Cathode material and lithium ion battery

By controlling the atomic occupancy of transition metal sites and the proportion of doped elements in the matrix, combined with a carbon coating layer, the problem of Mn dissolution in lithium manganese iron phosphate cathode materials was solved, thereby improving the voltage stability and cycle performance of the battery.

CN123073036APending Publication Date: 2026-11-10SHENZHEN CITY BATTERY NANOMETER TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510603522.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing technologies, Mn is easily dissolved in lithium manganese iron phosphate cathode materials during long-term use, leading to voltage decay, and the improvement effect of commonly used ion doping is not significant.

Method used

By controlling the atomic occupancy of transition metal sites and the proportion of doping elements in the matrix, more defect vacancies are formed, and a carbon layer is coated on the matrix surface to synergistically suppress Mn dissolution.

Benefits of technology

It effectively improves the voltage decay of lithium manganese iron phosphate and enhances the cycle stability and capacity of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073036A_ABST
    Figure CN123073036A_ABST
Patent Text Reader

Abstract

This invention provides a cathode material and a lithium-ion battery. The cathode material includes a matrix and a carbon coating layer located on at least a portion of the surface of the matrix, wherein the matrix has the general chemical formula LiMn. a Fe b N m PO4 and N include at least one of Ti or Mg; 0.586≤a≤0.6, 0.391≤b≤0.4, 0.005≤m≤0.023, a+b+m=1; the atomic occupancy of the transition metal satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, 0.0022≤Occ(N)<m. This application controls the atomic occupancy of the transition metal sites in the matrix, causing the dopant element N to be doped in the transition metal, as well as in the interstitial sites and Li sites, thereby forming more defect vacancies internally. This effectively improves the Jan Taylor effect of Mn, reduces the lattice strain caused by the Jan Taylor effect, and inhibits Mn dissolution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of cathode material technology, and more specifically, to a cathode material and a lithium-ion battery. Background Technology

[0002] Lithium manganese iron phosphate (LMFP) is widely used as a cathode material in lithium-ion batteries due to its high theoretical capacity, excellent cycle performance, low cost, and environmental friendliness. However, during long-term use, LMFP suffers from the problem of manganese (Mn) easily dissolving, leading to voltage decay. Currently, the commonly used method to suppress Mn dissolution and improve the voltage decay of LMFP is ion doping. However, ion doping alters the crystal lattice to a negligible degree, and the formation of point defects in the lattice has little effect on improving the Jan Taylor effect of Mn, resulting in poor suppression of Mn dissolution.

[0003] In view of this, the present invention is hereby proposed. Summary of the Invention

[0004] The main objective of this invention is to provide a cathode material and a lithium-ion battery to solve the technical problem that the existing technology uses ion doping to change the crystal lattice by a small amount, and the point defects formed in the crystal lattice have little effect on improving the Jan Taylor effect of Mn and the effect on inhibiting Mn dissolution is not good.

[0005] To achieve the above objectives, according to one aspect of the present invention, a cathode material is provided, comprising a matrix and a carbon coating layer located on at least a portion of the surface of the matrix, wherein the matrix has the general chemical formula LiMn. a Fe b N m PO4, N includes at least one of Ti or Mg; 0.586≤a≤0.6, 0.391≤b≤0.4, 0.005≤m≤0.023, a+b+m=1; the atomic occupancy of the transition metals satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, 0.0022≤Occ(N)<m.

[0006] Furthermore, N is Ti, 0.005≤m≤0.023.

[0007] Furthermore, N is Mg, and 0.005 ≤ m ≤ 0.023.

[0008] Furthermore, N is Ti and Mg, and the general chemical formula of the matrix is ​​LiMn. a Fe b Ti c Mg dFor PO4, 0.005≤c≤0.009 and 0.005≤d≤0.014; and the atomic occupancy of the transition metal sites satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg)≤0.9955, Occ(Ti)<c, Occ(Mg)<d.

[0009] Furthermore, the cathode material was characterized by Raman spectroscopy, and the cathode material satisfies: 5.70 ≤ I(G) / I(PO4) 3- )≤5.90; where I(G) is the Raman spectrum of the cathode material measured at 1585 cm⁻¹. -1 C=C bond vibration peak intensity at the location; I(PO4) 3- The 950 cm⁻¹ Raman spectrum of the positive electrode material was measured. -1 PO4 at the location 3- Peak intensity of stretching vibration.

[0010] Furthermore, the carbon mass content is C%, where 1.58 ≤ C ≤ 1.64, and 0.27 ≤ C / [I(G) / I(PO4)] 3- )]≤0.29.

[0011] Furthermore, the median particle size D50 of the cathode material's volume distribution is 6μm-12μm.

[0012] Furthermore, the specific surface area of ​​the cathode material is 8m². 2 / g-16m 2 / g.

[0013] Furthermore, the pH of the positive electrode material is 8-11.

[0014] Furthermore, the tap density of the cathode material is 1.3 g / cm³. 3 -1.9g / cm 3 .

[0015] Furthermore, the resistivity of the cathode material powder is 100-300 S·cm.

[0016] According to another aspect of the present invention, a lithium-ion battery is provided, the lithium-ion battery comprising the positive electrode material provided in the first aspect above.

[0017] By applying the technical solution of this application, in the cathode material provided in this application, by controlling the atomic occupancy of the transition metal sites in the matrix to satisfy: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, the doping element N can not only be doped in the transition metal sites, but also in the interstitial sites and Li sites, resulting in the generation of vacancies. At the same time, by controlling 0.0022≤Occ(N)<m and 0.005≤m≤0.023, more defect vacancies are formed inside the cathode material. More defect vacancies can effectively improve the Ginger Taylor effect of Mn, reduce the lattice strain caused by the Ginger Taylor effect, thereby suppressing Mn dissolution and improving the voltage decay of lithium manganese iron phosphate.

[0018] In addition, the cathode material provided in this application has a carbon coating layer on the surface of the substrate, which can prevent the electrolyte from directly contacting the substrate. Through the synergistic effect of carbon coating and element doping, Mn dissolution is further suppressed, and the voltage decay of lithium manganese iron phosphate is improved. Attached Figure Description

[0019] The accompanying drawings, which form part of this application, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings:

[0020] Figure 1 This is a schematic diagram of the structure of a secondary battery during charging, provided in some embodiments of this application;

[0021] Figure 2 This is a schematic diagram of the structure of a secondary battery during discharge, provided in some embodiments of this application;

[0022] 100. Electrode assembly; 101. Positive electrode; 102. Negative electrode; 103. Separator.

