A_ABST
    Figure CN123073006A_ABST
Patent Text Reader

Abstract

This application provides a method for controlling the crystal surface of a zinc anode, a zinc anode, and a battery. The method for controlling the crystal surface of a zinc anode includes: heating the zinc anode to a preset temperature in a reactor, holding it at that temperature for a preset time, and then cooling and removing it to obtain an electrode with a preferred orientation of the (002) crystal surface. The preset temperature is 40°C to 120°C, and the preset time is 5 min to 240 min. The method for controlling the crystal surface of a zinc anode, the zinc anode, and the battery provided in this application are simple and convenient, can achieve a preferred orientation of the (002) crystal surface of the zinc anode, and have low process costs and short cycle time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of battery technology, and in particular to a method for controlling the crystal surface of a zinc anode, a zinc anode, and a battery. Background Technology

[0002] With the increasing demand for energy, aqueous batteries are attracting more and more attention. Aqueous batteries use water as the electrolyte, offering advantages over organic electrolyte batteries such as lower cost, environmental friendliness, and higher safety. Currently, in aqueous zinc-ion batteries, zinc metal anodes dominated by the (002) crystal plane can effectively improve the performance of zinc-ion batteries. However, methods for controlling the (002) crystal plane are generally costly, complex, and time-consuming. Therefore, a low-cost and efficient method for controlling the crystal plane is urgently needed. Summary of the Invention

[0003] In view of this, the purpose of this application is to propose a method for controlling the crystal surface of a zinc anode, a zinc anode, and a battery to solve the above-mentioned technical problems.

[0004] In a first aspect, this application provides a method for controlling the crystal plane of a zinc anode, comprising: heating the zinc anode to a preset temperature in a reaction furnace, then holding it at the temperature for a preset time and then cooling it to obtain an electrode sheet with a preferred orientation of (002) crystal plane, wherein the preset temperature is 40°C to 120°C and the preset time is 5 min to 240 min.

[0005] Furthermore, the zinc negative electrode comprises rolled zinc foil.

[0006] Furthermore, the zinc negative electrode includes a substrate and a zinc plating layer deposited on the substrate, wherein the substrate includes copper foil or stainless steel foil.

[0007] Furthermore, the thickness of the zinc anode is 40 μm to 70 μm.

[0008] Furthermore, the preset temperature is 60°C to 100°C.

[0009] Furthermore, the preset time is 30 minutes to 120 minutes.

[0010] Furthermore, the thickness of the zinc anode is 50 μm, the preset temperature is 80 °C, and the preset time is 60 min.

[0011] Furthermore, the reactor includes a vacuum furnace or an inert gas atmosphere furnace, the heating rate is 1°C / min to 3°C / min, and the cooling temperature is 20°C to 40°C.

[0012] In a second aspect of this application, a zinc anode is provided, which is obtained using the zinc anode crystal plane control method described in the first aspect above.

[0013] A third aspect of this application provides a battery comprising a zinc negative electrode as described in the second aspect above.

[0014] As can be seen from the above, this application provides a method for controlling the crystal surface of a zinc anode, a zinc anode, and a battery. The method for controlling the crystal surface of a zinc anode includes: heating the zinc anode to a preset temperature in a reactor, then holding it at that temperature for a preset time, and then cooling it to obtain an electrode sheet with a preferred orientation of the (002) crystal surface. The preset temperature is 40°C to 120°C, and the preset time is 5 min to 240 min. By recrystallizing and annealing the zinc anode at low temperature, a preferred orientation of the (002) crystal surface can be achieved. Tests have shown that the I(002) / I(101) crystal surface ratio can be increased by tens or even hundreds of times. Moreover, the annealing time is short, the energy consumption is low, the process cost is low, and the cycle is short. This method for controlling the crystal surface of a zinc anode, the zinc anode, and the battery are simple and convenient, and can achieve a preferred orientation of the (002) crystal surface of the zinc anode. At the same time, the process cost is low and the cycle is short. Attached Figure Description

[0015] To more clearly illustrate the technical solutions in this application or related technologies, the drawings used in the description of the embodiments or related technologies will be briefly introduced below. Obviously, the drawings described below are only embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0016] Figure 1 This is a scanning electron microscope image of the zinc negative electrode sheet in Comparative Example 1 of this application.

