A negative electrode active material, a method for preparing the negative electrode active material, an electrode assembly, a secondary battery, and an electrical device.

By constructing a multi-level pore structure of micropores, mesopores, and macropores in porous graphite materials, the volume expansion effect of traditional artificial graphite anode active materials is solved, thereby improving the energy density, fast charging performance, and cycle stability of the battery.

CN123073064APending Publication Date: 2026-11-10HEFEI HONGCHU TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611346661.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Traditional artificial graphite anode active materials suffer from volume expansion during charge and discharge, leading to problems such as electrode structure damage, reduced coulombic efficiency, and short cycle life.

Method used

The material is a porous graphite material with micropores on the surface and mesopores and macropores arranged sequentially inside. The micropores and mesopores are connected, and the macropores and mesopores are partially connected. A multi-level pore structure is constructed through a specific process, including mixing carbon source and MOF-derived catalyst, pre-carbonization, catalytic activation and graphitization treatment.

Benefits of technology

It improves the specific capacity and first-cycle coulombic efficiency of the negative electrode active material, enhances the lithium-ion transport rate, provides physical buffer space, suppresses structural pulverization, and achieves high energy density, fast charging capability and long cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073064A_ABST
    Figure CN123073064A_ABST
Patent Text Reader

Abstract

This invention discloses a negative electrode active material, a method for preparing the negative electrode active material, an electrode assembly, a secondary battery, and an electrical device, relating to the field of battery manufacturing technology. The negative electrode active material includes a porous graphite material with a porosity of 15% to 30%. The surface of the porous graphite material has micropores, and mesopores and macropores are sequentially arranged in the direction close to the interior of the porous graphite. At least some of the mesopores are connected to the micropores, and at least some of the macropores are connected to the mesopores, thereby achieving synergistic enhancement of the three functions of "micropore lithium storage, mesopore transport, and macropore wetting buffer", ultimately realizing a comprehensive improvement in the negative electrode active material in terms of volume stability, fast charging performance, energy density, and economy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery manufacturing technology, and in particular to a negative electrode active material, a method for preparing the negative electrode active material, an electrode assembly, a secondary battery, and an electrical device. Background Technology

[0002] Due to its abundant resources, stable structure, and good safety, artificial graphite has become the mainstream anode active material for lithium-ion batteries. However, traditional artificial graphite anode active materials still face many technical bottlenecks in meeting the requirements of high energy density, fast charging, and long cycle life in today's lithium-ion batteries.

[0003] Existing technologies exhibit a volume expansion effect: taking graphite materials as an example, during charging and discharging, they undergo lithium ion insertion and extraction, resulting in a volume change (approximately 20%). This repeated volume change disrupts the integrity of the electrode structure, accelerates the rupture and reconstruction of the solid electrolyte interphase (SEI) film, continuously consumes electrolyte and active lithium, and reduces coulombic efficiency and cycle life.

[0004] The patent CN120423538B proposes to reduce volume expansion by introducing specific additives to generate a closed-cell structure. Although this method can effectively alleviate structural changes during cycling, the closed-cell structure may hinder ion transport, leading to a decrease in rate performance, and the process control is difficult.

[0005] Therefore, there is an urgent need to develop a material that can alleviate volume expansion, take into account ion transport dynamics, and is simple to process. Summary of the Invention

[0006] The main objective of this invention is to provide a negative electrode active material, a method for preparing the negative electrode active material, an electrode assembly, a secondary battery, and an electrical device, aiming to solve the problem of battery performance degradation caused by the volume expansion effect during charging and discharging of traditional artificial graphite negative electrode active materials in the prior art.

[0007] To achieve the above objectives, the present invention proposes a negative electrode active material, wherein the negative electrode active material comprises a porous graphite material with a porosity of 15% to 30%, the surface of the porous graphite material has micropores, and mesopores and macropores are sequentially arranged in the direction near the interior of the porous graphite, at least some of the mesopores are connected to the micropores, and at least some of the macropores are connected to the mesopores.

[0008] In one embodiment, in the hierarchical channels, the pore size of the micropores is <2 nm, and the number of micropores accounts for 50%-70% of the total number of pores in the porous graphite material; and / or, The mesopores have a pore size of 2-50 nm, and their number accounts for 25%-50% of the total number of pores in the porous graphite material; and / or, The pore size of the macropores is ≥50nm, and the number of macropores accounts for 5%-15% of the total number of pores in the porous graphite material.

[0009] In one embodiment, the grain size La(110) of the porous graphite material is 80-140 nm, and Lc(002) is 35-45 nm; and / or, The particle size of the negative electrode active material is 8~15μm.

[0010] In one embodiment, the porous graphite material comprises a carbon material, which includes at least one of graphite and amorphous carbon.