[0023] Figure 3 A cross-sectional SEM image of the cathode material provided in Example 2 is shown;

[0024] Figure 4 The cross-sectional EDS image of the cathode material provided in Example 2 is shown;

[0025] Figure 5 Raman spectra of the cathode materials provided in Example 2 and Comparative Examples 1-2 are shown.

[0026] Figure 6 This is the charge-discharge curve diagram for the 1st, 30th, and 50th cycles of Example 2. Detailed Implementation

[0027] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0028] As analyzed in the background section of this application, ion doping is currently a commonly used method to suppress Mn dissolution and improve the voltage decay of lithium manganese iron phosphate. However, since ion doping alters the crystal lattice only slightly, the point defects formed in the lattice do not significantly improve the Jan Taylor effect of Mn, resulting in poor suppression of Mn dissolution. To suppress Mn dissolution and improve the voltage decay of lithium manganese iron phosphate, this application provides a cathode material and a lithium-ion battery.

[0029] In a first typical embodiment of this application, a cathode material is provided, comprising a substrate and a carbon coating layer located on at least a portion of the surface of the substrate, wherein the substrate has the general chemical formula LiMn. a Fe b N m PO4, N includes at least one of Ti or Mg, 0.586≤a≤0.6, 0.391≤b≤0.4, 0.005≤m≤0.023, a+b+m=1; the atomic occupancy of the transition metal sites satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, 0.0022≤Occ(N)<m.

[0030] In this application, the atomic occupancy of transition metal sites is obtained by characterizing the cathode material using X-ray diffraction (XRD), followed by Reitveld refinement of the XRD data using GSAS. Reitveld refinement of XRD refers to the process of refining the raw slow-scan XRD data of the LMFP obtained by crystal X-ray diffraction. The data obtained from the slow-scan XRD is then refined using the specialized Reitveld refinement software GSAG. During the refinement process, parameters such as zero-point drift, scaling factor, background, cell parameters, peak shape parameters, atomic occupancy, atomic coordinates, temperature factor, and preferred orientation are corrected sequentially. During the refinement process, when chi 2 When Rwp < 3 and Rwp < 0.05, fine-tuning can be completed.

[0031] In this application, Occ(Mn) refers to the atomic occupancy of Mn, Occ(Fe) refers to the atomic occupancy of Fe, and Occ(N) refers to the atomic occupancy of N.

[0032] In the cathode material provided in this application, by controlling the atomic occupancy of the transition metal sites in the matrix to satisfy: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, the doping element N can not only be doped in the transition metal sites, but also in the interstitial sites and Li sites, resulting in the generation of vacancies. At the same time, by controlling 0.0022≤Occ(N)<m and 0.005≤m≤0.023, more defect vacancies are formed inside the cathode material. More defect vacancies can effectively improve the Ginger Taylor effect of Mn, reduce the lattice strain caused by the Ginger Taylor effect, thereby suppressing Mn dissolution and improving the voltage decay of lithium manganese iron phosphate.

[0033] In addition, the cathode material provided in this application has a carbon coating layer on the surface of the substrate, which can prevent the electrolyte from directly contacting the substrate. Through the synergistic effect of carbon coating and element doping, Mn dissolution is further suppressed, and the voltage decay of lithium manganese iron phosphate is improved.

[0034] Typically, but not limitingly, the atomic occupancy of the transition metal in the cathode material matrix provided in this application, Occ(Mn)+Occ(Fe)+Occ(N), is 0.9797, 0.9831, 0.9834, 0.9839, 0.9850, 0.9887, 0.9934, 0.9942, 0.9952, 0.9955, or any range of two such values; m is 0.005, 0.009, 0.014, 0.015, 0.019, 0.023, or any range of two such values.

[0035] In some embodiments, the doping element N is Ti, 0.005≤m≤0.023. Ti is not only doped in transition metal sites, but also in interstitial sites and Li sites, thereby forming more vacancy defects inside the cathode material, effectively improving the Ginger Taylor effect of Mn, reducing the lattice strain caused by the Ginger Taylor effect, suppressing Mn dissolution, and improving the voltage decay of lithium manganese iron phosphate.

[0036] In some embodiments, the doping element N is Mg, 0.005≤m≤0.023. Mg is not only doped in transition metal sites, but also in interstitial sites and Li sites, which results in more vacancy defects inside the cathode material, effectively improving the Ginger Taylor effect of Mn, reducing the lattice strain caused by the Ginger Taylor effect, inhibiting Mn dissolution, and improving the voltage decay of lithium manganese iron phosphate.

[0037] In some embodiments, N is Ti and Mg, and the general chemical formula of the matrix is ​​LiMn. a Fe b Ti c Mg dFor PO4, 0.005≤c≤0.009, 0.010≤d≤0.014, and the atomic occupancy of the transition metal sites satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg)≤0.9955, Occ(Ti)<c, Occ(Mg)<d. By simultaneously doping with Ti and Mg, more vacancy defects are formed inside the cathode material, which can more effectively improve the Jamette effect of Mn, further reduce the lattice strain caused by the Jamette effect, further suppress Mn dissolution, and thus further reduce the voltage decay of lithium manganese iron phosphate.

[0038] The cathode material provided in this application has a carbon coating layer on the surface of the substrate. The more complete and uniform the carbon coating layer is on the substrate surface, the more effectively it can prevent direct contact between the electrolyte and the substrate, thereby inhibiting Mn dissolution. The applicant found that, when the cathode material is characterized by Raman spectroscopy, when the cathode material satisfies 5.70 ≤ I(G) / I(PO4) 3- When the carbon coating layer on the substrate surface is ≤5.90, it has excellent integrity and uniformity, which can further suppress the dissolution of Mn and reduce the voltage decay of lithium manganese iron phosphate.

[0039] It should be noted that the I(G) mentioned above refers to the 1585 cm⁻¹ value in the Raman spectrum measured for the cathode material. -1 C=C bond vibration peak intensity at the location; I(PO4) 3- This refers to the 950 cm⁻¹ region in the Raman spectrum measured for the cathode material. -1 PO4 at the location 3- Peak intensity of stretching vibration.

