A doped silicon-carbon electrode material and its preparation method, and a battery

By doping silicon-carbon electrode materials with nitrogen and/or phosphorus to form a porous structure and dense lattice, combined with vapor deposition and surface modification, the problem of electrode material pulverization caused by volume expansion of silicon-based materials is solved, the structural stability and lithium-ion transport performance of the electrode materials are improved, and the service life is extended.

CN123073052APending Publication Date: 2026-11-10YINSI (NINGBO) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611594904.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Silicon-based materials suffer from rapid capacity decay and shortened cycle life due to volume expansion during long-term use, which leads to electrode material pulverization and repeated rupture of the solid electrolyte interface film. This limits their commercialization process.

Method used

The structure of the silicon-carbon electrode material includes a doped carbon matrix, a vapor deposition layer, a doped non-carbon layer, and a carbon coating layer. By doping nitrogen and/or phosphorus elements into the carbon matrix, a porous structure and a dense lattice are formed. Combined with vapor deposition and surface modification treatment, the structural stability and conductivity are improved.

Benefits of technology

It effectively alleviates structural stress caused by volume expansion, reduces the risk of electrode material cracking, improves the structural integrity and service life of electrode materials, and enhances lithium-ion transport performance and cycle stability of electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application discloses a doped silicon-carbon electrode material, its preparation method, and a battery. The doped silicon-carbon electrode material includes: a doped carbon matrix, the doped carbon matrix comprising a doping element, the doping element being at least one selected from nitrogen and phosphorus; a vapor-phase deposition layer covering the outer surface and pores of the doped carbon matrix; a doped modified non-carbon layer disposed on the periphery of the vapor-phase deposition layer, the doped modified non-carbon layer containing at least one selected from nitrogen and phosphorus; and a carbon coating layer covering the periphery of the doped modified non-carbon layer. This application, by doping the doped carbon matrix with nitrogen and / or phosphorus, improves the interfacial affinity between the carbon matrix and the subsequent vapor-phase deposition layer, as the introduction of nitrogen and / or phosphorus is beneficial for controlling the electron cloud density of the doped carbon matrix and increasing active sites, thereby providing a stable adhesion basis for the uniform loading of the vapor-phase deposition layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of electrode material technology, and in particular to a doped silicon-carbon electrode material, its preparation method, and a battery. Background Technology

[0002] Lithium-ion batteries, as a key carrier of new energy storage technology, are widely used in new energy vehicles, consumer electronics, and large-scale energy storage. With the continuous improvement of market demands for lithium-ion battery performance, lithium-ion battery technology is constantly iterating, and the market's requirements for the energy density of lithium-ion batteries are becoming increasingly stringent. This also means that electrode materials, as one of the four key materials for lithium-ion batteries, are undergoing an upgrade from traditional graphite systems to high-capacity, fast-charge-discharge materials.

[0003] Currently, the theoretical specific capacity of traditional graphite anode materials is only 372 mAh / g, which is a major bottleneck restricting the improvement of energy density in lithium-ion batteries. In contrast, the theoretical specific capacity of silicon-based materials is as high as 4200 mAh / g, about 10 times that of traditional graphite anode materials, and is therefore considered an ideal material for the next generation of high-energy-density electrode materials. However, during long-term use and cycling, silicon-based materials experience volume expansion of over 300%, leading to phenomena such as electrode material pulverization and repeated rupture and regeneration of the solid electrolyte interface film. This continuously consumes active lithium, resulting in rapid capacity decay and shortened cycle life, severely restricting the commercialization process of silicon-based materials. Summary of the Invention

[0004] One objective of this application is to provide a doped silicon-carbon electrode material and its preparation method, as well as a battery, which is beneficial to improving the structural stability, operational stability, and conductivity of the silicon-carbon electrode material, as well as to improving the mechanical strength of the silicon-carbon electrode material to suppress the volume expansion of silicon, thereby improving operational stability and service life.

[0005] To achieve the above objectives, this application provides a doped silicon-carbon electrode material, comprising: a doped carbon matrix, wherein the doped carbon matrix includes a doping element, wherein the doping element includes at least one of nitrogen and phosphorus; a vapor deposition layer, wherein the vapor deposition layer covers the outer surface and the interior of the pores of the doped carbon matrix; a doped modified non-carbon layer, wherein the doped modified non-carbon layer is disposed on the outer periphery of the vapor deposition layer, wherein the doped modified non-carbon layer contains at least one of nitrogen and phosphorus; and a coated carbon layer, wherein the coated carbon layer covers the outer periphery of the doped modified non-carbon layer.

[0006] In some embodiments, the thickness of the doped non-carbon layer is 1 nm to 10 nm.

[0007] In some embodiments, the bulk phase and surface of the doped carbon matrix are doped with the doping element, and the doped silicon-carbon electrode material satisfies at least one of the following conditions: (a) the doped carbon matrix is ​​at least one of porous carbon material, carbon nanotube network, graphene network, and carbon nanotube / graphene composite network; (b) the specific surface area of ​​the doped carbon matrix is ​​500 m². 2 / g~2500m 2 / g, pore volume 0.5cm³ 3 / g~1.3cm 3 / g; (c) When the doping element includes nitrogen, the nitrogen content is 0.5wt%~15wt% based on the total mass of the doped carbon matrix; (d) When the doping element includes phosphorus, the phosphorus content is 1wt%~10wt% based on the total mass of the doped carbon matrix; (e) The vapor deposition layer includes nano-silicon particles, the median particle size of the nano-silicon particles is 1~30nm, and the mass fraction of the nano-silicon particles is 20wt%~70wt% based on the total mass of the doped silicon-carbon electrode material.