[0011] This invention provides a method for preparing the aforementioned negative electrode active material, the method comprising the following steps: The carbon source and MOF-derived catalyst are mixed and pulverized to obtain a mixture. The mixture is then pre-carbonized under an inert atmosphere to obtain a pre-carbonized product. The pre-carbonized product is mixed with a pore-forming agent and catalytically activated in a water vapor atmosphere to form a carbon precursor with multi-level pores. The carbon precursor with the multi-level channels is graphitized, demagnetized, and sieved to obtain the negative electrode active material.

[0012] In one embodiment, the MOF-derived catalyst accounts for 0.5-5% of the mass of the carbon source; and / or, The carbon source includes at least one selected from pitch coke, petroleum coke, needle coke, shot coke, metallurgical coke, and anthracite; and / or, The MOF-derived catalysts include ZIF-67-derived cobalt-nitrogen-carbon catalysts or ZIF-8-derived zinc oxide-nitrogen-carbon catalysts.

[0013] In one embodiment, the pre-carbonization treatment step includes: heating the mixture in an inert gas atmosphere at a heating rate of 10-50°C / min to a temperature of 800-1000°C, holding the temperature for 2-4 hours, and then cooling it to 100-200°C to obtain the pre-carbonized product.

[0014] In one embodiment, the pore-forming agent accounts for 10-30% of the mass of the pre-carbonized product; and / or, The pore-forming agent includes organic or inorganic pore-forming agents; and / or, The pore-forming agent includes at least one of ammonium bicarbonate, ammonium chloride, and urea; and / or, In the catalytic activation step, catalytic activation is carried out under conditions of 5-15% water vapor concentration, wherein the catalytic activation temperature is 850-950℃ and the catalytic activation time is 1-3h.

[0015] In one embodiment, in step S30, the temperature of the graphitization treatment is 2400-3200℃, and the time of the graphitization treatment is 24-48h.

[0016] In one embodiment, the present invention also provides an electrical device comprising a secondary battery as described above.

[0017] In the technical solution of this invention, the micropores distributed on the surface and / or inside of the porous graphite material greatly increase the specific surface area of ​​the material, providing abundant short-range lithium-ion storage active sites, effectively improving the specific capacity and first-cycle coulombic efficiency of the negative electrode active material; the mesopores distributed in the porous graphite material and communicating with the micropores serve as intermediate transport bridges connecting the micropores and macropores, significantly shortening the solid-phase diffusion path of lithium ions migrating from the interior to the exterior of the porous graphite material, significantly reducing ion transport resistance, thereby improving the rate performance and fast charging capability of the material; the macropores distributed in the porous graphite material and communicating with the mesopores serve as electrolyte reservoirs and high-speed ion transport channels, ensuring the electrolyte... The electrolyte can quickly and fully penetrate the deep regions of porous graphite materials, allowing for full utilization of the internal microporous active sites. Simultaneously, it provides the necessary physical buffer space for the volume expansion of the porous graphite material during lithium-ion insertion and extraction, effectively suppressing structural pulverization and electrode stripping during cycling. Furthermore, the simple preparation process ensures low cost and the feasibility of large-scale production. Interconnected structures ensure the integrity of the ion transport pathway, while a reasonable proportion ensures that the functional capacity of each pore level matches its role in the transport chain. The combined effect of these two factors ultimately achieves a comprehensive improvement in the negative electrode active material's volume stability, fast-charging performance, energy density, and economic efficiency. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0019] Figure 1 This is a schematic cross-sectional view of the negative electrode active material according to an embodiment of the present invention.

[0020] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0021] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially. Furthermore, the meaning of "and / or" throughout the text includes three parallel solutions; for example, "A and / or B" includes solution A, or solution B, or a solution where both A and B are satisfied simultaneously. In addition, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0022] Existing technologies exhibit a volume expansion effect: taking graphite materials as an example, during charging and discharging, they undergo lithium ion insertion and extraction, resulting in a volume change (approximately 20%). This repeated volume change disrupts the integrity of the electrode structure, accelerates the rupture and reconstruction of the solid electrolyte interphase (SEI) film, continuously consumes electrolyte and active lithium, and reduces coulombic efficiency and cycle life.

[0023] The patent CN120423538B proposes to reduce volume expansion by introducing specific additives to generate a closed-cell structure. Although this method can effectively alleviate structural changes during cycling, the closed-cell structure may hinder ion transport, leading to a decrease in rate performance, and the process control is difficult.

[0024] Therefore, there is an urgent need to develop a material that can alleviate volume expansion, take into account ion transport dynamics, and is simple to process.

[0025] In view of this, the present invention proposes a negative electrode active material, the negative electrode active material comprising a porous graphite material, the porous graphite material having a porosity of 15% to 30%, the surface of the porous graphite material having micropores, and mesopores and macropores being sequentially arranged in the direction near the interior of the porous graphite, at least some of the mesopores communicating with the micropores, and at least some of the macropores communicating with the mesopores.