[0040] A higher I(G) indicates a higher carbon content in the cathode material and a thicker coating layer. I(PO4) 3- The larger the value of I(G) / I(PO4), the more exposed lithium manganese iron phosphate is on the surface of the cathode material. 5.70 ≤ I(G) / I(PO4) 3- A value of ≤5.90 indicates that the carbon coating layer on the surface of the cathode material has good integrity and the coating layer thickness is moderate.

[0041] Generally, the thickness of the carbon coating layer has a certain impact on the electrochemical performance and Mn dissolution of the cathode material. When the carbon coating layer is too thick, it will lead to a decrease in tap density and an increase in specific surface area, which is not conducive to the practical application of the material and may even affect Li + The migration of Mn reduces the capacity and rate performance of the material, while an excessively thin carbon coating layer has a poor effect on inhibiting Mn dissolution, resulting in excessively rapid voltage decay and reduced cycle performance of the cathode material.

[0042] In some embodiments, the carbon mass content in the cathode material is C%, where the cathode material satisfies 1.58 ≤ C ≤ 1.64 and 0.27 ≤ C / [I(G) / I(PO4)]. 3- When the carbon coating thickness is ≤0.29, the thickness of the carbon coating layer on the surface of the cathode material is more moderate, with better uniformity and integrity, without affecting the Li + It diffuses and effectively inhibits Mn dissolution. When C > 1.64, C / [I(G) / I(PO4)] 3- When the carbon coating is too thick, the tap density decreases and the specific surface area increases, which is detrimental to the practical application of the material. Conversely, a thinner coating will negatively impact the material's electrochemical performance, Mn dissolution, and cycling performance.

[0043] In some embodiments, the cathode material is spherical with a median particle size D50 of 6 μm-12 μm, which improves the material's fluidity without significantly inhibiting its electrochemical performance. Specifically, the D50 of the cathode material can be 6 μm, 8 μm, 10 μm, 12 μm, or any range of two values.

[0044] In some embodiments, the specific surface area of ​​the cathode material is 8m². 2 / g–16m 2 / g, reducing the occurrence of jelly-like and agglomerated phenomena during pulping and processing, and promoting effective contact between the material and the conductive agent, thereby improving the electrochemical performance of the material. Specifically, the specific surface area of ​​the cathode material can be 8m². 2 / g, 10m 2 / g、12m 2 / g、14m 2 / g, 16m 2 / g or a range of values ​​consisting of any two numbers.

[0045] In some embodiments, the pH of the cathode material is 8-11, which ensures both the processing performance and the electrochemical performance of the material. Specifically, the pH of the cathode material can be 8, 9, 10, 11, or any range of two values.

[0046] In some embodiments, the tap density of the positive electrode material is 1.3 g / cm³. 3 -1.9g / cm 3 This significantly improves the material's flowability and processing performance, allowing for direct application in dry-process electrodes. Specifically, the tap density of the cathode material can reach 1.3 g / cm³. 3 1.5g / cm 3 1.7g / cm 3 1.9g / cm 3 Or a range of values ​​consisting of any two numerical values.

[0047] In some embodiments, the resistivity of the positive electrode material powder is 100 S·cm-300 S·cm, ensuring the mutual conduction of electrons between the active particles and the conductive agent. Specifically, the resistivity of the positive electrode material powder can be 100 S·cm, 200 S·cm, 300 S·cm, or any range of two values.

[0048] In some embodiments, the matrix in the cathode material is selected from LiMn. 0.591 Fe 0.394 Ti 0.005 Mg 0.010 PO4, LiMn 0.58 9Fe 0.392 Ti 0.009 Mg 0.010 PO4, LiMn 0.586 Fe 0.391 Ti 0.009 Mg 0.014 PO4, LiMn 0.589 Fe 0.392 Ti 0.009 Mg 0.010 PO4, LiMn 0.589 Fe 0.392 Ti 0.009 Mg 0.010 One of the PO4 groups.

[0049] In another typical embodiment of this application, a method for preparing the above-mentioned cathode material is also provided. The method includes the following steps: Step S1, mixing and grinding a lithium source, a phosphorus source, a soluble iron source, a manganese source, a titanium source and / or a magnesium source, an organic carbon source, and water to obtain a mixed slurry; Step S2, spray drying the mixed slurry to obtain a lithium manganese iron phosphate precursor; Step S3, calcining the lithium manganese iron phosphate precursor to obtain the cathode material.

[0050] This application uses lithium source, phosphorus source, soluble iron source, manganese source, titanium source and / or magnesium source, and organic carbon source dispersed in water and then ground. Various ions can be mixed at the ion level, so that doped ions titanium and magnesium can effectively enter the crystal lattice, thereby introducing lattice vacancies, rather than simply being enriched on the material surface. Organic carbon source can also be mixed at the molecular level, thereby forming molecular-level in-situ carbon coating, so that a uniform and complete carbon coating layer is formed on the surface of the cathode material, effectively suppressing Mn dissolution.

[0051] In some embodiments, the specific type of lithium source in step S1 above is not limited; any commonly used lithium source in the art can be used, including but not limited to any one or at least two of lithium carbonate, lithium hydroxide, and lithium phosphate. The specific type of phosphorus source is also not limited, with PO4 as the anion source. 3-Any substance is acceptable, including but not limited to any one or at least two of phosphoric acid, lithium dihydrogen phosphate, ferric phosphate, and ferric manganese phosphate. The specific type of soluble iron source is also not limited, including but not limited to any one or at least two of ferrous oxalate dihydrate, anhydrous ferrous oxalate, and ferrous acetate. The specific type of manganese source is not limited; any commonly used manganese source in the field is acceptable, including but not limited to any one or at least one of manganese acetate and manganese acetate tetrahydrate. Titanium sources include but are not limited to titanium oxalate. Magnesium sources include any one or at least one of magnesium acetate and magnesium acetate tetrahydrate. A wide variety of organic carbon sources are acceptable, including but not limited to any one or at least two of polydopamine, glucose, fructose, cellulose, starch, sucrose, PEG (polyethylene glycol), ascorbic acid, citric acid, polyvinylpyrrolidone, and tannic acid.

[0052] In some embodiments, the grinding method is sand milling to further improve the preparation efficiency of the mixed slurry.