[0008] To achieve the above objectives, this application also provides a method for preparing a doped silicon-carbon electrode material, comprising the following steps: S100, dispersing a carbon precursor and a doping agent in a liquid medium, and drying the mixture to obtain a doped precursor, wherein the doping agent is used to provide the doping element; S200, subjecting the doped precursor to a first heating carbonization treatment in a protective gas atmosphere to obtain a first intermediate product, and subjecting the first intermediate product to a second heating carbonization treatment to obtain a second intermediate product; S300, activating the second intermediate product in a protective gas atmosphere to obtain a doped carbon matrix; S400, in a protective gas atmosphere... In an atmosphere, a silane gas source and a carbon gas source are used sequentially to perform vapor phase deposition on the outer surface and inside the pores of the doped carbon substrate to form a vapor phase deposition layer, thus obtaining a third intermediate product; S500, a precursor is introduced into the surface of the third intermediate product for surface modification treatment to form a doped modified non-carbon layer, thus obtaining a fourth intermediate product, wherein the doped modified non-carbon layer contains at least one of nitrogen and phosphorus elements, and the precursor includes at least one of a nitrogen source and a phosphorus source; S600, in a protective gas atmosphere, the fourth intermediate product and a carbon source are mixed and carbonized to form a coated carbon layer, thus obtaining a doped silicon-carbon electrode material.

[0009] In some embodiments, the preparation method satisfies at least one of the following conditions: (a) the carbon precursor is selected from at least one of glucose, sucrose, fructose, starch, cellulose, phenolic resin, resorcinol-formaldehyde resin, polyacrylonitrile, polyvinyl alcohol, polyethylene glycol, asphalt, epoxy resin, polyimide resin, and furan resin; (b) the dopant is selected from urea, melamine, dicyandiamide, cyanamide, hexamethylenediamine, aniline, pyrrole, dopamine, polypyrrole, polyaniline, polyethyleneimine, ammonia, nitric acid, amino acids, phosphoric acid, phytic acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium hypophosphite, triphenylphosphine, and triphenylphosphine. (c) The mass ratio of the carbon precursor to the doping agent is 1:(0.15~3.5); (d) When the doping element includes both nitrogen and phosphorus, the doping agent includes a nitrogen source providing nitrogen and a phosphorus source providing phosphorus, and the mass ratio of the carbon precursor, the nitrogen source and the phosphorus source is 1:(0.1~3):(0.05~2.5); (e) In step S100, the drying temperature is 60℃~100℃, the drying time is 12h~24h, and the liquid medium is ethanol and / or deionized water.

[0010] In some embodiments, the preparation method satisfies at least one of the following conditions: (a) the temperature of the first heating carbonization treatment is 300℃~500℃, and the time of the first heating carbonization treatment is 1h~3h; (b) the temperature of the second heating carbonization treatment is 600℃~1000℃, and the time of the second heating carbonization treatment is 1h~5h; (c) when the vapor phase deposition method is used in step S500, step S500 is: placing the third intermediate product in a gaseous precursor atmosphere, so that the silicon in the vapor phase deposition layer reacts in situ with the gaseous precursor to form a doped and modified non-carbon layer, wherein the gaseous precursor is selected from at least one of NH3, N2H4, PH3, and tris(dimethylamino)phosphine; d) In step S500, the nitrogen source in the precursor is selected from at least one of ammonia and nitrogen; the phosphorus source in the precursor is selected from at least one of phosphine, trimethyl phosphate, and tris(dimethylamino)phosphine; (e) In step S600, the carbon source is selected from at least one of glucose, sucrose, pitch, and polyacrylonitrile, the mass of the coated carbon layer is m1, the mass of the doped silicon-carbon electrode material is m2, 0.005m2≤m1≤0.02m2, the carbonization temperature is 500℃~800℃, the carbonization time is 0.5h~2h, and the thickness of the coated carbon layer is 2nm~10nm; (f) The surface modification temperature is 300℃~600℃, and the surface modification time is 0.5h~2h.

[0011] In some embodiments, step S300 includes the following steps: placing the second intermediate product in an activation furnace under a protective gas atmosphere and introducing water vapor and / or carbon dioxide to obtain a doped carbon matrix through activation treatment. The activation treatment temperature is 600℃~1000℃, the activation treatment time is 1h~15h, the activation treatment heating rate is 1℃ / min~10℃ / min, and the total flow rate of water vapor and / or carbon dioxide is 0.5L / min~10L / min. Step S500 includes the following steps: introducing a precursor into the surface of the third intermediate product for surface modification treatment to form a doped modified non-carbon layer to obtain an intermediate product to be treated; immersing the intermediate product to be treated in dilute hydrofluoric acid to remove unreacted impurities and generated phosphorus oxides; washing with deionized water until neutral; and drying to obtain a fourth intermediate product.

[0012] In some embodiments, the silane gas source is selected from at least one of methane, ethylsilane, propane, monochlorosilane, dichlorosilane, trichlorosilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane, and trimethylsilane; the carbon gas source is selected from at least one of methane, ethane, butane, propane, ethylene, propylene, butene, and acetylene; the flow rate ratio of the silane gas source to the protective gas is 1:(1~15), the flow rate ratio of the carbon gas source to the protective gas is 1:(1~15), the flow rate of the silane gas source is 0.5 L / min to 8 L / min, and the flow rate of the carbon gas source is... The flow rate is 0.5 L / min to 8 L / min; the protective gas is at least one of argon, nitrogen, and helium; the vapor deposition temperature of the silane gas source is 400℃ to 800℃, the vapor deposition heating rate of the silane gas source is 4℃ / min to 10℃ / min, and the vapor deposition time of the silane gas source is 60 min to 900 min; the vapor deposition temperature of the carbon gas source is 500℃ to 800℃, the vapor deposition heating rate of the carbon gas source is 4℃ / min to 10℃ / min, and the vapor deposition time of the carbon gas source is 60 min to 480 min.

[0013] To achieve the above objectives, this application also provides an electrode sheet, comprising the doped silicon-carbon electrode material as described above or the doped silicon-carbon electrode material prepared by the aforementioned preparation method.

[0014] To achieve the above objectives, this application also provides a battery including at least one electrode as described above.