[0026] In the technical solution of this invention, the micropores distributed on the surface and / or inside of the porous graphite material greatly increase the specific surface area of ​​the material, providing abundant short-range lithium-ion storage active sites, effectively improving the specific capacity and first-cycle coulombic efficiency of the negative electrode active material; the mesopores distributed in the porous graphite material and connected to the micropores serve as intermediate transport bridges connecting the micropores and macropores, significantly shortening the solid-phase diffusion path of lithium ions migrating from the interior to the exterior of the porous graphite material, significantly reducing ion transport resistance, thereby improving the rate performance and fast charging capability of the material; the macropores distributed in the porous graphite material and connected to the mesopores serve as electrolyte reservoirs and high-speed ion transport channels, ensuring electrolysis The liquid can quickly and fully penetrate the deep regions of porous graphite materials, allowing for full utilization of the internal microporous active sites. Simultaneously, it provides the necessary physical buffer space for the volume expansion of the porous graphite material during lithium-ion insertion and extraction, effectively suppressing structural pulverization and electrode stripping during cycling. Furthermore, the simple preparation process ensures low cost and the feasibility of large-scale production. Specifically, interconnectedness ensures the integrity of the ion transport path, while a reasonable proportion ensures that the functional capacity of each pore level matches its role in the transport chain. The combined effect of these two factors ultimately achieves a comprehensive improvement in the negative electrode active material's volume stability, fast-charging performance, energy density, and economic efficiency.

[0027] In this article, "the percentage of the number of pores" refers to the percentage of a certain level of pores (micropores, mesopores, or macropores) in the total number of pores in the porous graphite material.

[0028] In some embodiments, the pore size of the micropores is <2 nm, and the number of micropores accounts for 50%-70% of the total number of pores in the porous graphite material; and / or, The mesopores have a pore size of 2-50 nm, and their number accounts for 25%-50% of the total number of pores in the porous graphite material; and / or, The pore size of the macropores is ≥50nm, and the number of macropores accounts for 5%-15% of the total number of pores in the porous graphite material.

[0029] In the technical solution of this invention, micropores smaller than 2 nm have extremely high specific surface areas, providing a large number of additional adsorption and storage sites for lithium ions, thereby improving the overall specific capacity of the negative electrode active material. This helps guide the uniform growth of the solid electrolyte interphase (SEI) film within the pores, reducing the continuous consumption of electrolyte, and thus improving the first-cycle coulombic efficiency and long-cycle stability of the battery. Meanwhile, the mesopore size matches the kinetic diameter of solvated lithium ions. As the main channels for lithium ion transport within the particles, they significantly shorten the lithium ion diffusion path and significantly reduce ion transport resistance. This rapid transport channel ensures that lithium ions can be rapidly inserted / extracted in high-current charge-discharge (fast charging) scenarios, avoiding polarization and thus endowing the material with excellent fast-charging capabilities. Macropores larger than 50 nm act as electrolyte reservoirs and macroscopic permeation channels, ensuring that the electrolyte can quickly and deeply penetrate the core area of ​​the secondary particles, avoiding the formation of "dry zones" inside. They provide sufficient physical space to effectively accommodate and buffer the huge volume expansion stress generated during lithium ion insertion, preventing particle pulverization.

[0030] Specifically, the pore size of micropores can be 1 nm or 2 nm, the pore size of mesopores can be 2 nm, 4 nm, 10 nm, 15 nm, 20 nm, 40 nm or 50 nm, and the pore size of macropores can be 55 nm, 60 nm, 65 nm or 70 nm. Within the above range, micropores, mesopores and macropores form interconnected multi-level channels to construct a "three-dimensional ion diffusion network", thereby achieving comprehensive performance advantages of high capacity, fast charging, long cycle time and low expansion.

[0031] In some embodiments, the grain size La(110) of the porous graphite material is 80-140 nm, and Lc(002) is 35-45 nm. Controlling La within a relatively large range of 80-140 nm means that the basal plane of the carbon microcrystals is longer and the degree of graphitization is higher. This can significantly reduce the electron transport resistance of the material, provide excellent electronic conductivity, and ensure that the battery still has excellent capacity performance during high-rate charge and discharge. The Lc value represents the stacking height of the graphite microcrystals in the direction perpendicular to the carbon layer (c-axis). Controlling Lc within a moderate range of 35-45 nm can provide more channels for the insertion / extraction of sodium ions, significantly reduce ion diffusion resistance, improve rate performance, and prevent pulverization or structural collapse, thereby ensuring the long-term cycle stability of the battery.

[0032] In some embodiments, the porous graphite material is a carbon material, which includes at least one of graphite and amorphous carbon. Graphite provides high capacity and excellent conductivity, while the introduction of amorphous carbon can effectively improve the interfacial stability of the material, buffer volume expansion and improve rate performance, so that the final negative electrode active material achieves a better overall balance between energy density, cycle life and fast charging capability.

[0033] In some embodiments, the preparation steps of the negative electrode active material include: The carbon source and MOF-derived catalyst are mixed and pulverized to obtain a mixture. The mixture is then pre-carbonized under an inert atmosphere to obtain a pre-carbonized product. The pre-carbonized product is mixed with a pore-forming agent and catalytically activated in a water vapor atmosphere to form a carbon precursor with multi-level pores. The carbon precursor with the multi-level channels is graphitized, demagnetized, and sieved to obtain the negative electrode active material.