[0053] In some embodiments, the solid content of the mixed slurry is 10wt%-50wt%, the viscosity at 25°C is 100-1000mPa.s, and the median particle size D50 of the volume distribution satisfies 0.1μm≤D50≤0.2μm, so as to facilitate the formation of spherical lithium manganese iron phosphate precursors with uniform particle size distribution by spraying.

[0054] Specifically, the solid content of the mixed slurry can be 10wt%, 12wt%, 15wt%, 18wt%, 20wt%, 22wt%, 25wt%, 28wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt%, or any range of two such values. The viscosity of the slurry at 25°C can be 100mPa.s, 300mPa.s, 500mPa.s, 1000mPa.s, or any range of two such values, and the particle size D50 can be 0.1μm, 0.12μm, 0.15μm, 0.18μm, 0.2μm, or any range of two such values.

[0055] In some embodiments, the temperature for grinding to prepare the mixed slurry is 15-40°C to further reduce energy consumption. Specifically, the temperature for grinding to prepare the slurry can be 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, or any range of two values.

[0056] In some embodiments, in step S2 above, the inlet air temperature of the spray dryer is 200℃-300℃, the outlet air temperature is 80-150℃, and the feed rate of the mixed slurry is 10mL / min-100mL / min, so as to facilitate the preparation of spherical lithium manganese iron phosphate precursor with uniform particle size distribution.

[0057] Specifically, the inlet air temperature of the spray dryer can be 200℃, 220℃, 250℃, 280℃, 300℃, or any combination of two values; the outlet air temperature can be 80℃, 90℃, 100℃, 110℃, 120℃, 130℃, 140℃, 150℃, or any combination of two values; and the slurry feeding rate can be 10mL / min, 20mL / min, 30mL / min, 50mL / min, 60mL / min, 80mL / min, 100mL / min, or any combination of two values.

[0058] In some embodiments, in step S3 above, calcination is carried out under a protective atmosphere to avoid introducing impurity ions into the cathode material, which would affect the electrochemical performance of the cathode material. The protective atmosphere includes any one or a mixture of at least two of nitrogen, argon, or helium.

[0059] In some embodiments, the calcination temperature is 650-850℃, the holding time is 6-12h, and the calcination furnace pressure is 0-50mPa, in order to improve the preparation efficiency of the cathode material. Specifically, the calcination temperature can be 650℃, 680℃, 700℃, 720℃, 750℃, 780℃, 800℃, 820℃, 850℃, or any range of two values; the holding time can be 6h, 7h, 8h, 9h, 10h, 11h, 12h, or any range of two values.

[0060] In some embodiments, the heating rate of the lithium manganese iron phosphate precursor from room temperature to the calcination temperature before calcination is 1-5 °C / min, which facilitates the formation of a uniform and complete carbon coating layer on the substrate surface. Specifically, the heating rate can be 1 °C / min, 2 °C / min, 3 °C / min, 4 °C / min, 5 °C / min, or any combination of two values.

[0061] In another typical embodiment of this application, a lithium-ion battery is provided, which includes the positive electrode material provided in the first typical embodiment described above.

[0062] The lithium-ion battery provided in this application uses the above-mentioned ion-doped and carbon-coated co-modified cathode material, which is more conducive to suppressing Mn dissolution and improving its capacity and cycle stability.

[0063] In some embodiments, a lithium-ion battery includes a casing, an electrode assembly, and an electrolyte. Both the electrode assembly and the electrolyte are located within the casing.

[0064] The outer casing can be a packaging bag encapsulated with a sealing film (such as aluminum-plastic film), for example, a pouch battery. In other embodiments, it can also be a steel-cased battery, an aluminum-cased battery, etc.

[0065] Please see Figure 1 and Figure 2 The electrode assembly 100 includes a positive electrode 101, a negative electrode 102, and a separator 103, with the separator 103 disposed between the positive electrode 101 and the negative electrode 102. When an electrolyte (not shown) is present, please refer to [reference needed] for charging. Figure 1 Active ions (such as lithium ions) are extracted from the lattice of the positive electrode material (such as a lithium-ion intercalation compound) in the positive electrode 101, pass through the electrolyte and the separator 103, reach the negative electrode 102, and insert into the lattice of the negative electrode material. For discharge procedures, please refer to [link to relevant documentation]. Figure 2 Active ions (such as lithium ions) are deintercalated from the lattice of the negative electrode material of the negative electrode 102, pass through the electrolyte through the separator 103, reach the positive electrode 101 and are embedded in the lattice of the positive electrode material (such as lithium intercalation compound), generating electrons that travel from the negative electrode 102 to the positive electrode 101 through the external circuit. The reverse movement of electrons forms an electric current, which can be used by electrical appliances.

[0066] In some embodiments, the electrode assembly 100 may be a stacked structure, which is formed by alternatingly stacking a positive electrode 101, a separator 103, and a negative electrode 102. In other embodiments, the electrode assembly 100 may also be a wound structure, which is formed by sequentially stacking and then winding the positive electrode 101, the separator 103, and the negative electrode 102.

[0067] Positive electrode film

[0068] The positive electrode 101 includes a positive current collector and a positive electrode material active layer disposed on at least one surface of the positive current collector. The positive current collector can be aluminum foil or nickel foil, or any composite current collector disclosed in the prior art, such as, but not limited to, a current collector formed by combining the aforementioned conductive foil and polymer substrate. The positive electrode material active layer includes the aforementioned positive electrode active material.

[0069] The positive electrode material active layer also includes an adhesive for bonding the positive electrode active material particles to facilitate the formation of the film layer, and also to improve the bonding force between the positive electrode material active layer and the positive electrode current collector. In some embodiments, the adhesive may include, but is not limited to, at least one of polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon.

[0070] The positive electrode material active layer may further include a conductive material, which includes, but is not limited to, carbon-based materials, metal-based materials, conductive polymers, or any combination thereof. In some embodiments, carbon-based materials may include, but are not limited to, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, metal-based materials may include, but are not limited to, metal powders or metal fibers, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.

[0071] negative electrode sheet

[0072] The negative electrode 102 includes a negative electrode current collector and an active layer of negative electrode material disposed on at least one surface of the negative electrode current collector. The negative electrode current collector can be at least one of copper foil, nickel foil, stainless steel foil, titanium foil or carbon-based current collector, or any composite current collector disclosed in the prior art, such as, but not limited to, a current collector formed by combining the aforementioned conductive foil and polymer substrate.