[0015] Compared with the prior art, the beneficial effects of this application are as follows: (1) This application involves doping a carbon matrix with nitrogen and / or phosphorus. The introduction of nitrogen and / or phosphorus helps to regulate the electron cloud density of the carbon matrix and increase active sites, thereby improving the interfacial affinity between the carbon matrix and the subsequent vapor deposition layer, providing a stable adhesion basis for the uniform loading of the vapor deposition layer. Furthermore, the porous structure of the carbon matrix facilitates the containment of subsequently deposited active materials and provides a physical buffer space for volume changes of the active materials during charge-discharge cycles, thus alleviating structural stress caused by volume expansion and reducing the risk of cracking in the electrode material. Based on this, since the vapor deposition layer covers the outer surface and the interior of the pores of the carbon matrix, the active materials not only exist outside the particles but are also distributed within the internal pores. This increases the loading of active materials through the three-dimensional space within the carbon matrix. Simultaneously, the confinement effect of the pores helps to suppress the aggregation of active materials during subsequent heat treatment or charge-discharge processes. Meanwhile, by setting a doped and modified non-carbon layer on the periphery of the vapor-deposited layer, compared with the traditional carbon coating layer, the doped and modified non-carbon layer has a dense lattice structure and good chemical stability. It can act as a physical barrier to reduce direct contact between the electrolyte and the internal vapor-deposited layer, thereby reducing the risk of irreversible decomposition side reactions of the electrolyte on the surface of the active material. On the other hand, nitrogen-based and phosphorus-based compounds can form lithium-ion transport channels in the nanometer-thick doped and modified non-carbon layer during charge and discharge. Furthermore, the doped and modified non-carbon layer has good mechanical strength and rigidity, which can suppress the expansion of the active material, thereby enhancing the structural integrity of the electrode material. By setting a coating carbon layer with good electronic conductivity, the deficiency of insufficient electronic conductivity of the doped and modified non-carbon layer can be compensated, and the impact of external forces on the internal doped and modified non-carbon layer can also be reduced.

[0016] (2) In this application, the carbon precursor and dopant are dispersed in a liquid medium and dried to ensure uniform dispersion of the dopant and full contact with the carbon precursor. Based on this, the dopant precursor undergoes a first heating carbonization to achieve preliminary cross-linking and solidification, preventing structural collapse during subsequent high-temperature processing. A second heating carbonization is then performed to rearrange and graphitize the carbon framework to form a conductive network. Simultaneously, the dopant element is embedded into the lattice defect sites of the carbon framework through thermal diffusion, achieving uniform doping in both the bulk and surface phases. Furthermore, an activation treatment controllably introduces nanoscale pores into the second intermediate product. While increasing the specific surface area and providing sufficient pore volume, these pores offer ample loading space for subsequent vapor deposition and reserve a physical buffer region for the volume expansion of the active material during charging and discharging, thereby reducing the risk of cracking in the electrode material. Furthermore, silane and carbon gas sources were used sequentially for vapor phase deposition. First, silane was pyrolyzed to nucleate and grow into nano-silicon particles, which were uniformly loaded onto the three-dimensional porous structure and surface of the carbon-doped matrix. Subsequently, the carbon gas source formed a carbon coating layer on the surface of the nano-silicon particles, which helps to isolate adjacent nano-silicon particles, further reducing the risk of high-temperature agglomeration and sintering growth, and maintaining their nanoscale active state. Afterward, the precursor was introduced onto the surface of the third intermediate product for surface modification treatment, forming a doped and modified non-carbon layer with a dense lattice structure and good chemical stability. This helps to prevent direct contact between the electrolyte and the internal active material, reducing the risk of side reactions. By mixing carbon sources and carbonizing to form a coated carbon layer, the deficiency of insufficient electronic conductivity of the doped and modified non-carbon layer can be compensated for, and the impact of external forces on the internal doped and modified non-carbon layer can also be reduced. Detailed Implementation

[0017] The present application will be further described below with reference to specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0018] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variation thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements and may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0019] When a quantity, concentration, or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range is disclosed as “1 to 5”, the described range should be interpreted as including ranges “1 to 4”, “1 to 3”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range includes its endpoints and all integers and fractions within that range.

[0020] Approximate terms used in the specification and claims to modify quantities indicate that the invention is not limited to that specific quantity, but also includes acceptable modifications close to that quantity that do not alter the relevant essential function. Correspondingly, the use of "about," "approximately," etc., to modify a numerical value means that the invention is not limited to that precise value. In some instances, approximate terms may correspond to the precision of the instrument used to measure the value. In this application's specification and claims, scope definitions can be combined and / or interchanged, unless otherwise stated, these scopes include all subscopes contained therein.

[0021] This application provides a doped silicon-carbon electrode material, comprising: a doped carbon matrix, the doped carbon matrix including a doping element, the doping element including at least one of nitrogen and phosphorus; a vapor deposition layer, the vapor deposition layer covering the outer surface and the interior of the pores of the doped carbon matrix; a doped modified non-carbon layer, the doped modified non-carbon layer disposed on the periphery of the vapor deposition layer, the doped modified non-carbon layer containing at least one of nitrogen and phosphorus; and a coated carbon layer, the coated carbon layer covering the periphery of the doped modified non-carbon layer.

[0022] This application involves doping a carbon matrix with nitrogen and / or phosphorus. The introduction of nitrogen and / or phosphorus helps to regulate the electron cloud density of the carbon matrix and increase active sites, thereby improving the interfacial affinity between the carbon matrix and the subsequent vapor deposition layer, providing a stable adhesion basis for the uniform loading of the vapor deposition layer. Furthermore, the porous structure of the carbon matrix facilitates the containment of subsequently deposited active materials and provides a physical buffer space for volume changes of the active materials during charge-discharge cycles, thus alleviating structural stress caused by volume expansion and reducing the risk of electrode material cracking. Based on this, since the vapor deposition layer covers the outer surface and the interior of the pores of the carbon matrix, the active materials are not only present on the outside of the particles but also distributed within the internal pores. This increases the loading of active materials through the three-dimensional space within the carbon matrix. Simultaneously, the confinement effect of the pores helps to suppress the aggregation of active materials during subsequent heat treatment or charge-discharge processes. Meanwhile, by setting a doped and modified non-carbon layer on the periphery of the vapor-deposited layer, compared with the traditional carbon coating layer, the doped and modified non-carbon layer has a dense lattice structure and good chemical stability. It can act as a physical barrier to reduce direct contact between the electrolyte and the internal vapor-deposited layer, thereby reducing the risk of irreversible decomposition side reactions of the electrolyte on the surface of the active material. On the other hand, nitrogen-based and phosphorus-based compounds can form lithium-ion transport channels in the nanometer-thick doped and modified non-carbon layer during charge and discharge. Furthermore, the doped and modified non-carbon layer has good mechanical strength and rigidity, which can suppress the expansion of the active material, thereby enhancing the structural integrity of the electrode material. By setting a coating carbon layer with good electronic conductivity, the deficiency of insufficient electronic conductivity of the doped and modified non-carbon layer can be compensated, and the impact of external forces on the internal doped and modified non-carbon layer can also be reduced.

