An in-situ polymerized cyclic ether gel electrolyte, a high-voltage alkali metal battery, and its applications.
By using the in-situ ring-opening polymerization of 1,3,5-trioxepane cyclic ether monomer in lithium metal batteries, the safety and conductivity issues of traditional electrolytes have been solved, achieving high oxidation stability and simplified processes, thereby improving the energy density and cycle performance of lithium metal batteries.
Patent Information
- Application Number
- CN202611216863.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-12
- Publication Date
- 2026-11-10
AI Technical Summary
Traditional organic liquid electrolytes for existing lithium metal batteries are highly volatile, flammable, and pose safety hazards, while solid polymer electrolytes have low conductivity, high interfacial impedance, and a narrow electrochemical stability window. Furthermore, existing modification strategies are complex and unsuitable for high-voltage cathode materials, which hinders the commercial application of lithium metal batteries.
Using 1,3,5-trioxepane as a cyclic ether monomer, a gel network is formed in situ within the battery through a ring-opening polymerization reaction initiated by Lewis acids, avoiding the need for additional initiators, achieving high oxidation stability and simplifying the process.
It improves the conductivity and oxidation stability of lithium metal batteries, simplifies the preparation process, is suitable for high-voltage cathode materials, and enhances the energy density and cycle stability of batteries.
Smart Images

Figure CN123073159A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal / metal ion batteries, specifically relating to an in-situ polymerized cyclic ether gel electrolyte, a high-voltage alkali metal battery, and their applications. Background Technology
[0002] The energy density of current lithium-ion batteries is gradually reaching a bottleneck, making it difficult to meet the growing energy density demands of portable electronics and electric vehicles. Lithium metal batteries, using lithium as the negative electrode, have become the alternative electrochemical device for next-generation high-energy-density battery systems. Traditional organic liquid electrolytes pose serious safety hazards when combined with high-voltage cathodes due to their high volatility, flammability, and leakage tendency, limiting the large-scale commercial application of lithium metal batteries. In recent years, researchers have discovered that solid polymer electrolytes can significantly improve the safety of lithium metal batteries; however, these electrolytes also suffer from drawbacks such as low conductivity, high interfacial impedance, and a narrow electrochemical stability window.
[0003] In-situ polymerization is a simple method for preparing polymer electrolytes that is highly compatible with existing battery manufacturing processes. This technology involves injecting a precursor solution containing monomers, lithium salts, and optionally an initiator into the battery, allowing it to fully wet the electrodes, and then initiating a polymerization reaction inside the battery to form the polymer electrolyte in situ. This significantly improves the conductivity of the polymer electrolyte, and in-situ polymerization offers advantages such as ease of operation and scale-up, facilitating the commercial production of lithium metal batteries.
[0004] Currently, 1,3-dioxolane (DOL) is one of the most commonly used in-situ polymerized cyclic ether monomers. However, DOL-based gel electrolytes have significant performance bottlenecks: First, they exhibit poor oxidative stability, with a voltage window typically around 4.0V, making them difficult to match with high-voltage cathode materials (such as NCM811), and they are prone to oxidative decomposition under high voltage. Second, the linear segment structure of DOL is highly regular, easily forming crystalline regions, which limits further improvement in room-temperature ionic conductivity. Third, unreacted monomers remaining after polymerization are also easily oxidized and decomposed under high voltage, further deteriorating cycle performance.
[0005] To improve the high-pressure resistance of ether gel electrolytes, researchers have tried various modification strategies. Chinese patent application CN121097192A proposes to overcome the performance bottleneck of traditional linear polyether electrolytes by copolymerizing 1,3,5-trioxane with DOL, 1,4-dioxane, or tetrahydrofuran. However, this approach has the following shortcomings: (1) a copolymerization system of two cyclic ether monomers must be used, preferably a 1:1 mass ratio of mixed monomers; (2) 10% to 30% of ether additives (such as ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, etc.) must be added as plasticizers / cosolvents; (3) polymerization must be carried out under heating conditions of 60°C to 80°C. It can be seen that this approach improves performance through a complex strategy of copolymerization + additives + heating, resulting in a complex system composition and demanding process conditions.
[0006] Currently, most gel polymer electrolytes require the introduction of additional initiators to achieve in-situ polymerization in the battery. These initiators, difficult to remove after polymerization, further deteriorate during cycling, significantly jeopardizing the cycle stability of lithium metal batteries. Simultaneously, most ether polymer electrolytes are difficult to match with high-voltage cathode materials, easily undergoing oxidative decomposition under high pressure, leading to a sharp decline in battery performance.