[0034] In this article, "hierarchical pores" refers to the objectively existing pores (micropores, mesopores, macropores) of different sizes within the material. A schematic diagram of the micropores, mesopores, and macropores in the final prepared negative electrode active material is shown below. Figure 1 As shown.

[0035] In the technical solution of this invention, the mixing, pulverization, and pre-carbonization treatment of the carbon source and MOF-derived catalyst enable the MOF-derived catalyst nanoparticles to be uniformly anchored on the surface of the carbon source particles. The pre-carbonization process initially transforms the carbon source into a porous material structure with a certain degree of crystallinity, while simultaneously fixing the catalyst firmly in the microscopic region of the porous material, laying the foundation for the subsequent precise positioning of micropores. Next, the pore-forming agent is mixed with the pre-carbonization product and catalytically activated in a water vapor atmosphere. This step simultaneously constructs multi-level channels through a dual mechanism: on the one hand, the MOF-derived catalyst is activated into highly catalytically active nano-metal oxide particles in a water vapor atmosphere, catalyzing the decomposition of water vapor to generate localized active oxygen species that perform nanoscale etching on the porous graphite material, generating a large number of micropores in situ on the surface and inside of the porous material; on the other hand, the pore-forming agent decomposes upon heating at the activation temperature, releasing a large amount of gas. The resulting expansion pressure opens up the microscopic gaps inside the porous material, forming mesopores and macropores. Simultaneously, the porous material undergoes structural densification and agglomeration under the action of gas expansion and thermal recombination, forming a framework within the porous material. The accumulated voids further form a macroporous network, thereby creating a hierarchical distribution structure in the carbon precursor, where micropores are distributed on the surface and inside of the porous graphite material, and mesopores and macropores are distributed inside the porous material, with the three types of channels spatially interconnected. Finally, graphitization treatment imparts a highly graphitized crystalline structure to the porous material to improve conductivity and lithium storage capacity, while effectively preserving the hierarchical pore structure constructed in step S20. In addition, the metal components (such as Zn) in the MOF-derived catalyst may be reduced, evaporated, or... Aggregation and deactivation result in the formation of macropores in their original locations. After demagnetization and sieving to remove some residual metal components of the catalyst, a negative electrode active material with a three-dimensional ion diffusion network of micropores, mesopores, and macropores from the outside to the inside is obtained. This achieves precise control over the pore size and spatial distribution, ensuring the functional division and synergistic effect of micropores providing abundant lithium storage active sites, mesopores accelerating lithium-ion transport, and macropores promoting electrolyte wetting and buffering volume expansion. This improves specific capacity and rate performance while also ensuring cycle stability and volume stability.

[0036] Specifically, the micropores are mainly formed by MOF-derived catalyst (such as ZnO) nanoparticles anchoring on primary particles during the pre-carbonization stage. During the catalytic activation stage, active oxygen species use these catalysts as a starting point to "nanoscale sculpt" the surrounding carbon atoms, thereby etching a large number of extremely small micropores on the surface of the porous graphite material.

[0037] Mesopores are mainly distributed between the pore walls of porous graphite materials, connecting the micropore entrances on the surface and the macropore network inside to form an ion transport path from the outside to the inside. This is mainly because, in the catalytic activation process, the etching effect of water vapor on the porous graphite material at high temperature will gradually expand some of the micropores and form mesopores.

[0038] Macropores are mainly distributed inside porous graphite materials, primarily formed by the compression of some gas generated by the pore-forming agent. In addition, the metal components (such as Zn) in MOF-derived catalysts undergo reduction, evaporation, or agglomeration deactivation at high temperatures, and the "cavities" left in situ directly contribute to the macroporous structure.

[0039] In some embodiments, the MOF-derived catalyst accounts for 0.5-5% of the total mass of the carbon source; for example, it can be 0.5%, 0.8%, 1%, 2%, 4% or 5%. Too little catalyst will lead to insufficient pore formation and incomplete pore development; while too much catalyst will not only increase the amount of non-carbon impurities in the material and reduce the carbon purity and electrochemical performance of the final product, but may also cause the metal nanoparticles to agglomerate at high temperatures, which will reduce the catalytic efficiency. Within the above range, the catalytic activation reaction can be fully carried out to obtain the ideal hierarchical pore structure, while the high carbon content and structural integrity of the product can be maintained to the maximum extent.

[0040] In some embodiments, the average particle size D50 of the mixture is 8-15 μm. Specifically, the average particle size D50 of the mixture can be 8 μm, 10 μm, 12 μm or 12 μm. Within the above range, good processing fluidity can be ensured, and the depth and uniformity of catalytic activation pore formation can be ensured.