[0017] Figure 2 This is a scanning electron microscope image of the zinc negative electrode sheet in Example 2 of this application.

[0018] Figure 3 This is a scanning electron microscope image of the zinc negative electrode sheet in Example 3 of this application.

[0019] Figure 4 This is a scanning electron microscope image of the zinc negative electrode sheet in Example 9 of this application.

[0020] Figure 5 This is a scanning electron microscope image of the zinc negative electrode sheet in Comparative Example 2 of this application.

[0021] Figure 6 This is a scanning electron microscope image of the zinc negative electrode sheet in Example 28 of this application. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with specific embodiments and the accompanying drawings.

[0023] It should be noted that, unless otherwise defined, the technical or scientific terms used in the embodiments of this application should have the ordinary meaning understood by one of ordinary skill in the art to which this application pertains. The terms "first," "second," and similar terms used in the embodiments of this application do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed after the word and their equivalents, without excluding other elements or objects. Terms such as "connected" or "linked" are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. Terms such as "upper," "lower," "left," and "right" are only used to indicate relative positional relationships; when the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0024] Lithium-ion batteries have become the preferred choice for power and energy storage batteries due to their high energy density and long cycle life. However, lithium metal resources are scarce and expensive, and its high reactivity leads to violent reactions in air and water, requiring processing in a dry room for safety. Furthermore, lithium batteries pose safety risks such as fires and explosions in electric vehicles and energy storage stations. Therefore, low-cost, high-safety aqueous batteries are increasingly attracting attention. Aqueous batteries use water as a solvent. Compared to organic electrolyte batteries, aqueous zinc-ion batteries offer advantages such as lower cost, no need for a dry room during manufacturing, environmental friendliness, and higher safety. Therefore, they have broad application prospects in future energy storage, uninterruptible power supplies (UPS), marine applications, and two-wheeled vehicles.

[0025] Currently, zinc powder, rolled zinc foil, and electroplated zinc foil are commonly used as negative electrode materials for aqueous zinc-ion batteries. In the battery, the uniform deposition of zinc ions on the negative electrode surface is closely related to the crystal orientation of the zinc negative electrode surface. The (002) crystal plane has the lowest surface energy, which is beneficial for the wetting of the electrolyte on this crystal plane and subsequent Zn deposition. Furthermore, the (002) crystal plane is parallel to the substrate, while the (100) and (101) crystal planes are perpendicular to the substrate or at a certain angle, thus easily forming dendrites that pierce the separator, leading to battery failure. Meanwhile, H... + The activation energy is highest on the (002) crystal plane, which has the best effect on suppressing hydrogen evolution; OH - The adsorption energy is highest on the (002) crystal plane, i.e., OH - Since it cannot spontaneously adsorb on this crystal plane, it can also suppress alkaline corrosion. Therefore, in order to suppress dendrites, suppress hydrogen evolution, and suppress alkaline corrosion, the core solution is to induce preferential growth of the (002) crystal plane.

[0026] Currently, the preparation process of zinc anodes with preferred (002) crystal plane orientation is complex. Common methods include annealing or cold rolling, which requires annealing the Zn metal anode at high temperatures (300℃~500℃) or repeated rolling combined with annealing. This process is energy-intensive and cumbersome. The high-temperature annealing temperature of the melt recrystallization method is typically 600℃~650℃, with a time of 6min~10min. This process, with its high annealing temperature and short time, is unsuitable for processing large quantities of zinc anodes. For example, within 6min~10min of forming the anode roll, the Zn temperature in the inner layer of the anode roll has not yet risen above the Zn melting point, making recrystallization impossible. Extending the annealing time may cause the Zn in the outer layer of the anode roll to melt, thus this process cannot be scaled up for mass production. For the epitaxial growth electrodeposition method, graphene parallel to the substrate surface is first prepared on the current collector, and then the electrodeposited Zn grows epitaxially along the graphene. Because graphene has different surface orientations, this process requires a special shear flow to induce the graphene sheets to be parallel to the Cu foil substrate. This step makes it difficult to ensure that all graphene sheets are parallel to the Cu foil substrate, which makes it difficult to scale up production.