[0007] Therefore, it is evident that developing a novel cyclic ether monomer that combines good polymerization activity and high oxidation stability, enabling it to be polymerized directly from lithium salts without the need for an external initiator, while possessing sufficiently high oxidation stability to match high-voltage cathodes, is crucial to meeting the comprehensive performance requirements of electrolyte materials for high-energy-density lithium metal batteries. Summary of the Invention
[0008] To address the shortcomings of existing technologies, this invention provides an in-situ polymerized cyclic ether gel electrolyte, a high-voltage alkali metal battery, and their applications. The gel polymer electrolyte designed in this invention consists of a lithium salt and a seven-membered ring-shaped ether monomer, which are polymerized in-situ within the battery via a Lewis acid-initiated ring-opening polymerization reaction to form a gel network. This invention leverages the mild, simple, and efficient conditions of the in-situ ring-opening polymerization reaction, along with the advantage of lithium salt-initiated in-situ polymerization without side reactions, to successfully achieve the in-situ preparation of the polymer gel electrolyte, which holds promise for widespread application in the field of alkali metal / ion batteries.
[0009] To achieve the above objectives, the present invention adopts the following technical solution:
[0010] A first aspect of the present invention is to provide an in-situ polymerized cyclic ether gel electrolyte, wherein the gel electrolyte is prepared by an in-situ ring-opening polymerization reaction of a precursor solution;
[0011] The precursor solution contains a cyclic ether monomer and an alkali metal salt;
[0012] The cyclic ether monomer is 1,3,5-trioxepane (hereinafter referred to as TOP). The preparation principle of TOP molecules is as follows:
[0013] .
[0014] The alkali metal salt acts as an initiator to initiate the ring-opening polymerization of 1,3,5-trioxepane, and the precursor solution does not contain any additional polymerization initiator.
[0015] Furthermore, the alkali metal salt is selected from one or more of MFSI, MTFSI, MOTf, MBF4, MClO4, MBOB, MTFA, MClO4, MPF6, or MDFOB, where M represents Li, Na, or K. It can be selected from LiFSI, LiTFSI, LiPF6, LiOTf, LiBF4, LiClO4, LiBOB, LiDFOB, or NaFSI, NaTFSI, NaPF6, NaOTf, NaBF4, NaClO4, NaBOB, NaDFOB, or KFSI, KTFSI, KPF6, KOTf, KBF4, KClO4, KBOB, KDFOB. These are all commonly used reagents in battery electrolytes and can be obtained through commercial purchases.
[0016] The polymerization mechanism is: M + As a Lewis acid, it coordinates with the oxygen atom on the TOP ring, polarizes the CO bond, activates the ring, and then performs ring-opening polymerization without the need for additional initiators.
[0017] Furthermore, the concentration of the alkali metal salt in the precursor solution is 0.1-10 mol / L.
[0018] Furthermore, the 1,3,5-trioxepane in the precursor solution has a mass percentage content of 34% to 95%.
[0019] Furthermore, the in-situ ring-opening polymerization reaction is carried out by standing at room temperature for 12-72 hours.
[0020] A second aspect of the present invention is to provide a high-voltage alkali metal battery, comprising a positive electrode, a negative electrode, a separator, and the aforementioned in-situ polymerized gel electrolyte.
[0021] Furthermore, the active material of the positive electrode is selected from one or more of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium-rich manganese-based materials, lithium nickel manganese oxide, nickel cobalt manganese ternary materials, sodium / potassium ion layered oxides, sodium / potassium ion polyanionic compounds, sodium / potassium Prussian blue compounds, or sodium / potassium organic materials.
[0022] The active material of the negative electrode is selected from one or more of lithium, sodium, potassium, and carbon-based alloy materials;
[0023] The diaphragm is one of glass fiber diaphragm, cellulose diaphragm or porous polyolefin diaphragm.
[0024] Furthermore, the alkali metal battery is a lithium metal battery, the active material of the positive electrode is a nickel-cobalt-manganese ternary material or lithium iron phosphate, and the negative electrode is lithium metal.
[0025] Further, under an inert atmosphere, an alkali metal salt was added to 1,3,5-trioxepane and stirred until homogeneous to obtain a precursor solution;
[0026] The precursor solution is injected into a battery casing containing a positive electrode, a negative electrode, and a separator, and then undergoes an in-situ ring-opening polymerization reaction to form the in-situ polymerized gel electrolyte inside the battery.
[0027] A third aspect of the present invention is to provide the application of the aforementioned high-voltage alkali metal battery in new energy vehicles, large-scale energy storage, or electronic products.
[0028] Advantages and beneficial effects of the present invention:
[0029] 1. This invention provides a seven-membered ring ether monomer, which is used as a precursor for in-situ polymerization and has a low HOMO energy level and excellent oxidative stability.
[0030] 2. The monomers of this invention can be directly polymerized by alkali metal salts without the need for additional initiators, effectively avoiding the adverse effects of residual initiators on battery performance and simplifying the preparation process. Furthermore, the in-situ polymerization method results in a simple manufacturing process with high controllability, facilitating large-scale production.