[0023] In some embodiments, the thickness of the doped non-carbon layer is 1 nm to 10 nm.

[0024] More preferably, the carbon matrix is ​​simultaneously doped with nitrogen and phosphorus. First, using a nitrogen-phosphorus co-doped carbon matrix as the vapor deposition matrix improves the conductivity and charge density of the carbon matrix while reducing interfacial impedance and enhancing its mechanical strength. This provides a more stable buffer space for the volume expansion of silicon nanoparticles and improves lithium storage kinetics and first coulombic efficiency due to the increased active sites. After vapor deposition, a surface-doped non-carbon layer is introduced. This surface-doped non-carbon layer can be in situ transformed into a high-ionic-conductivity interfacial phase (such as Li3PO4), thereby promoting lithium-ion desolvation, accelerating interfacial transport, suppressing electrolyte side reactions, and further improving the cycle stability and rate performance of the electrode material.

[0025] It is worth mentioning that the nitrogen and phosphorus co-doped carbon matrix and the vapor deposition layer work together to achieve the dual functions of confinement and conduction. The coated carbon layer and the doped carbon matrix jointly construct a three-dimensional dual carbon network, which further buffers volume expansion and improves the stability of the solid electrolyte interface film. The outermost coated carbon layer is beneficial to improving ion conduction performance and interface enhancement protection performance, thus forming a functional gradient of "conductivity enhancement - volume buffering - interface protection - ion transport optimization".

[0026] In some embodiments, the bulk phase and surface of the doped carbon matrix are doped with doping elements, and the doped carbon matrix is ​​at least one of porous carbon materials, carbon nanotube networks, graphene networks, and carbon nanotube / graphene composite networks. By selecting a suitable type of doped carbon matrix, it is beneficial to prepare silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0027] In some embodiments, the specific surface area of ​​the doped carbon matrix is ​​500 m². 2 / g~2500m 2 / g, pore volume 0.5cm³ 3 / g~1.3cm 3 By selecting a doped carbon matrix with a suitable pore structure, it is beneficial to prepare silicon-carbon electrode materials with good structural stability, operational stability and conductivity.

[0028] In some embodiments, when nitrogen is included in the doping elements, the nitrogen content is 0.5wt% to 15wt% based on the total mass of the doped carbon matrix. By selecting a doped carbon matrix with an appropriate amount of nitrogen, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability and conductivity.

[0029] In some embodiments, when phosphorus is included in the doping elements, the phosphorus content is 1wt% to 10wt% based on the total mass of the doped carbon matrix. By selecting a doped carbon matrix with an appropriate amount of phosphorus, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, usage stability and conductivity.

[0030] In some embodiments, the vapor-deposited layer includes nano-silicon particles with a median particle size of 1-30 nm and a mass fraction of 20 wt%-70 wt% based on the total mass of the doped silicon-carbon electrode material. By selecting a vapor-deposited layer with suitable composition, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0031] This application also provides a method for preparing a doped silicon-carbon electrode material, comprising the following steps: S100, dispersing a carbon precursor and a doping agent in a liquid medium, and drying the mixture to obtain a doped precursor, wherein the doping agent is used to provide the doping element; S200, subjecting the doped precursor to a first heating carbonization treatment in a protective gas atmosphere to obtain a first intermediate product, and subjecting the first intermediate product to a second heating carbonization treatment to obtain a second intermediate product; S300, activating the second intermediate product in a protective gas atmosphere to obtain a doped carbon matrix; S400, in a protective gas atmosphere... A third intermediate product is obtained by sequentially performing vapor deposition on the outer surface and inside the pores of a doped carbon matrix using silane gas source and carbon gas source to form a vapor deposition layer; S500, a precursor is introduced into the surface of the third intermediate product for surface modification treatment to form a doped modified non-carbon layer to obtain a fourth intermediate product, wherein the doped modified non-carbon layer contains at least one of nitrogen and phosphorus elements, and the precursor includes at least one of nitrogen source and phosphorus source; S600, the fourth intermediate product and carbon source are mixed in a protective gas atmosphere and carbonized to form a coated carbon layer to obtain a doped silicon-carbon electrode material.

[0032] This application disperses a carbon precursor and a dopant in a liquid medium and dries them, ensuring uniform dispersion and full contact between the dopant and the carbon precursor. Following this, the precursor undergoes a first-stage carbonization process to achieve initial cross-linking and solidification, preventing structural collapse during subsequent high-temperature processing. A second carbonization process then rearranges the carbon framework into graphitized material, forming a conductive network. Simultaneously, the dopant element diffuses into lattice defects in the carbon framework, achieving uniform doping in both the bulk and surface phases. Furthermore, an activation process controllably introduces nanoscale pores into the second intermediate product. This increases the specific surface area and provides ample pore volume, offering sufficient loading space for subsequent vapor deposition and reserving a physical buffer zone for the volume expansion of the active material during charging and discharging, thereby reducing the risk of cracking in the electrode material. Furthermore, silane and carbon gas sources were used sequentially for vapor phase deposition. First, silane was pyrolyzed to nucleate and grow into nano-silicon particles, which were uniformly loaded onto the three-dimensional porous structure and surface of the carbon-doped matrix. Subsequently, the carbon gas source formed a carbon coating layer on the surface of the nano-silicon particles, which helps to isolate adjacent nano-silicon particles, further reducing the risk of high-temperature agglomeration and sintering growth, and maintaining their nanoscale active state. Afterward, the precursor was introduced onto the surface of the third intermediate product for surface modification treatment, forming a doped and modified non-carbon layer with a dense lattice structure and good chemical stability. This helps to prevent direct contact between the electrolyte and the internal active material, reducing the risk of side reactions. By mixing carbon sources and carbonizing to form a coated carbon layer, the deficiency of insufficient electronic conductivity of the doped and modified non-carbon layer can be compensated for, and the impact of external forces on the internal doped and modified non-carbon layer can also be reduced.