[0027] Compared to the aforementioned technical routes, non-epitaxial electrodeposition does not require a specific orientation substrate, making the method more practical. Some technologies use a "sheet-to-sheet" preparation method, using a specific aqueous electroplating solution such as Zn(CF3SO3)2, adding additives to the electroplating solution or increasing the electroplating current density to prepare Zn anodes with high (002) orientation. This preparation method uses sheet-like Zn as a sacrificial anode, depositing Zn on a corresponding sheet-like substrate using constant current electroplating. However, in the mass production of Zn anodes, the production speed of "sheet-to-sheet" cannot meet the demand. When switching to "roll-to-roll" continuous electroplating, the electrodeposition substrate is directly used, such as rolled copper foil, and the copper foil is continuously rolled during electrodeposition, with Zn... 2+ Continuous electroplating on copper foil surfaces is hundreds of times more efficient than sheet-to-sheet electrodeposition. Research on continuous electroplating revealed that under the sheet-to-sheet electroplating process, the electric field distribution and Zn... 2+ Concentration polarization and other processes are relatively simple, making it easy to generate (002) crystal planes. However, when switching to continuous roll-to-roll electroplating, the cathode copper foil continuously travels, and to increase the electrodeposition rate, the current density reaches 6 A / dm. 2 Even 30A / dm 2 This exceeds the range of high-current electroplating. For example, some technologies specify a high-current electroplating range of 0.5 A / dm². 2 ~20A / dm 2 Pulse electroplating is required, and the methods of stirring the electroplating solution vary considerably. Applying the "sheet-to-sheet" constant current electroplating process directly to continuous "roll-to-roll" electroplating yielded completely different results, with a significant reduction in the proportion of the (002) crystal plane of Zn. This is because the electric field distribution and Zn... 2+Concentration polarization and other factors are quite complex, and studies have found that it is difficult to adjust the electroplating solution, additives, or current to control the (002) crystal plane of Zn. Furthermore, the Zn anode crystal plane obtained by continuous electroplating is unstable, making it difficult to obtain a stable (002) crystal plane through electrodeposition processes.

[0028] Based on the above problems, this application provides a simple annealing method that adjusts the preferred orientations of Zn anodes, such as (101) and (103) crystal planes, to a preferred orientation of (002) crystal plane through low-temperature annealing. This process has low annealing temperature, short time, low energy consumption, and is simple and easy to scale up for mass production, providing important technical support for promoting the mass production of water-zinc zinc-ion batteries.

[0029] The following describes specific embodiments in conjunction with... Figures 1 to 6 The technical solution of this application will be described in detail below.

[0030] In some embodiments of this application, a method for controlling the crystal plane of a zinc anode is provided, comprising: heating the zinc anode to a preset temperature in a reaction furnace, then holding it at the temperature for a preset time and then cooling it to obtain an electrode sheet with a preferred orientation of (002) crystal plane, wherein the preset temperature is 40°C to 120°C and the preset time is 5 min to 240 min.

[0031] The preset temperature ranges from 40℃ to 120℃, such as 40℃, 50℃, 60℃, 70℃, 80℃, 90℃, 100℃, 110℃, or 120℃, etc., without any specific limitation. The preset time ranges from 5 minutes to 240 minutes, such as 5 minutes, 10 minutes, 20 minutes, 30 minutes, 60 minutes, 90 minutes, 120 minutes, or 240 minutes, etc., without any specific limitation.

[0032] The zinc anode can be an electroplated zinc anode including a substrate, such as copper foil or stainless steel foil. The zinc anode can also be a rolled zinc anode without a substrate. The zinc anode is placed in a reaction furnace and heated to a preset temperature. After holding at that temperature for a preset time, it is cooled and removed. The recrystallization temperature of Zn is 36°C. Because the (002) crystal plane is a close-packed plane with low surface energy, recrystallization and grain growth occur after low-temperature annealing, resulting in a preferred orientation of the (002) crystal plane. For example, for zinc anodes prepared by electrodeposition, since deposition is often performed at overpotential, there is high internal stress and high surface energy within the grains. Annealing at a temperature higher than the recrystallization temperature will cause recrystallization.