[0041] In some embodiments, the carbon source includes at least one of pitch coke, petroleum coke, needle coke, shot coke, metallurgical coke, and anthracite, because these carbon sources are all high-carbon, low-heteroatom, high-quality precursors with extremely high carbon yields and good graphitization potential. They readily form ordered carbon microcrystalline structures under high-temperature processing and are widely available and inexpensive. By introducing MOF-derived catalysts for catalytic activation and pore formation, the shortcomings of underdeveloped natural pores in these traditional carbon materials can be effectively overcome. While retaining their high conductivity and high stability, they are endowed with a rich hierarchical pore structure, thereby significantly improving their sodium storage performance as a sodium-ion battery anode active material.

[0042] In some embodiments, the MOF-derived catalyst includes a ZIF-67-derived cobalt-nitrogen-carbon catalyst or a ZIF-8-derived zinc oxide-nitrogen-carbon catalyst. This is because ZIFs (zeolite imidazole ester frameworks) can form a unique structure after high-temperature pyrolysis, forming highly dispersed metal / metal oxide nanoparticles (such as Co and ZnO) embedded in a nitrogen-doped carbon matrix. This structure not only possesses extremely high catalytic activity, efficiently catalyzing the reaction of water vapor with porous graphite materials to create directional pores, but also allows the residual trace metals and nitrogen elements to serve as active sites, further enhancing the material's lithiophilicity and electrochemical energy storage performance.

[0043] Taking the ZIF-8 derived zinc oxide nitrogen-carbon catalyst as an example, since the pyrolysis temperature is lower than the temperature at which zinc undergoes significant carbothermic reduction, zinc is highly dispersed in the nitrogen-doped carbon matrix mainly in the form of ZnO nanoparticles. It should be noted that in the subsequent high-temperature activation step, the ZnO nanoparticles are tightly coated by the graphitized carbon matrix, and volatilization is significantly suppressed, thus allowing them to remain stably present in the final negative electrode active material in the form of ZnO.

[0044] In some embodiments, the pre-carbonization treatment step includes: heating the mixture in an inert gas atmosphere at a heating rate of 10-50°C / min to a temperature of 800-1000°C, holding at that temperature for 2-4 hours, and then cooling it to 100-200°C to obtain a pre-carbonized product. The pre-carbonization treatment imparts suitable porosity and reactivity to the pre-carbonized product, enabling it to be efficiently etched and pore-created by a catalyst in subsequent steps.

[0045] In some embodiments, the pore-forming agent accounts for 10-30% of the total mass of the pre-carbonized product. For example, it can be 10%, 15%, 20%, 25%, or 30%. If the amount of pore-forming agent added is too low, the amount of gas generated will be insufficient to form a sufficient number and size of pores in the porous graphite material, failing to achieve the desired pore-forming effect. If the amount added is too high, the large amount of gas released instantaneously will cause the porous graphite material to over-expand or even collapse, damaging the structural integrity and mechanical strength of the material, resulting in a decrease in yield. This ratio range ensures that the gas generated by the decomposition of the pore-forming agent forms uniform, interconnected hierarchical pores inside the porous graphite material, while maintaining the structural stability of the framework.

[0046] In some embodiments, the pore-forming agent includes at least one of ammonium bicarbonate, ammonium chloride, and urea because these substances undergo rapid and complete thermal decomposition reactions during heating, generating a large amount of gas. This gas generates high pressure within the closed or semi-closed porous graphite material, acting as both a "physical explosion" and a "chemical etching" process, thereby expanding and forming abundant mesopores and macropores within the carbon material.

[0047] In some embodiments, the catalytic activation step is carried out under the condition of a water vapor concentration of 5-15%, wherein the catalytic activation temperature is 850-950℃ and the catalytic activation time is 1-3h. Within the above range, water vapor physical activation has high pore-forming efficiency while maintaining the structural integrity of porous graphite materials. The concentration of 5-15% is a volume percentage, that is, the volume percentage of water vapor in the total volume of the mixed protective gas.

[0048] In some embodiments, the graphitization temperature is 2400-3200℃ and the graphitization time is 24-48h. Within the above range, not only can precise etching be achieved, but the pore structure can also be fully developed, while avoiding excessive reaction that would damage the crystallinity of the porous graphite material.

[0049] The present invention also provides an electrode assembly, wherein the lithium-ion battery includes the aforementioned negative electrode active material. Therefore, this electrode assembly possesses all the beneficial effects of the aforementioned negative electrode active material, which will not be elaborated further here.

[0050] The present invention also provides a secondary battery comprising the electrode assembly described above, and thus the secondary battery has all the beneficial effects of the aforementioned electrode assembly, which will not be repeated here.

[0051] The present invention also provides an electrical device comprising the secondary battery described above. Therefore, this electrical device possesses all the beneficial effects of the aforementioned secondary battery, which will not be elaborated upon further here. The technical solution of the present invention will be further described in detail below with reference to specific embodiments and accompanying drawings. It should be understood that the following embodiments are merely illustrative of the present invention and are not intended to limit the present invention.