[0033] It is understandable that introducing heteroatoms (such as nitrogen and phosphorus) into carbon materials is beneficial for altering the electronic structure and surface chemistry of carbon. Nitrogen doping, in particular, can introduce active sites such as pyridine nitrogen, pyrrole nitrogen, and graphitic nitrogen into carbon materials, improving their electronic conductivity and lithium-ion adsorption capacity. Due to the large covalent radius and lone pair electron effect of phosphorus atoms, phosphorus doping is beneficial for further expanding the carbon interlayer spacing, lowering the lithium-ion diffusion barrier, and inducing the formation of a stable solid electrolyte interface film rich in fast ion conductors such as Li3PO4.

[0034] In some embodiments, the carbon precursor is selected from at least one of glucose, sucrose, fructose, starch, cellulose, phenolic resin, resorcinol-formaldehyde resin, polyacrylonitrile, polyvinyl alcohol, polyethylene glycol, asphalt, epoxy resin, polyimide resin, and furan resin. By selecting a suitable type of carbon precursor, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0035] In some embodiments, the dopant is selected from at least one of urea, melamine, dicyandiamide, cyanamide, hexamethylenediamine, aniline, pyrrole, dopamine, polypyrrole, polyaniline, polyethyleneimine, ammonia, nitric acid, amino acids, phosphoric acid, phytic acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium hypophosphite, triphenylphosphine, phosphorus trichloride, and triethyl phosphate. By selecting suitable dopant, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0036] In some embodiments, the amino acid selected in the dopant may be at least one of L-lysine and arginine.

[0037] In some embodiments, the doping agent is preferably a mixture of phytic acid and ammonium dihydrogen phosphate, wherein the mass ratio of phytic acid to ammonium dihydrogen phosphate is 1:(0.5~3).

[0038] In some embodiments, the mass ratio of carbon precursor to doping agent is 1:(0.15~3.5). By selecting appropriate amounts of carbon precursor and doping agent, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, use stability and conductivity.

[0039] It is understandable that the mass ratio of carbon precursor to dopant can be 1:0.15, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, or 1:3.5.

[0040] In some embodiments, when the doping elements include both nitrogen and phosphorus, the doping agent includes a nitrogen source providing nitrogen and a phosphorus source providing phosphorus, and the mass ratio of the carbon precursor, nitrogen source, and phosphorus source is 1:(0.1~3):(0.05~2.5). By selecting appropriate amounts of carbon precursor, nitrogen source, and phosphorus source, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0041] In some embodiments, in step S100, the drying temperature is 60°C to 100°C, the drying time is 12h to 24h, and the liquid medium is ethanol and / or deionized water. By selecting suitable drying conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0042] In some embodiments, the temperature of the first heating carbonization treatment is 300℃~500℃, and the time of the first heating carbonization treatment is 1h~3h. By selecting suitable conditions for the first heating carbonization treatment, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, use stability and conductivity.

[0043] In some embodiments, the temperature of the second heating carbonization treatment is 600℃~1000℃, and the time of the second heating carbonization treatment is 1h~5h. By selecting appropriate conditions for the second heating carbonization treatment, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, use stability and conductivity.

[0044] In some embodiments, when vapor deposition is used in step S500, step S500 involves placing the third intermediate product in a gaseous precursor atmosphere, causing the silicon in the vapor-deposited layer to undergo an in-situ chemical reaction with the gaseous precursor to form a doped and modified non-carbon layer. The gaseous precursor is selected from at least one of NH3, N2H4, PH3, and tris(dimethylamino)phosphine. By selecting suitable processing conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0045] In some embodiments, the surface modification treatment temperature in step S500 is 300℃~600℃, and the surface modification treatment time is 0.5h~2h. By selecting suitable treatment conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, usage stability, and conductivity.

[0046] In some embodiments, a doped and modified non-carbon layer may be prepared in step S500 using chemical vapor deposition (CVD).

[0047] In some embodiments, in step S500, the nitrogen source in the precursor is selected from at least one of ammonia and nitrogen; the phosphorus source in the precursor is selected from at least one of phosphine, trimethyl phosphate, and tris(dimethylamino)phosphine. By selecting suitable processing conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0048] In some embodiments, the phosphorus source in the precursor can form a phosphorus-containing matrix during high-temperature processing. During subsequent charge and discharge of the battery, lithium ions in the electrolyte (or lithium ions provided by the counter electrode) will undergo insertion or extraction. During this process, some lithium ions will undergo an electrochemical reaction with the phosphorus element in the material to generate Li3PO4 in situ. This in-situ generated Li3PO4 typically serves as an effective component or buffer matrix for solid electrolyte interfacial films, helping to improve the structural stability and conductivity of the material.

[0049] In some embodiments, in step S600, the carbon source is selected from at least one of glucose, sucrose, pitch, and polyacrylonitrile; the mass of the carbon coating layer is m1; the mass of the doped silicon-carbon electrode material is m2; 0.005m2≤m1≤0.02m2; the carbonization temperature is 500℃~800℃; the carbonization time is 0.5h~2h; and the thickness of the carbon coating layer is 2nm~10nm. By selecting suitable processing conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0050] In some embodiments, step S300 includes the following steps: placing the second intermediate product in an activation furnace under a protective gas atmosphere and introducing water vapor and / or carbon dioxide to obtain a doped carbon matrix through activation treatment. The activation treatment temperature is 600℃~1000℃, the activation treatment time is 1h~15h, the activation treatment heating rate is 1℃ / min~10℃ / min, and the total flow rate of water vapor and / or carbon dioxide is 0.5L / min~10L / min. Step S500 includes the following steps: introducing a precursor onto the surface of the third intermediate product for surface modification treatment to form a doped modified non-carbon layer to obtain the intermediate product to be treated; immersing the intermediate product to be treated in dilute hydrofluoric acid to remove unreacted impurities and generated phosphorus oxides; washing with deionized water until neutral; and drying to obtain the fourth intermediate product. By selecting appropriate processing conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, usage stability, and conductivity.