[0033] By recrystallizing and annealing the zinc anode at low temperature, the preferred orientation of the (002) crystal plane can be achieved. According to the test, the ratio of I(002) / I(101) crystal plane of the electrode obtained by this crystal plane control method can be increased by tens or even hundreds of times. Moreover, the annealing time is short, the energy consumption is low, the process cost is low, and the cycle is short.

[0034] This method for controlling the crystal plane of zinc anode is simple and convenient, and can achieve the preferred orientation of the (002) crystal plane of zinc anode. At the same time, the process cost is low and the cycle is short.

[0035] In some embodiments, the zinc anode comprises rolled zinc foil; or, the zinc anode comprises a substrate and a zinc plating layer deposited on the substrate, the substrate comprising copper foil or stainless steel foil.

[0036] Tests showed that the (002) crystal orientation of the copper foil zinc-plated negative electrode and the stainless steel foil zinc-plated negative electrode was significantly higher than that of the rolled zinc foil.

[0037] In some embodiments, the thickness of the zinc anode is 40 μm to 70 μm, the preset temperature is 60°C to 100°C, and the preset time is 30 min to 120 min.

[0038] The thickness of the zinc anode is 40μm to 70μm, for example, 40μm, 50μm, 60μm, or 70μm, etc., without specific limitation. The preset temperature is 60℃ to 100℃, for example, 60℃, 70℃, 80℃, 90℃, or 100℃, etc., without specific limitation. The preset time is 30 min to 120 min, for example, 30 min, 60 min, 90 min, or 120 min, etc., without specific limitation. Testing has shown that this parameter setting can further improve the I(002) / I(101) crystal plane ratio.

[0039] In some embodiments, the thickness of the zinc anode is 50 μm, the preset temperature is 80 °C, and the preset time is 60 min. Testing has shown that the optimal I(002) / I(101) crystal plane ratio can be obtained.

[0040] In some embodiments, the reactor includes a vacuum furnace or an inert gas atmosphere furnace, the heating rate is 1°C / min to 3°C / min, and the cooling temperature is 20°C to 40°C.

[0041] The inert gas may be, for example, nitrogen or a rare gas. The heating rate may be, for example, 1°C / min, 2°C / min, or 3°C / min, etc., without specific limitation. The cooling temperature may be, for example, 20°C, 25°C, 30°C, or 40°C, etc., without specific limitation.

[0042] In some embodiments of this application, a zinc anode is provided, which is obtained using the zinc anode crystal plane control method described in any of the above embodiments.

[0043] The zinc negative electrode facilitates the wetting of the electrolyte on the (002) crystal surface and subsequent zinc deposition, and can suppress dendrite formation, hydrogen evolution, and alkaline corrosion.

[0044] In some embodiments of this application, a battery is provided, including a zinc negative electrode as described in any of the above embodiments.

[0045] Aqueous zinc batteries consist of a positive electrode, a negative electrode, an electrolyte, and a separator. Positive electrode materials include, for example, manganese-based oxides, vanadium-based oxides, Prussian blue analogs (PBAs), or organic materials. The electrolyte typically uses water as the solvent, with the solute being a soluble salt containing zinc ions, such as ZnSO4, Zn(CF3SO3)2, or Zn(NO3)2. Separator materials include, for example, glass fiber, polymer separators, and composite separators. This type of battery is low in cost, has good stability, high safety, and a long cycle life.

[0046] Comparative Example 1

[0047] A 260mm wide, 10μm thick copper foil was used as the substrate for electroplating. The electroplating solution was a 1.5mol / L zinc sulfate solution, and the electroplating process was continuous. The current for both cathode rollers was 160A, and the electroplating speed was 2m / min. After electroplating, the zinc plating layer thickness on both sides of the copper foil was 20μm, resulting in a total zinc anode thickness of 50μm.