[0052] Example 1 This embodiment 1 provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (98wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (2wt%) were mixed and mechanically ground to D50=8.5μm. Under nitrogen protection, the mixture was heated to 900℃ at 5℃ / min and held for 3h for pre-carbonization; (2) The pre-carbonized product is uniformly mixed with ammonium bicarbonate (20 wt% relative to the mass of the pre-carbonized product), and catalytically activated at 900°C for 2 h in an argon atmosphere containing 10% water vapor by volume to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 3000℃ for 36h, and finally demagnetized and sieved to obtain the negative electrode active material.

[0053] The ZIF-8 derived zinc oxide nitrogen-carbon catalyst used in this embodiment and the following embodiments can be prepared as follows: 0.54 g (about 1.8 mmol) of zinc nitrate hexahydrate (Zn(NO3)2·6H2O) was weighed and dissolved in 30 mL of methanol to prepare a zinc nitrate methanol solution with a concentration of about 0.06 mol / L; 1.18 g (about 14.4 mmol) of 2-methylimidazole (2-MIM) was weighed and dissolved in 30 mL of methanol to prepare a 2-methylimidazole methanol solution with a concentration of about 0.48 mol / L, wherein the molar ratio of 2-methylimidazole to zinc ions was about 8:1; the 2-methylimidazole methanol solution was added to the zinc nitrate methanol solution, and the mixture was stirred at room temperature (25°C) for 24 h to allow ZIF-8 crystals to grow fully; then the precipitate was collected by centrifugation (8000 rpm, 10 min), washed three times with methanol (30 mL each time), and dried under vacuum at 60°C for 12 h to obtain the ZIF-8 precursor. The ZIF-8 precursor was placed in a tube furnace and heated to 700°C at a heating rate of 5°C / min under nitrogen protection and held at that temperature for 3 hours for high-temperature pyrolysis. The furnace was then allowed to cool naturally to room temperature to obtain the ZIF-8-derived zinc oxide carbon catalyst, which is also the ZIF-8-derived ZnO / NC catalyst.

[0054] Example 2 This embodiment provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (95wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (5wt%) were mixed and mechanically ground to D50=11μm. Under nitrogen protection, the mixture was heated to 900℃ at 5℃ / min and held for 3h for pre-carbonization. (2) The pre-carbonized product is uniformly mixed with ammonium bicarbonate (30wt%) and catalytically activated at 900℃ for 2h in an argon atmosphere containing 15% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level pores is loaded into a graphitization furnace, then treated at 3000℃ for 36h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0055] Example 3 This embodiment provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (99.5 wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (0.5 wt%) were mixed and mechanically ground to D50=11 μm. Under nitrogen protection, the mixture was heated to 850℃ at 5℃ / min and held for 2h for pre-carbonization. (2) The pre-carbonized product is uniformly mixed with urea (10wt%) and catalytically activated at 900℃ for 2h in an argon atmosphere containing 5% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 3000℃ for 36h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0056] Example 4 This embodiment provides a method for preparing a negative electrode active material, including the following steps: (1) Needle coke (95wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (5wt%) were mixed and mechanically ground to D50=15.5μm. Under nitrogen protection, the mixture was heated to 900℃ at 5℃ / min and held for 3h for pre-carbonization. (2) The pre-carbonized product is uniformly mixed with ammonium bicarbonate (10wt%) and catalytically activated at 900℃ for 2h in an argon atmosphere containing 10% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 3000℃ for 36h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0057] Comparative Example 1 This comparative example provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (99.6 wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (0.4 wt%) were mixed and mechanically ground to D50=11 μm. Under nitrogen protection, the mixture was heated to 950℃ at 5℃ / min and held for 4h for pre-carbonization. (2) The pre-carbonized product was uniformly mixed with urea (20wt%) and catalytically activated at 950℃ for 3h in an argon atmosphere containing 10% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 2800℃ for 30h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0058] Comparative Example 2 This comparative example provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (94.9 wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (5.1 wt%) were mixed and mechanically ground to D50=11 μm. Under nitrogen protection, the mixture was heated to 950℃ at 5℃ / min and held for 4h for pre-carbonization. (2) The pre-carbonized product was uniformly mixed with urea (20wt%) and catalytically activated at 950℃ for 3h in an argon atmosphere containing 10% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 2800℃ for 30h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0059] Comparative Example 3 This comparative example provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (98wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (2wt%) were mixed and mechanically ground to D50=11μm. Under nitrogen protection, the mixture was heated to 950℃ at 5℃ / min and held for 4h for pre-carbonization; (2) The pre-carbonized product was uniformly mixed with urea (9.9 wt%) and catalytically activated at 950 °C for 3 h in an argon atmosphere containing 4.9% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 2800℃ for 30h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0060] Comparative Example 4 This comparative example provides a method for preparing a negative electrode active material, including the following steps: (1) Petroleum coke (98wt%) and ZIF-8 derived zinc oxide nitrogen-carbon catalyst (2wt%) were mixed and mechanically ground to D50=11μm. Under nitrogen protection, the mixture was heated to 950℃ at 5℃ / min and held for 4h for pre-carbonization; (2) The pre-carbonized product was uniformly mixed with urea (30.1 wt%) and catalytically activated at 950 °C for 3 h in an argon atmosphere containing 15.1% water vapor to form a carbon precursor with multi-level pores. (3) The carbon precursor with multi-level channels is loaded into a graphitization furnace, then treated at 2800℃ for 30h, and finally the negative electrode active material is obtained after demagnetization and sieving.