[0051] The concentration of dilute hydrofluoric acid was 0.1wt%~2wt%, and the soaking time in dilute hydrofluoric acid was 1min~30min. After washing with deionized water until neutral, the fourth intermediate product was obtained by vacuum drying for 6h~12h at a temperature of 60℃~80℃.

[0052] In some embodiments, the silane gas source is selected from at least one of methane, ethylsilane, propane, monochlorosilane, dichlorosilane, trichlorosilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane, and trimethylsilane; the carbon gas source is selected from at least one of methane, ethane, butane, propane, ethylene, propylene, butene, and acetylene; the flow rate ratio of the silane gas source to the protective gas is 1:(1~15), the flow rate ratio of the carbon gas source to the protective gas is 1:(1~15), the flow rate of the silane gas source is 0.5 L / min to 8 L / min, and the flow rate of the carbon gas source is 0.5 L / min to 8 L / min. The vapor deposition rate is L / min, the vapor deposition pressure of the silane gas source is 10 Pa to 500 Pa; the protective gas is at least one of argon, nitrogen, and helium; the vapor deposition temperature of the silane gas source is 400℃ to 800℃, the vapor deposition heating rate of the silane gas source is 4℃ / min to 10℃ / min, and the vapor deposition time of the silane gas source is 60 min to 900 min; the vapor deposition temperature of the carbon gas source is 500℃ to 800℃, the vapor deposition heating rate of the carbon gas source is 4℃ / min to 10℃ / min, and the vapor deposition time of the carbon gas source is 60 min to 480 min. By selecting appropriate processing conditions, it is beneficial to obtain silicon-carbon electrode materials with good structural stability, operational stability, and conductivity.

[0053] This application also provides an electrode sheet, comprising the doped silicon-carbon electrode material as described above or the doped silicon-carbon electrode material prepared by the aforementioned preparation method. Using the doped silicon-carbon electrode material provided in this application, or the doped silicon-carbon electrode material prepared by the method provided in this application, in the electrode sheet is beneficial for improving the structural stability, operational stability, and conductivity of the electrode sheet.

[0054] This application also provides a battery including at least one electrode as described above. Using the electrode provided in this application in the battery is beneficial for improving the battery's energy density and rate performance.

[0055] Example 1 Example 1 provides a method for preparing a silicon-carbon doped electrode material and a battery, including the following steps: Step (1): Dissolve aqueous phenolic resin, urea, and phosphoric acid in deionized water at a mass ratio of 1:0.5:0.5. After stirring evenly, dry at 80℃ for 24 hours to obtain the doped precursor. Carbonize the doped precursor at 400℃ for 2 hours under an inert atmosphere, then heat to 850℃ for 3 hours to obtain the second intermediate product. Place the obtained second intermediate product under a nitrogen atmosphere and activate it by introducing steam at a flow rate of 5 L / min for 8 hours to obtain the doped carbon matrix.

[0056] Step (2): The doped carbon matrix was placed in a fluidized bed, and a SiH4 gas source was introduced under a nitrogen atmosphere. Chemical vapor deposition was carried out for 10 hours at 500℃ and a SiH4 gas source flow rate of 2.5 L / min. Subsequently, acetylene gas was introduced for coating under an inert atmosphere. The ratio of acetylene gas flow rate to nitrogen gas flow rate was 1:1, the acetylene gas flow rate was 3 L / min, the acetylene coating temperature was 500℃, the acetylene coating heating rate was 5℃ / min, and the acetylene coating time was 240 min, yielding a third intermediate product. The third intermediate product contained 50 wt% silicon, 6.3 wt% nitrogen, and 5.8 wt% phosphorus.

[0057] Step (3): The third intermediate product was placed in an NH3 atmosphere and treated at 400°C for 1 hour to allow the silicon in the vapor-deposited layer to undergo an in-situ chemical reaction with the gaseous precursor to form a nitrogen-doped modified non-carbon layer, thus obtaining the fourth intermediate product. The fourth intermediate product was then immersed in 0.2 wt% dilute hydrofluoric acid for 30 minutes, washed with deionized water until neutral, and vacuum dried at 70°C for 10 hours to obtain the fourth intermediate product. The fourth intermediate product contained 50 wt% silicon, 14.6 wt% nitrogen, and 4.3 wt% phosphorus.

[0058] Step (4): Mix the fourth intermediate product with polyacrylonitrile and carbonize at 500°C for 2 hours under a nitrogen atmosphere to obtain a doped silicon-carbon electrode material. The mass fraction of silicon in the doped silicon-carbon electrode material is 50 wt%, the mass fraction of nitrogen is 13.2 wt%, the mass fraction of phosphorus is 3.5 wt%, the mass of the carbon coating layer in the doped silicon-carbon electrode material is m1, the mass of the doped silicon-carbon electrode material is m2, and m1 = 0.005m2.

[0059] Step (5): Mix the doped silicon-carbon electrode material, Super P, carbon nanotubes, and LA132 in a mass ratio of 94:1:1:4, dissolve and disperse them evenly in pure water, coat them onto copper foil, dry them, and roll them to form a negative electrode sheet. Use the prepared negative electrode sheet as the working electrode, lithium metal sheet as the counter electrode and reference electrode, and a 1.2 mol / L LiPF6 electrolyte (the solvent is ethylene carbonate (EC) and diethyl carbonate (DEC), with a volume ratio of EC to DEC of 1:1) as the electrolyte. Use polypropylene as the separator and assemble it into a CR2032 button battery in a glove box.

[0060] Example 2 The difference between Example 2 and Example 1 is that step (1) is replaced by: dissolving aqueous phenolic resin and phytic acid in deionized water at a mass ratio of 1:1, stirring evenly, and drying at 80°C for 24 hours to obtain a doped precursor. The doped precursor is then carbonized at 400°C for 2 hours under an inert atmosphere, followed by carbonization at 850°C for 3 hours to obtain a second intermediate product. The obtained second intermediate product is placed under a nitrogen atmosphere and activated by introducing steam at a flow rate of 5 L / min for 8 hours to obtain a doped carbon matrix.