[0073] The active layer of the negative electrode material includes the negative electrode material, which includes graphite, silicon, etc.

[0074] The active layer of the negative electrode material also includes a binder to bond the negative electrode active material particles, thereby facilitating the formation of the film layer and improving the bonding force between the active layer of the negative electrode material and the negative electrode current collector. In some embodiments, the binder may include, but is not limited to, polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, or nylon, etc.

[0075] The active layer of the negative electrode material may further include a conductive material, which includes, but is not limited to, carbon-based materials, metal-based materials, conductive polymers, or any combination thereof. In some embodiments, carbon-based materials may include, but are not limited to, natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, or any combination thereof. In some embodiments, metal-based materials may include, but are not limited to, metal powders or metal fibers, such as copper, nickel, aluminum, or silver. In some embodiments, the conductive polymer may be a polyphenylene derivative.

[0076] Separating membrane

[0077] The separator 103 includes a membrane layer with a porous structure, and its material includes, but is not limited to, at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyethylene terephthalate, polyimide, or aramid. For example, the separator 103 may be a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene nonwoven fabric, a polyethylene nonwoven fabric, or a polypropylene-polyethylene-polypropylene porous composite membrane, etc.

[0078] electrolytes

[0079] The electrolyte serves to conduct ions between the positive electrode 101 and the negative electrode 102. The electrolyte can be in one or more of the following states: gel, solid, and liquid. In some embodiments, the electrolyte is an electrolyte solution. The electrolyte solution conducts active ions between the positive electrode 101 and the negative electrode 102. In some embodiments, the electrolyte solution includes a lithium salt and an organic solvent. The lithium salt may be selected from, but is not limited to, lithium hexafluorophosphate (LiPF6). 6) One or more of the following lithium salts are used: lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium tetraphenylborate (LiB(C6H5)4), lithium methanesulfonate (LiCH3SO3), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl)imide (LiN(SO2CF3)2), lithium tris(trifluoromethanesulfonyl)methyl lithium (LiC(SO2CF3)3), lithium dioxarate borate (LiBOB), and lithium difluorophosphate (LiPO2F2). For example, LiPF6 is chosen as the lithium salt because it provides high ionic conductivity and improves cycling characteristics. The organic solvent can be a carbonate compound, a carboxylic acid ester compound, an ether compound, a nitrile compound, or others. Organic solvents or combinations thereof. Examples of carbonate compounds include, but are not limited to, diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), butyl carbonate (BC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, trifluoromethylethylene carbonate, or combinations thereof.

[0080] The beneficial effects of this application will be further illustrated below with reference to embodiments and comparative examples.

[0081] Example 1

[0082] This embodiment provides a cathode material, which is prepared according to the following steps:

[0083] (1) Weigh 1028.34g of ferrous acetate, 1533.65g of manganese acetate, 17.55g of titanium oxalate, and 32.18g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0084] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0085] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.591 Fe 0.394 Ti 0.005 Mg 0.010 PO4.

[0086] Example 2

[0087] This embodiment provides a cathode material, which is prepared according to the following steps:

[0088] (1) Weigh 1023.12g of ferrous acetate, 1528.46g of manganese acetate, 31.59g of titanium oxalate, and 32.18g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0089] (2) Pump the mixed slurry into the spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0090] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.589 Fe 0.392 Ti 0.009 Mg 0.010 PO4.

[0091] Example 3

[0092] This embodiment provides a cathode material, which is prepared according to the following steps:

[0093] (1) Weigh 1020.51g ferrous acetate, 1520.67g manganese acetate, 31.59g titanium oxalate, and 45.05g magnesium acetate tetrahydrate into a sand mill, add 4000g purified water, and add 156g tannic acid. After stirring for 30min, add 1560g lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0094] (2) Pump the mixed slurry into a spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃ to obtain the lithium manganese iron phosphate precursor.

[0095] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.586 Fe 0.391 Ti 0.009 Mg 0.014 PO4.

[0096] Example 4

[0097] This embodiment provides a cathode material, which is prepared according to the following steps:

[0098] (1) Weigh 1023.12g of ferrous acetate, 1536.25g of manganese acetate, and 45.02g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 156g of tannic acid (total mass of lithium source). After stirring for 30min, add 1560g of lithium dihydrogen phosphate (mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0099] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0100] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.592 Fe 0.394 Mg 0.014 PO4.

[0101] Example 5

[0102] This embodiment provides a cathode material, which is prepared according to the following steps:

[0103] (1) Weigh 1033.56g ferrous acetate, 1544.03g manganese acetate, and 31.59g titanium oxalate into a sand mill, add 4000g of purified water and 156g of tannic acid, stir for 30min, then add 1560g lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10), so that the solution reacts fully and the solid content of the mixture is controlled at 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0104] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0105] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.595 Fe 0.396 Ti 0.009 PO4.

[0106] Example 6

[0107] This embodiment provides a cathode material, which is prepared according to the following steps:

[0108] (1) Weigh 1038.78g of ferrous acetate, 1549.22g of manganese acetate, and 17.55g of titanium oxalate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0109] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0110] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.597 Fe 0.398 Ti 0.005 PO4.

[0111] Example 7

[0112] This embodiment provides a cathode material, which is prepared according to the following steps:

[0113] (1) Weigh 1020.51g of ferrous acetate, 1520.67g of manganese acetate, and 80.73g of titanium oxalate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0114] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0115] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.586 Fe 0.391 Ti 0.023 PO4.

[0116] Example 8

[0117] This embodiment provides a cathode material, which is prepared according to the following steps:

[0118] (1) Weigh 1038.78g of ferrous acetate, 1549.22g of manganese acetate, and 16.09g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0119] (2) Pump the mixed slurry into the spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0120] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.597 Fe 0.398 Mg 0.005 PO4.

[0121] Example 9

[0122] This embodiment provides a cathode material, which is prepared according to the following steps:

[0123] (1) Weigh 1020.51g of ferrous acetate, 1520.67g of manganese acetate, and 74.01g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate to allow the solution to react fully, and control the solid content of the mixture to 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0124] (2) Pump the mixed slurry into the spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0125] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.586 Fe 0.391 Mg 0.023 PO4.