[0061] Comparative Example 5 Compared with Example 1, Comparative Example 5 has the same pore ratio (60% micropores, 25% mesopores, and 15% macropores), but the pore connectivity is poor. The preparation steps of Comparative Example 5 are as follows: the negative electrode active material was prepared according to the method of patent CN120423538B.

[0062] Comparative Example 6 Commercial graphite was used, specifically the FSN-1 model from Shanghai Shanshan Technology Co., Ltd.

[0063] Performance testing The negative electrode active materials in Examples 1-4 and Comparative Examples 1-6 were subjected to the following tests: (1) Particle size test, the specific steps are as follows: the Malvern 3000 particle size analyzer is used for testing; (2) The test method for the porosity, micropores, mesopores and macropores is as follows: the nitrogen adsorption method (micropores, mesopores) and mercury porosimeter (macropores) are used to test the total pores. (3) Grain size testing method, the specific steps are as follows: XRD peaks are measured using a Bruker XRD diffractometer, then the C peak in the XRD is fitted using Jade software, and the grain size is calculated from the diffraction peak width using the Scherrer formula. The results are shown in Table 1.

[0064] Table 1. Test results of physical property parameters of negative electrode active materials in the examples and comparative examples.

[0065] Electrochemical performance testing The performance of the artificial graphite anode active materials prepared in the examples and comparative examples was tested using a coin cell half-cell test method. The artificial graphite anode active material was prepared by mixing PVDF (polyvinylidene fluoride) in a ratio of 96:4 (wt%) with NMP (N-methylpyrrolidone) to form a slurry, which was then coated onto copper foil. The coated electrode was then vacuum dried in a vacuum drying oven at 100℃ for 8 hours. The electrolyte was 1 mol / L LiPF6+EC:DEC:DMC = 1:1:1 (volume ratio). A lithium metal sheet was used as the counter electrode, and a polypropylene microporous membrane was used as the separator. The battery was assembled. The charge / discharge voltage range was 0.005V to 2.0V, and the charge / discharge rate was 0.1C. The test results are shown in Table 2.

[0066] Table 2 Performance test results of artificial graphite anode active materials in Examples 1-4 and Comparative Example 1

[0067] As shown in Tables 1 and 2, compared with the comparative examples, the negative electrode active materials of Examples 1 to 4 exhibited higher specific capacity, excellent rate performance, and good cycle stability when the ratio of micropores, mesopores, and macropores was within the above-mentioned range and the channels were interconnected. This indicates that within this ratio range, an effective multi-level interconnected transport network was formed between micropores, mesopores, and macropores. Micropores provided sufficient lithium storage active sites, mesopores constructed low-resistance ion transport bridges, and macropores ensured rapid electrolyte wetting and volume expansion buffering. The synergistic effect of these three elements enabled the material to achieve a good balance between high specific capacity and high rate performance.

[0068] In contrast, the catalyst dosage in Comparative Example 1 was too low, resulting in excessively low porosity of the negative electrode active material and a micropore ratio below the lower limit of the range. Although there were sufficient lithium storage sites, the ion transport channels were narrow and insufficient in number, severely hindering ion diffusion at high rates and causing a significant decrease in rate performance.

[0069] In Comparative Example 2, the excessive amount of catalyst resulted in an excessively low porosity of the negative electrode active material, with the proportion of micropores exceeding the upper limit. This led to insufficient overall density of the porous graphite material, damage to the electronic conductivity network, a significant reduction in volumetric energy density, and decreased stability of the framework structure during cycling, resulting in a shortened cycle life.

[0070] In Comparative Example 3, the amount of pore-forming agent was too low, resulting in excessively high porosity of the negative electrode active material, severe compression of mesopores, narrow and insufficient ion transport channels, severe obstruction of ion diffusion at high rates, and a significant decrease in rate performance.

[0071] In Comparative Example 4, the amount of pore-forming agent was too high, resulting in excessively low porosity of the negative electrode active material. The proportion of mesopores and macropores exceeded the upper limit of the range, the overall density of the porous graphite material was insufficient, the electronic conductivity network was damaged, the volumetric energy density was significantly reduced, and the stability of the skeleton structure deteriorated during cycling, shortening the cycle life.