[0061] Example 3 The difference between Example 3 and Example 1 is that the mass ratio of waterborne phenolic resin, urea and phosphoric acid in step (1) is 1:0.1:0.1.

[0062] Example 4 The difference between Example 4 and Example 1 is that the mass ratio of waterborne phenolic resin, urea and phosphoric acid in step (1) is 1:2.5:2.

[0063] Example 5 The difference between Example 5 and Example 1 is that step (3) is replaced by: placing the third intermediate product in a pH3 atmosphere and treating it at 400°C for 1 hour to allow the silicon in the vapor-deposited layer to undergo an in-situ chemical reaction with the gaseous precursor to form a phosphorus-containing doped and modified non-carbon layer, thus obtaining the fourth intermediate product. The fourth intermediate product is then immersed in 0.2 wt% dilute hydrofluoric acid for 30 minutes, washed with deionized water until neutral, and vacuum dried at 70°C for 10 hours to obtain the fourth intermediate product.

[0064] Example 6 The difference between Example 6 and Example 1 is that step (1) is replaced by: dissolving aqueous phenolic resin and dopamine in deionized water at a mass ratio of 1:0.5, stirring evenly, and drying at 80°C for 24 hours to obtain a doped precursor. The doped precursor is then carbonized at 400°C for 2 hours under an inert atmosphere, followed by carbonization at 850°C for 3 hours to obtain a second intermediate product. The obtained second intermediate product is placed under a nitrogen atmosphere and activated by introducing steam at a flow rate of 5 L / min for 8 hours to obtain a doped carbon matrix.

[0065] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that steps (3) and (4) were not performed.

[0066] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that step (4) was not performed.

[0067] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that urea and phosphoric acid were not added in step (1), and steps (3) and (4) were not performed.

[0068] The initial coulombic efficiency, initial charge specific capacity, and 50-cycle capacity retention of the lithium-ion batteries prepared in Examples 1-6 and Comparative Examples 1-3 were tested. The initial charge and discharge were performed using a stepped decreasing current regime, and the specific steps were as follows: (1) Let the battery stand for 10 minutes to allow the open circuit potential to stabilize; (2) Perform constant current discharge at a rate of 0.1C, with a cutoff voltage of 0.005V (relative to Li / Li). + (3) Let stand for 10 minutes; (4) Discharge at a constant current rate of 0.05C, with a cutoff voltage of 0.005V (relative to Li / Li). + (5) Let stand for 10 minutes; (6) Discharge at a constant current rate of 0.02C, with a cutoff voltage of 0.005V (relative to Li / Li). + (7) Let stand for 10 minutes; (8) Charge at a constant current rate of 0.1C with a cutoff voltage of 1.5V (relative to Li / Li). + ).

[0069] Table 1: Performance Tests of Lithium-ion Batteries

[0070] Comparative studies of Examples 1-6 show that doping with an appropriate amount of heteroatoms is beneficial for controlling the electron cloud density of the doped carbon matrix, increasing the density of active sites, and thus enhancing the interfacial affinity between the doped carbon matrix and the vapor-deposited layer, providing a stable adhesion basis for the uniform loading of nano-silicon. Therefore, when the doping amount of nitrogen and / or phosphorus is too low, the improvement on the electronic structure and interfacial affinity of the doped carbon matrix is ​​limited. When the doping amount of nitrogen and / or phosphorus is too high, excessive heteroatoms introduce too many defect sites, reducing electronic conductivity. Simultaneously, excessive doping may cause some heteroatoms to exist in an unstable form within the carbon framework, increasing the risk of irreversible side reactions.

[0071] By comparing Example 1 with Comparative Examples 1-3, it can be seen that selecting appropriate preparation conditions is beneficial to obtaining battery materials with high initial charge specific capacity, initial coulombic efficiency and usage stability.

[0072] The basic principles, main features, and advantages of this application have been described above. Those skilled in the art should understand that this application is not limited to the above embodiments. The embodiments and descriptions in the specification are merely the principles of this application. Various changes and modifications can be made to this application without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claims. The scope of protection claimed by this application is defined by the appended claims and their equivalents.

Claims

1. A silicon-doped carbon electrode material, characterized in that, include: A doped carbon matrix, wherein the doped carbon matrix comprises a doping element, wherein the doping element comprises at least one of nitrogen and phosphorus; A vapor deposition layer, wherein the vapor deposition layer covers the outer surface and the interior of the pores of the doped carbon matrix; A doped and modified non-carbon layer is disposed on the outer periphery of the vapor deposition layer, and the doped and modified non-carbon layer contains at least one of nitrogen and phosphorus elements. A carbon coating layer is applied to the periphery of the doped and modified non-carbon layer.

2. The doped silicon-carbon electrode material according to claim 1, characterized in that, The thickness of the doped and modified non-carbon layer is 1 nm to 10 nm.

3. The doped silicon-carbon electrode material according to claim 1, characterized in that, The bulk phase and surface of the doped carbon matrix are doped with the doping element, and the doped silicon-carbon electrode material satisfies at least one of the following conditions: (a) The doped carbon matrix is ​​at least one of porous carbon materials, carbon nanotube networks, graphene networks and carbon nanotube / graphene composite networks; (b) The specific surface area of ​​the doped carbon matrix is ​​500 m². 2 / g~2500m 2 / g, pore volume 0.5cm³ 3 / g~1.3cm 3 / g; (c) When the doping element includes nitrogen, the nitrogen content is 0.5 wt% to 15 wt% based on the total mass of the doped carbon matrix; (d) When the doping element includes phosphorus, the phosphorus content is 1 wt% to 10 wt% based on the total mass of the doped carbon matrix; (e) The vapor-deposited layer includes nano-silicon particles with a median particle size of 1 to 30 nm and a mass fraction of 20 wt% to 70 wt% based on the total mass of the doped silicon-carbon electrode material.