[0126] Example 10

[0127] This embodiment provides a cathode material, which is prepared according to the following steps:

[0128] (1) Weigh 1023.12g of ferrous acetate, 1528.46g of manganese acetate, 31.59g of titanium oxalate, and 32.18g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 4140.4g of tannic acid, the total mass of lithium source. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:9.5) to allow the solution to react fully, and control the solid content of the mixture at 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0129] (2) Pump the mixed slurry into the spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0130] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.589 Fe 0.392 Ti 0.009 Mg 0.010 PO4.

[0131] Example 11

[0132] This embodiment provides a cathode material, which is prepared according to the following steps:

[0133] (1) Weigh 1023.12g of ferrous acetate, 1528.46g of manganese acetate, 31.59g of titanium oxalate, and 32.18g of magnesium acetate tetrahydrate into a sand mill, add 4000g of purified water, and add 163.8g of tannic acid (total mass of lithium source). After stirring for 30min, add 1560g of lithium dihydrogen phosphate (mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10.5) to allow the solution to react fully, and control the solid content of the mixture at 50wt%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0134] (2) Pump the mixed slurry into a spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃ to obtain the lithium manganese iron phosphate precursor.

[0135] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.589 Fe 0.392 Ti 0.009 Mg 0.010 PO4.

[0136] Example 12

[0137] This embodiment provides a cathode material that differs from Embodiment 2 in that, in step (1), the mass of tannic acid added is 15.0% of the mass of lithium dihydrogen phosphate.

[0138] Example 13

[0139] This embodiment provides a cathode material that differs from Embodiment 2 in that, in step (1), the mass of tannic acid added is 8.0% of the mass of lithium dihydrogen phosphate.

[0140] Comparative Example 1

[0141] This comparative example provides a cathode material, which is prepared according to the following steps:

[0142] (1) Weigh 738.90g of lithium carbonate and 3006.00g of ferromanganese phosphate (manganese-iron molar ratio 1.5) into a sand mill, and add 10.0% tannic acid by mass of the total lithium carbonate. Add 4000g of purified water to control the solid content of the mixture at 50%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0143] (2) Pump the mixed slurry into a spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃ to obtain the lithium manganese iron phosphate precursor.

[0144] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.6 Fe 0.4 PO4.

[0145] Comparative Example 2

[0146] This comparative example provides a cathode material, which is prepared according to the following steps:

[0147] (1) Weigh 1044.00g of ferrous acetate and 1737.00g of manganese acetate into a sand mill, add 4000g of purified water and 156g of tannic acid. After stirring for 30min, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully, and control the solid content of the mixture to 50%. Sand mill at 1200r / min for 2h until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0148] (2) Pump the mixed slurry into a spray dryer, control the slurry feed rate to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃ to obtain the LMFP precursor.

[0149] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.6 Fe 0.4 PO4.

[0150] Comparative Example 3

[0151] This comparative example provides a cathode material, which is prepared according to the following steps:

[0152] Weigh 1041.69g of ferrous acetate, 1554.41g of manganese acetate, 3.51g of titanium oxalate, and 3.22g of magnesium acetate tetrahydrate into a sand mill. Add 4000g of purified water and 156g of tannic acid. After stirring for 30 minutes, add 1560g of lithium dihydrogen phosphate (the mass ratio of lithium dihydrogen phosphate to tannic acid is 100:10) to allow the solution to react fully. The solid content of the mixture should be controlled at 50wt%. Sand mill at 1200r / min for 2 hours until the particle size D50 of the slurry is in the range of 0.15-0.2μm to obtain the mixed slurry.

[0153] (2) Pump the mixed slurry into the spray dryer, control the feeding speed of the mixed slurry to 40 mL / min, the inlet air temperature to 240℃, and the outlet air temperature to 100-120℃. After spray drying, the lithium manganese iron phosphate precursor is obtained.

[0154] (3) The above-mentioned lithium manganese iron phosphate precursor was placed in a graphite crucible and calcined in a box furnace. The initial calcination temperature was 30℃, the heating rate was 3℃ / min, and the calcination temperature was 750℃. The sample was held at 750℃ for 10 hours and then naturally cooled. The sample was then passed through a 200-mesh sieve to obtain a spherical cathode material. The spherical cathode material includes a matrix and a carbon coating layer on the surface of the matrix. The chemical formula of the matrix is ​​LiMn. 0.599 Fe 0.399 Ti 0.001 Mg 0.001 PO4.

[0155] Comparative Example 4

[0156] This comparative example provides a cathode material that differs from Example 2 in that tannic acid was not added in step (1).

[0157] Experimental Example 1

[0158] The cathode material provided in Example 2 was examined using scanning electron microscopy (SEM) and energy-dispersive X-ray spectroscopy (EDS). Figure 3 A cross-sectional SEM image of the cathode material provided in Example 2; Figure 4 The image shows a cross-sectional EDS diagram of the cathode material provided in Example 2.

[0159] from Figure 3 It can be seen that the surface of the positive electrode material provided in Example 2 is smooth and flat, which indicates that a uniform and complete coating layer is formed on the surface of the positive electrode material.

[0160] Figure 4 In the image, the brown highlights represent carbon, from... Figure 4 It can be seen that carbon is uniformly dispersed on the surface of the cathode material, indicating that the cathode material provided in Example 2 is coated with a carbon coating layer in situ, and the carbon coating layer is uniformly and continuously coated on the surface of the substrate.

[0161] Experimental Example 2

[0162] The cathode materials provided in Example 2 and Comparative Examples 1-2 were subjected to Raman spectroscopy. Figure 5 The Raman spectra of the cathode materials provided in Example 2 and Comparative Examples 1-2 are shown, with the peak value at 950 cm⁻¹. 1 The peak at that location represents PO4 3- The higher the intensity of the stretching vibration peak, the more matrix material is exposed to the Raman detection light source, and the higher the intensity of the peak, the more matrix material is exposed to the Raman detection light source. (1595 cm⁻¹) -1 The peak at that location represents the G band. A higher peak intensity indicates more graphite carbon exposed to the Raman detection light source. Therefore, the ratio of the two peaks, I(G) / I(PO4), is... 3- ) can represent the integrity of carbon coating on the matrix surface, and I(G) / I(PO4)3- The larger the value, the better the integrity of the coverage.