[0072] Although the proportion of channels in Comparative Example 5 is the same as that in Example 1, its rate performance is significantly lower than that in Example 1 due to the structural differences between the two, which fully demonstrates that connectivity is a necessary prerequisite for realizing the synergistic effect of multi-level channels. Based on the above results, it can be concluded that the interconnection and synergistic cooperation of micropores, mesopores, and macropores within a specific ratio range are key to achieving high specific capacity, high rate performance, and long cycle life in anode active materials. A reasonable ratio without connectivity, or connectivity with an unbalanced ratio, cannot achieve the optimal comprehensive performance brought about by the synergy of these three elements. The embodiments of this invention significantly outperform the comparative examples in specific capacity, first-efficiency performance, volume stability, cycle life, and rate performance, demonstrating comprehensive performance advantages. In particular, the volume expansion rate of Example 1 is only 10%, far lower than the 17% of Comparative Example 5 and the 20% of Comparative Example 6. Furthermore, under 3C high-current charging conditions, the capacity retention rate of Example 1 is as high as 92.5%, far exceeding the 82.7% of Comparative Example 5 and the 82.2% of Comparative Example 6, fully demonstrating the mitigating effect of the multi-level pore structure and the proportion of pores on volume expansion and the promoting effect on ion transport.

[0073] The above are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the patent protection scope of the present invention.

Claims

1. A negative electrode active material, characterized in that, The negative electrode active material includes a porous graphite material with a porosity of 15% to 30%. The surface of the porous graphite material has micropores, and mesopores and macropores are sequentially arranged in the direction close to the interior of the porous graphite. At least some of the mesopores are in communication with the micropores, and at least some of the macropores are in communication with the mesopores.

2. The negative electrode active material as described in claim 1, characterized in that, The pore size of the micropores is <2 nm, and the number of micropores accounts for 50%-70% of the total number of pores in the porous graphite material; and / or, The mesopores have a pore size of 2-50 nm, and their number accounts for 25%-45% of the total number of pores in the porous graphite material; and / or, The pore size of the macropores is ≥50nm, and the number of macropores accounts for 5%-15% of the total number of pores in the porous graphite material.

3. The negative electrode active material as described in claim 1, characterized in that, The porous graphite material has a grain size La(110) of 80-140 nm and an Lc(002) of 35-45 nm; and / or, The particle size of the negative electrode active material is 8~15μm.

4. The negative electrode active material as described in claim 1, characterized in that, The porous graphite material is made of carbon materials, and the carbon materials include at least one of graphite and amorphous carbon.

5. A method for preparing a negative electrode active material as described in any one of claims 1 to 4, characterized in that, The preparation method of the negative electrode active material includes the following steps: The carbon source and MOF-derived catalyst are mixed and pulverized to obtain a mixture. The mixture is then pre-carbonized under an inert atmosphere to obtain a pre-carbonized product. The pre-carbonized product is mixed with a pore-forming agent and catalytically activated in a water vapor atmosphere to form a carbon precursor with multi-level pores. The carbon precursor with the multi-level channels is graphitized, demagnetized, and sieved to obtain the negative electrode active material.

6. The method for preparing the negative electrode active material as described in claim 5, characterized in that, The MOF-derived catalyst accounts for 0.5-5% of the mass of the carbon source; and / or, The average particle size D50 of the mixture is 8-15 μm; and / or, The carbon source includes at least one selected from pitch coke, petroleum coke, needle coke, shot coke, metallurgical coke, and anthracite; and / or, The MOF-derived catalysts include ZIF-67-derived cobalt-nitrogen-carbon catalysts or ZIF-8-derived zinc oxide-nitrogen-carbon catalysts.

7. The method for preparing the negative electrode active material as described in claim 5, characterized in that, The pre-carbonization process includes: heating the mixture in an inert gas atmosphere at a rate of 10-50℃ / min until the temperature reaches 800-1000℃, holding the temperature for 2-4 hours, and then cooling it to 100-200℃ to obtain the pre-carbonized product.

8. The method for preparing the negative electrode active material as described in claim 5, characterized in that, The pore-forming agent accounts for 10-30% of the mass of the pre-carbonized product; and / or, The pore-forming agent includes organic or inorganic pore-forming agents; and / or, The pore-forming agent includes at least one of ammonium bicarbonate, ammonium chloride, and urea; and / or, In the catalytic activation step, catalytic activation is carried out under conditions of 5-15% water vapor concentration, wherein the catalytic activation temperature is 850-950℃ and the catalytic activation time is 1-3h.

9. The method for preparing the negative electrode active material as described in claim 5, characterized in that, The graphitization treatment temperature is 2400-3200℃, and the graphitization treatment time is 24-48h.

10. An electrode assembly, characterized in that, The negative electrode active material includes the negative electrode active material as described in any one of claims 1 to 4 or the negative electrode active material prepared by any one of claims 5 to 9.

11. A secondary battery, characterized in that, The secondary battery includes the electrode assembly as described in claim 10.

12. An electrical appliance, characterized in that, The electrical device includes the secondary battery as described in claim 11.

Citation Information

Patent Citations

  • A method for preparing low-expansion and high-capacity artificial graphite

    CN120423538B