4. A method for preparing a silicon-carbon doped electrode material, characterized in that, Including the following steps: S100. A carbon precursor and a doping agent are dispersed in a liquid medium and dried to obtain a doped precursor, wherein the doping agent is used to provide doping elements. S200. In a protective gas atmosphere, the doped precursor is subjected to a first heating carbonization treatment to obtain a first intermediate product. The first intermediate product is subjected to a second heating carbonization treatment to obtain a second intermediate product. S300. In a protective gas atmosphere, the second intermediate product is activated to obtain a doped carbon matrix; S400. In a protective gas atmosphere, a silane gas source and a carbon gas source are used successively to perform vapor phase deposition on the outer surface and inside the pores of the doped carbon matrix to form a vapor phase deposition layer, thereby obtaining a third intermediate product. S500. Introduce the precursor into the surface of the third intermediate product for surface modification treatment to form a doped and modified non-carbon layer to obtain a fourth intermediate product. The doped and modified non-carbon layer contains at least one of nitrogen and phosphorus elements, and the precursor includes at least one of nitrogen source and phosphorus source. S600. In a protective gas atmosphere, the fourth intermediate product is mixed with a carbon source and subjected to carbonization treatment to form a coated carbon layer, thereby obtaining a doped silicon-carbon electrode material.

5. The preparation method according to claim 4, characterized in that, The preparation method satisfies at least one of the following conditions: (a) The carbon precursor is selected from at least one of glucose, sucrose, fructose, starch, cellulose, phenolic resin, resorcinol-formaldehyde resin, polyacrylonitrile, polyvinyl alcohol, polyethylene glycol, asphalt, epoxy resin, polyimide resin, and furan resin; (b) The doping agent is selected from at least one of urea, melamine, dicyandiamide, cyanamide, hexamethylenediamine, aniline, pyrrole, dopamine, polypyrrole, polyaniline, polyethyleneimine, ammonia, nitric acid, amino acids, phosphoric acid, phytic acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, sodium hypophosphite, triphenylphosphine, phosphorus trichloride, and triethyl phosphate; (c) The mass ratio of the carbon precursor to the doping agent is 1:(0.15~3.5); (d) When the doping element includes both nitrogen and phosphorus, the doping agent includes a nitrogen source providing nitrogen and a phosphorus source providing phosphorus, and the mass ratio of the carbon precursor, the nitrogen source, and the phosphorus source is 1:(0.1~3):(0.05~2.5). (e) In step S100, the drying temperature is 60℃~100℃, the drying time is 12h~24h, and the liquid medium is ethanol and / or deionized water.

6. The preparation method according to claim 4, characterized in that, The preparation method satisfies at least one of the following conditions: (a) The temperature of the first heating carbonization treatment is 300℃~500℃, and the time of the first heating carbonization treatment is 1h~3h; (b) The temperature of the second heating carbonization treatment is 600℃~1000℃, and the time of the second heating carbonization treatment is 1h~5h; (c) When the vapor deposition method is used in step S500, step S500 is: placing the third intermediate product in a gaseous precursor atmosphere, so that the silicon in the vapor deposition layer reacts in situ with the gaseous precursor to form a doped and modified non-carbon layer, wherein the gaseous precursor is selected from at least one of NH3, N2H4, PH3, and tris(dimethylamino)phosphorus. (d) In step S500, the nitrogen source in the precursor is selected from at least one of ammonia and nitrogen; the phosphorus source in the precursor is selected from at least one of phosphine, trimethyl phosphate, and tris(dimethylamino)phosphine. (e) In step S600, the carbon source is selected from at least one of glucose, sucrose, pitch, and polyacrylonitrile, the mass of the coated carbon layer is m1, the mass of the doped silicon-carbon electrode material is m2, 0.005m2≤m1≤0.02m2, the carbonization temperature is 500℃~800℃, the carbonization time is 0.5h~2h, and the thickness of the coated carbon layer is 2nm~10nm; (f) In step S500, the surface modification treatment temperature is 300℃~600℃ and the surface modification treatment time is 0.5h~2h.

7. The preparation method according to claim 4, characterized in that, Step S300 includes the following steps: In a protective gas atmosphere, the second intermediate product is placed in an activation furnace and water vapor and / or carbon dioxide are introduced to obtain a doped carbon matrix through activation treatment. The activation treatment temperature is 600℃~1000℃, the activation treatment time is 1h~15h, the activation treatment heating rate is 1℃ / min~10℃ / min, and the total flow rate of water vapor and / or carbon dioxide is 0.5L / min~10L / min. Step S500 includes the following steps: introducing a precursor into the surface of the third intermediate product for surface modification treatment to form a doped and modified non-carbon layer to obtain the intermediate product to be treated; immersing the intermediate product to be treated in dilute hydrofluoric acid to remove unreacted impurities and generated phosphorus oxides; washing it with deionized water until neutral; and drying it to obtain the fourth intermediate product.

8. The preparation method according to any one of claims 4 to 7, characterized in that, The silane gas source is selected from at least one of methylsilane, ethylsilane, propane, monochlorosilane, dichlorosilane, trichlorosilane, tetrafluorosilane, hexamethyldisilane, dichlorodimethylsilane, and trimethylsilane; The carbon source is selected from at least one of methane, ethane, butane, propane, ethylene, propylene, butene, and acetylene; The flow rate ratio of the silane gas source to the protective gas is 1:(1~15), the flow rate ratio of the carbon gas source to the protective gas is 1:(1~15), the flow rate of the silane gas source is 0.5L / min~8L / min, and the flow rate of the carbon gas source is 0.5L / min~8L / min. The protective gas is at least one of argon, nitrogen, and helium; The vapor deposition temperature of the silane gas source is 400℃~800℃, the vapor deposition heating rate of the silane gas source is 4℃ / min~10℃ / min, and the vapor deposition time of the silane gas source is 60min~900min. The vapor deposition temperature of the carbon gas source is 500℃~800℃, the vapor deposition heating rate of the carbon gas source is 4℃ / min~10℃ / min, and the vapor deposition time of the carbon gas source is 60min~480min.

9. An electrode sheet, characterized in that, This includes the doped silicon-carbon electrode material as described in any one of claims 1 to 3, or the doped silicon-carbon electrode material prepared by the preparation method described in any one of claims 4 to 8.

10. A battery, characterized in that, It includes at least one electrode as described in claim 9.