[0163] Experimental Example 3

[0164] The cathode materials provided in the examples and comparative examples were tested for D50, specific surface area, tap density, pH and powder resistivity, respectively. The results are shown in Table 1.

[0165] Among them, (1) the method for determining D50 is: the median particle size D50 of the volume distribution of the cathode material is tested using a Malvern 3000 laser particle size analyzer.

[0166] (2) The specific surface area was determined by using a Micron DX400 instrument to test the specific surface area of ​​the cathode material. Under constant temperature and low temperature, the amount of gas adsorbed on the solid surface at different relative pressures was measured. Based on the Brown-Nauer-Etter-Taylor adsorption theory and its formula (BET formula), the amount of monolayer adsorption of the sample was obtained, thereby calculating the specific surface area and pore size distribution data of the cathode material.

[0167] (3) The tap density was determined by using a Canta Dual Autotap device to test the tap density of the positive electrode material. A 100 mL negative electrode material sample was placed in a graduated cylinder and mechanically vibrated 1000 times. The tap density of the positive electrode material was then calculated based on the sample mass and the volume after tapping.

[0168] (4) The pH measurement method is as follows: The pH of the positive electrode material is tested using a METTLER TOLEDO FE28. The specific procedure is as follows: Take about 5g of positive electrode material sample, add 45mL of water, sonicate for 5min, and then let it stand for 10min. After calibrating the pH meter, insert the composite electrode into the supernatant solution to be tested. Calculate the pH value of the solution based on the potential difference between the measuring electrode and the reference electrode.

[0169] (5) The method for determining the resistivity of powder is as follows: The resistivity of the positive electrode material is tested using an FT-8100A. A certain voltage is applied across the mold cavity containing the powder sample, and the current passing through the sample is measured under a pressure of 8 MPa, thereby calculating the resistivity of the sample.

[0170] Table 1

[0171]

[0172]

[0173] Note: " / " indicates that the value cannot be measured.

[0174] Test Example 4

[0175] The cathode materials provided in the examples and comparative examples were analyzed for carbon content (C%) and [I(G) / I(PO4)].3- The detection is performed, and C / [I(G) / I(PO4)] is calculated accordingly. 3- The results are shown in Table 2 below.

[0176] Among them, (1) the detection method of carbon content (C%) is: high frequency induction furnace combustion infrared absorption method, the positive electrode material is burned with oxygen in a high temperature furnace to generate and release CO2 gas. This method is used to separate carbon elements from metal elements and their compounds. By measuring the CO2 content, the carbon content in the positive electrode material is calculated.

[0177] (2)I(G) and I(PO4 3- The determination method is as follows: the cathode material is detected using an XPLORA laser confocal Raman spectrometer. I(G) refers to the Raman spectrum of the cathode material at 1585 cm⁻¹. -1 C=C bond vibration peak intensity at the location; I(PO4) 3- This refers to the 950 cm⁻¹ region in the Raman spectrum measured for the cathode material. -1 PO4 at the location 3- Peak intensity of stretching vibration.

[0178] Table 2

[0179]

[0180]

[0181] As shown in Table 2, the I(G) / I(PO4) ratio of Comparative Example 2 and Examples 1-11 is... 3- The values ​​are almost identical and all greater than those of Comparative Example 1, indicating that the integrity of the carbon coating in Comparative Example 2 and Examples 1-11 is much better than that in Comparative Example 1. Furthermore, the C / [I(G) / I(PO4)] ratio in Example 12 is significantly higher than that in Comparative Example 1. 3- The value of C / [I(G) / I(PO4)] is 0.32, indicating that the coating thickness of Example 12 is thicker than that of Comparative Example 2 and Examples 1-11, resulting in an excessively large specific surface area and a low tap density, which affects the processing performance of the material. Meanwhile, the C / [I(G) / I(PO4)] value of Example 13 is... 3- The value of 0.24 indicates that the coating thickness of Example 13 is relatively thinner, which weakens the ability of Example 13 to inhibit the dissolution of Mn, resulting in a decrease in cycle performance, a decrease in the conductivity of the material, and a reduction in the electrochemical performance of the material.

[0182] In contrast to Example 1, I(G) / I(PO4) 3- The value is 1.63, C / [I(G) / I(PO4)] 3-The value of 1.01 indicates that the integrity of the carbon coating is poor, with more exposed LMFP. This is because manganese iron phosphate is used as raw material in the preparation process, so there is no ionic or atomic mixing between the transition metal elements and carbon atoms, resulting in poor integrity and uniformity of the carbon coating and poor improvement of the Jan Taylor effect of Mn.

[0183] Experimental Example 5

[0184] The atomic occupancy of transition metal sites in the cathode materials provided in the examples and comparative examples was measured respectively, and the results are shown in Table 3 below.

[0185] The atomic occupancy of transition metals was characterized using X-ray diffraction (XRD), and the results were further refined using Reitveld refinement of the XRD data using GSAS2 software. Reitveld refinement of XRD refers to obtaining the raw slow-scan XRD data of the LMFP according to the general rules of crystal X-ray diffraction. The data obtained from the slow-scan XRD data were then refined using the specialized Reitveld refinement software GSAG. After importing the LMFP crystal structure file and instrument parameter file, the zero-point drift, scale factor, background, cell parameters, peak shape parameters, atomic occupancy, atomic coordinates, temperature factor, and preferred orientation were corrected sequentially. During the refinement process, when chi 2 When Rwp < 3 and Rwp < 0.05, fine-tuning can be completed.

[0186] Table 3

[0187]

[0188] Table 3 shows that the atomic occupancy of the transition metal sites in Comparative Examples 1-4 and Examples 1-13 is less than 1, i.e., Occ(Mn) + Occ(Fe) + Occ(Ti) + Occ(Mg) < 1. Comparative Example 4 shows that the cathode material still has a certain amount of vacancy defects even without elemental doping. Examples 1-11 show that as the doping concentration increases, Occ(Ti) and Occ(Mg) gradually increase, indicating an increase in the amount of Ti and Mg doped at the transition metal sites. Furthermore, as the doping concentration increases, Occ(Fe) and Occ(Mn) gradually decrease, also indicating an increase in the amount of Ti and Mg doped at the transition metal sites and an increase in the substitution of Fe and Mn.