[0048] Comparative Example 2 Obtain rolled zinc foil with a thickness of 50 μm.

[0049] Example 1 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 50°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0050] Example 2 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 60°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0051] Example 3 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0052] Example 4 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 100°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0053] Example 5 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 120°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0054] Example 6 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 5 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0055] Example 7 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 10 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0056] Example 8 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 30 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0057] Example 9 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0058] Example 10 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 120 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0059] Example 11 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 40°C at a rate of 2°C / min. After holding at this temperature for 30 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0060] Example 12 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 40°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0061] Example 13 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 40°C at a rate of 2°C / min. After holding at this temperature for 120 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0062] Example 14 The zinc-plated copper foil anode from Comparative Example 1 was obtained and its crystal surface was controlled. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 40°C at a rate of 2°C / min. After holding at this temperature for 240 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0063] Example 15 Electroplating was performed on a 260 mm wide and 10 μm thick stainless steel foil using a 1.5 mol / L zinc sulfate electroplating solution. The electroplating process was continuous, with both cathode rollers operating at a current of 160 A and a plating speed of 2 m / min. After electroplating, the zinc plating thickness on both sides of the stainless steel foil was 20 μm, resulting in a total zinc plating thickness of 50 μm for the stainless steel foil negative electrode.

[0064] Crystalline surface conditioning was performed on the zinc-plated stainless steel foil anode. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 10 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0065] Example 16 Crystalline surface conditioning was performed on the zinc-plated stainless steel foil anode in Example 15. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 30 min, it was cooled to room temperature and then the vacuum oven was opened to obtain the electrode sheet.

[0066] Example 17 Crystalline surface conditioning was performed on the zinc-plated stainless steel foil anode in Example 15. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and then the vacuum oven was opened to obtain the electrode sheet.

[0067] Example 18 Crystalline surface conditioning was performed on the zinc-plated stainless steel foil anode in Example 15. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 120 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0068] Example 19 A 260 mm wide and 10 μm thick copper foil was electroplated using a 1.5 mol / L zinc sulfate solution. The electroplating process was continuous, with both cathode rollers operating at a current of 160 A and a plating speed of 1 m / min. After electroplating, the zinc plating layer thickness on both sides of the copper foil was 30 μm, resulting in a total zinc plating thickness of 70 μm for the copper foil negative electrode.

[0069] Crystalline surface conditioning was performed on the zinc foil-plated anode. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 30 min, it was cooled to room temperature. The vacuum oven was then opened to obtain the electrode sheet.

[0070] Example 20 Crystalline surface conditioning was performed on the zinc foil-plated anode in Example 19. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0071] Example 21 Crystalline surface conditioning was performed on the zinc foil-plated anode in Example 19. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 90 min, it was cooled to room temperature and then the vacuum oven was opened to obtain the electrode sheet.

[0072] Example 22 Crystalline surface conditioning was performed on the zinc foil-plated anode in Example 19. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 120 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0073] Example 23 A 260 mm wide and 10 μm thick copper foil was electroplated using a 1.5 mol / L zinc sulfate solution. The electroplating process was continuous, with both cathode rollers operating at a current of 160 A and a plating speed of 2.5 m / min. After electroplating, the zinc plating layer thickness on both sides of the copper foil was 15 μm, resulting in a total zinc-plated negative electrode thickness of 40 μm.

[0074] Crystalline surface conditioning was performed on the zinc foil-plated anode. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature. The vacuum oven was then opened to obtain the electrode sheet.

[0075] Example 24 Crystalline surface conditioning was performed on the zinc-plated copper foil anode in Example 23. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 30 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0076] Example 25 Crystalline surface conditioning was performed on the zinc foil-plated anode in Example 23. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and then the vacuum oven was opened to obtain the electrode sheet.

[0077] Example 26 Crystalline surface conditioning was performed on the zinc-plated copper foil anode in Example 23. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 90 min, it was cooled to room temperature and then the vacuum oven was opened to obtain the electrode sheet.

[0078] Example 27 The rolled zinc foil zinc anode from Comparative Example 2 was obtained and its crystal surface was regulated. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 20 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0079] Example 28 The rolled zinc foil zinc anode from Comparative Example 2 was obtained and its crystal surface was regulated. The zinc anode was placed in a vacuum oven, evacuated to -14 psi, and then heated to 80°C at a rate of 2°C / min. After holding at this temperature for 60 min, it was cooled to room temperature and the vacuum oven was opened to obtain the electrode sheet.

[0080] Crystal plane tests were performed on the zinc negative electrode sheets of Examples 1 to 28, and Comparative Examples 1 and 2. The test results are shown in Table 1. In Table 1, I(002) represents the maximum intensity value of the XRD diffraction peak corresponding to the (002) crystal plane, I(101) represents the maximum intensity value of the XRD diffraction peak corresponding to the (101) crystal plane, and I(002) / I(101) represents the relative proportion of the (002) crystal plane, i.e. the degree of preferred orientation.

[0081] Table 1 Comparison of crystal planes of zinc anode

[0082] The preferred orientation of Zn crystal planes obtained by continuous electroplating is usually not the (002) crystal plane. In Comparative Example 1, direct electroplating yielded a zinc-plated copper foil anode with an I(002) / I(101) ratio of only 0.1, and its morphology is as follows. Figure 1 As shown, the grains are plate-like with disordered crystal orientations and non-parallel crystal planes to the matrix. Therefore, these crystal planes are highly susceptible to dendrite growth during battery cycling, leading to battery failure. For rolled zinc foil, such as Comparative Example 2, its morphology is as follows... Figure 5 As shown, the proportion of the (002) crystal plane is also relatively low, only 1.0.

[0083] In Example 1, the zinc anode from Comparative Example 1 was kept at 40°C for 20 min and then cooled, resulting in a significant increase in the I(002) / I(101) ratio. In Example 2, the zinc anode from Comparative Example 1 was kept at 60°C for 20 min and then cooled, yielding an electrode morphology as shown below. Figure 2 As shown, the coating surface is smoother, and the grains exhibit a certain degree of preferred orientation, with I(002) / I(101) increasing to 3.3. In Example 3, the zinc anode from Comparative Example 1 was kept at 80°C for 20 min and then cooled, resulting in an electrode morphology as shown. Figure 3 As shown, the coating surface is significantly smoother, and the grains exhibit a hexagonal spiral growth morphology, with I(002) / I(101) increasing to 8.1. Further increasing the temperature in Examples 4 and 5 had little effect on the (002) crystal plane. Comparing Examples 1 to 5, it can be seen that a heat preservation temperature of 80℃ provides the best effect.

[0084] Examples 6 to 10, based on an insulation temperature of 80℃, adjusted the insulation time and found that when the insulation time reached 30 minutes or more, the I(002) / I(101) ratio significantly improved. In Example 9, the insulation temperature was 80℃ and the insulation time was 60 minutes, resulting in an electrode morphology as shown below. Figure 4 As shown, the coating surface is significantly smoother, and the grains exhibit a distinct equilateral hexagonal morphology. This is because the (002) crystal plane of Zn is an equilateral hexagon parallel to the bottom surface. As can be seen from the figure, the orientation of the Zn crystal plane is significantly parallel to the Cu foil substrate. This is also the reason for the preferred orientation of the (002) crystal plane. This crystal plane can be parallel to the separator, making it less likely for dendrites to pierce the separator, thus ensuring a longer battery cycle life. Under the conditions of Example 9, I(002) / I(101) reached 98.6, with the (002) crystal plane accounting for the largest proportion, and the energy consumption was low, resulting in a fast production speed. Further increasing the heat preservation time on this basis did not have a significant effect on improving the proportion of the (002) crystal plane.

[0085] In Examples 11 to 14, the holding time was adjusted based on a holding temperature of 40°C. It was found that even with a holding time of 240 min, the I(002) / I(101) ratio could only be increased to 13.2. However, in Example 9, a holding temperature of 80°C and a holding time of 60 min resulted in a significant increase in I(002) / I(101), indicating that the holding temperature and holding time had a synergistic effect on the preferred orientation of the (002) crystal plane.