[0189] In addition, as shown in Table 3, Occ(Ti) and Occ(Mg) are both less than their corresponding stoichiometric ratios. This indicates that the soluble Ti and Mg sources not only occupy transition metal sites during the ionic or atomic level mixed doping process, but also some are doped in interstitial sites or Li sites. These occupation methods will also form a large number of point defects, thereby improving the electrochemical performance and cycle performance of the material.

[0190] From the Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg) combinations in Examples 1-3 and 4-9, although single-element doping can introduce point defects during ionic or atomic-level mixed doping, the number of point defects introduced by dual-element co-doping is greater, meaning the overall sum of Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg) is smaller. These doped point defect vacancies can effectively improve the Jamnelle effect of Mn, reduce the lattice strain caused by the Jamnelle effect, thereby suppressing Mn dissolution and improving the voltage decay of the cathode material.

[0191] Experimental Example 6

[0192] The cathode materials provided in the examples and comparative examples were assembled into coin-type lithium-ion batteries, and then electrochemical performance tests were conducted. The results are shown in Table 4 below.

[0193] Among them, (1) the button lithium-ion battery is prepared according to the following steps: the positive electrode material, the conductive agent acetylene black and the adhesive polyvinylidene fluoride are uniformly mixed in N-methylpyrrolidone at a mass ratio of 92:4:4 to form a slurry, which is then coated on aluminum foil and dried in a vacuum drying oven. Then, it is pressed into a positive electrode sheet by a tablet press, the negative electrode sheet is a lithium metal sheet, the electrolyte is 1 mol / L lithium hexafluorophosphate-ethylene carbonate: dimethyl carbonate (LiPF6-EC:DMC, volume ratio of 1:1), and a polypropylene porous membrane is used as the separator. The battery assembly is carried out in an argon glove box.

[0194] (2) Electrochemical performance test: The assembled coin cell battery was subjected to charge and discharge test. The charge and discharge voltage range was 2.5-4.3V, the nominal specific capacity was 154mAh / g, and the specific capacity of 1C discharge in the 1st / 30th / 50th cycle, the average voltage of 1C discharge in the 1st / 30th / 50th cycle / V, and the average voltage decay rate of 1C discharge in the 30th / 50th cycle were obtained.

[0195] Table 3

[0196]

[0197]

[0198] Note: "--" indicates no attenuation.

[0199] As shown in Table 4, compared with Examples 4-8 and Comparative Examples 1-4, in Examples 1-37 and 9-11, the discharge specific capacity of 1C increases with the increase of the number of cycles during the early stage of charge and discharge. This is due to the presence of a large number of transition metal atom vacancies in the crystal. The values ​​of Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg) are relatively low. These vacancies can promote the migration of lithium ions during cycling, thereby improving the capacity.

[0200] Furthermore, the formation of these transition metal atom vacancies significantly suppresses the decay of the average discharge voltage of the cathode material. Generally, the decrease in the average discharge voltage of the cathode material is mainly due to Mn dissolution, and the main reason for Mn dissolution is considered to be the lattice strain caused by the Jamette effect of Mn. These transition metal atom vacancies can weaken the Jamette distortion of Mn, suppress the lattice distortion of LMFP, and ultimately suppress Mn dissolution, thereby improving the voltage decay of LMFP. Therefore, the cycle performance of Examples 1-3, 7, and 9-11 is relatively better, with less voltage decay.

[0201] In Example 2, the average voltage increased in the early stage of the cycle, and the voltage decayed by only 0.24% after 50 cycles, resulting in a high voltage retention rate. Figure 6 These are the charge-discharge curves for the 1st, 30th, and 50th cycles of Example 2; from Figure 6 It can be seen that the cathode material provided in Example 2 has excellent cycle stability.

[0202] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A positive electrode material, characterized in that, The cathode material includes a matrix and a carbon coating layer located on at least a portion of the surface of the matrix, wherein the matrix has the general chemical formula LiMn. a Fe b N m PO4, N includes at least one of Ti or Mg; 0.586≤a≤0.6, 0.391≤b≤0.4, 0.005≤m≤0.023, a+b+m=1; the atomic occupancy of the transition metals satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(N)≤0.9955, 0.0022≤Occ(N)<m.

2. The cathode material according to claim 1, characterized in that, The N is Ti, where 0.005 ≤ m ≤ 0.

023.

3. The cathode material according to claim 1, characterized in that, The N is Mg, and 0.005 ≤ m ≤ 0.

023.

4. The cathode material according to claim 1, characterized in that, The N is Ti and Mg, and the general chemical formula of the matrix is ​​LiMn. a Fe b Ti c Mg d For PO4, 0.005≤c≤0.009 and 0.005≤d≤0.014; and the atomic occupancy of the transition metal sites satisfies: 0.9797≤Occ(Mn)+Occ(Fe)+Occ(Ti)+Occ(Mg)≤0.9955, Occ(Ti)<c, Occ(Mg)<d.

5. The cathode material according to any one of claims 1 to 4, characterized in that, The cathode material was characterized by Raman spectroscopy, and the cathode material satisfies: 5.70 ≤ I(G) / I(PO4). 3- )≤5.90; where I(G) is the Raman spectrum of the cathode material measured at 1585 cm⁻¹. -1 C=C bond vibration peak intensity at the location; I(PO4) 3- The 950 cm⁻¹ value in the Raman spectrum of the cathode material was measured. -1 PO4 at the location 3- Peak intensity of stretching vibration.

6. The cathode material according to claim 5, characterized in that, In the cathode material, the carbon mass content is C%, where 1.58 ≤ C ≤ 1.64, and 0.27 ≤ C / [I(G) / I(PO4)]. 3- )]≤0.

29.

7. The cathode material according to any one of claims 1 to 4, characterized in that, The median particle size D50 of the positive electrode material is 6μm-12μm. And / or, the specific surface area of ​​the positive electrode material is 8m². 2 / g-16m 2 / g.

8. The cathode material according to any one of claims 1 to 4, characterized in that, The pH of the positive electrode material is 8-11; And / or, the tap density of the positive electrode material is 1.3 g / cm³. 3 -1.9g / cm 3 .

9. The cathode material according to any one of claims 1 to 4, characterized in that, The resistivity of the positive electrode material is 100-300 S·cm.

10. A lithium-ion battery, characterized in that, The lithium-ion battery comprises the positive electrode material according to any one of claims 1 to 9.