[0086] Examples 15 to 18 compared the crystal plane changes of zinc-plated stainless steel foil anodes with adjustments to the holding time based on a holding temperature of 80°C. It was found that the highest proportion of (002) crystal planes could still be achieved when the holding temperature was 80°C and the holding time was 60 min.

[0087] Examples 19 to 26 compared the effects of zinc anodes with different zinc plating thicknesses on the preferred orientation of the (002) crystal plane. They found that different zinc anode thicknesses required different heat treatment processes to achieve the highest (002) crystal plane ratio. Therefore, by adjusting process parameters, anodes with the highest (002) crystal plane ratio corresponding to different Zn anode thicknesses can be obtained. This also indicates that the adjustment method of this application can be applied to different Zn anodes. A holding time of 60 min or more can increase the (002) crystal plane ratio, with the best effect observed when the zinc anode thickness is 50 μm.

[0088] In Example 27, the rolled zinc foil from Comparative Example 2 was held at 80°C for 20 min and then cooled, resulting in a significant increase in the I(002) / I(101) ratio. In Example 28, the holding time was further increased to 60 min, and the resulting electrode morphology was as follows... Figure 6As shown, the proportion of (002) crystal planes will also increase, but it is not as effective as that of electroplated zinc anode. This is because the preparation process of electroplated zinc anode uses a very high current, so the internal stress between the Zn grains generated by electroplating is higher, and the stress relief and the preferred orientation of the crystal plane can be adjusted at a lower temperature.

[0089] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of this application is limited to these examples; under the concept of this application, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of different aspects of the embodiments of this application as described above, which are not provided in detail for the sake of brevity.

[0090] Furthermore, given that details have been set forth to describe exemplary embodiments of this application, it will be apparent to those skilled in the art that embodiments of this application may be practiced without these details or with variations thereof. Therefore, these descriptions should be considered illustrative rather than restrictive.

[0091] To simplify the description and discussion, and to avoid obscuring the embodiments of this application, well-known power / ground connections to other components may or may not be shown in the provided drawings. Furthermore, the apparatus may be shown in block diagram form to avoid obscuring the embodiments of this application, and this also takes into account the fact that the details of implementation of these block diagram apparatuses are highly dependent on the platform on which the embodiments of this application will be implemented (i.e., these details should be fully understood by those skilled in the art). While specific details have been set forth to describe exemplary embodiments of this application, it will be apparent to those skilled in the art that the embodiments of this application may be implemented without these specific details or with variations thereof. Therefore, these descriptions should be considered illustrative rather than restrictive.

[0092] Although this application has been described in conjunction with specific embodiments thereof, many substitutions, modifications, and variations of these embodiments will be apparent to those skilled in the art based on the foregoing description. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of this application should be included within the scope of protection of this application.

Claims

1. A method for controlling the crystal plane of a zinc anode, characterized in that, include: The zinc anode is heated to a preset temperature in a reaction furnace, then held at the temperature for a preset time and cooled to obtain an electrode sheet with preferred orientation of (002) crystal plane, wherein the preset temperature is 40°C to 120°C and the preset time is 5 min to 240 min.

2. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The zinc negative electrode comprises rolled zinc foil.

3. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The zinc negative electrode includes a substrate and a zinc plating layer deposited on the substrate, wherein the substrate includes copper foil or stainless steel foil.

4. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The thickness of the zinc anode is 40 μm to 70 μm.

5. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The preset temperature is 60°C to 100°C.

6. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The preset time is 30 minutes to 120 minutes.

7. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The zinc anode has a thickness of 50 μm, the preset temperature is 80 °C, and the preset time is 60 min.

8. The method for controlling the crystal surface of the zinc anode according to claim 1, characterized in that, The reactor includes a vacuum furnace or an inert gas atmosphere furnace, the heating rate is 1°C / min to 3°C / min, and the cooling temperature is 20°C to 40°C.

9. A zinc negative electrode, characterized in that, Obtained using the zinc anode crystal plane control method as described in any one of claims 1-8.

10. A battery, characterized in that, Including the zinc anode as described in claim 9.