[0031] 3. This invention characterizes and further optimizes the concentration and ratio of alkali metal salts and cyclic ether compounds used in high-voltage electrolytes for alkali metal / alkali metal ion batteries, enabling them to work with high-voltage cathodes (such as LiNi). 0.8 Co 0.1 Mn 0.1 O2) matching enables the battery to have a higher overall energy density, making it more suitable for practical applications. Attached Figure Description
[0032] Figure 1 The 1H NMR spectrum of the TOP monomer of this invention ( 1 H NMR, CDCl3);
[0033] Figure 2 The image shows the carbon NMR spectrum of the TOP monomer of this invention. 13 C NMR, CDCl3);
[0034] Figure 3The 1H NMR spectrum of 0.5 M-PTOP in this invention ( 1 H NMR, CDCl3);
[0035] Figure 4 The 1.0 M-PTOP NMR spectrum of this invention ( 1 H NMR, CDCl3);
[0036] Figure 5 The 1.5 M-PTOP NMR spectrum of this invention ( 1 H NMR, CDCl3);
[0037] Figure 6 The 1H NMR spectrum of the LiDFOB-PTOP of this invention is shown below. 1 H NMR, CDCl3);
[0038] Figure 7 The 1H NMR spectrum of the LiTFSI-PTOP of this invention is shown below. 1 H NMR, CDCl3);
[0039] Figure 8 The nuclear magnetic resonance hydrogen spectrum of Comparative Example 2 of this invention ( 1 H NMR, DMSO)
[0040] Figure 9 The charge-discharge curves of the Li||LiNCM811 coin cells of polymerization Example 2 and Comparative Example 1 of the present invention are shown.
[0041] Figure 10 The performance curves of the gel polymer electrolyte Li||NCM811 battery of the present invention are shown.
[0042] Figure 11 The performance curves of the gel polymer electrolyte Li||LFP battery of the present invention are shown. Detailed Implementation
[0043] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0044] Unless otherwise specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0045] The components used in the following examples and comparative examples are all battery grade.
[0046] Synthesis Example 1:
[0047] TOP monomer was synthesized as follows: 30 g of paraformaldehyde (1 mol), 148 g of 1,3-dioxolane (DOL, 2 mol), and 10.5 g of polyphosphoric acid (0.06 mol) were added to a three-necked flask. The mixture was heated under reflux at 70 °C in an oil bath for 3 hours. At the end of the reaction, the mixture was cooled to room temperature and filtered. Subsequently, depolymerization was carried out under vacuum at 150 °C to obtain a mixture of DOL and TOP. The resulting mixture was then distilled under reduced pressure, and the product collected under vacuum at 40 °C was the TOP monomer.
[0048] Figure 1 The image shows the 1H NMR spectrum of the TOP monomer synthesized in Example 1 dissolved in deuterated chloroform (CDCl3). Figure 1 The peak positions correspond to the target product, indicating high purity. Figure 2 The corresponding carbon NMR spectrum is shown below.
[0049] Aggregation Example 1:
[0050] In an argon-atmospheric glove box, 18.7 mg of lithium bisfluorosulfonylimide (LiFSI) was dissolved in 200 μL of TOP monomer (0.5 M concentration) and stirred until completely clear to obtain the precursor solution. The battery was assembled in the order of negative electrode, precursor solution, separator, precursor solution, and positive electrode. After encapsulation, it was allowed to stand at room temperature for 72 hours to obtain the PTOP gel polymer electrolyte.
[0051] Figure 3 The TOP monomer and the PTOP polymer obtained in Example 1 1 H NMR spectrum. From Figure 3 It can be seen that the characteristic peaks at 4.90 ppm and 3.80 ppm attributable to the monomer weakened after polymerization, while new broad peaks appeared at 4.82 ppm and 3.73 ppm, indicating that alkali metal ions have initiated the ring-opening polymerization of TOP.
[0052] Aggregation Example 2:
[0053] The difference compared to polymerization example 1 is that the concentration of LiFSI is 1 M (37.4 mg LiFSI dissolved in 200 μL TOP). The remaining steps are the same as in polymerization example 1.
[0054] Aggregation Example 3:
[0055] The difference compared to polymerization example 1 is that the concentration of LiFSI is 1.5 M (56.1 mg LiFSI dissolved in 200 μL TOP). The remaining steps are the same as in polymerization example 1.
[0056] Aggregation Example 4:
[0057] Compared to polymerization example 1, the difference is that LiDFOB and LiTFSI were used instead of LiFSI, respectively, at a concentration of 1.0 M. The remaining steps are the same as in polymerization example 1. Figure 6 and Figure 7 LiDFOB and LiTFSI respectively triggered TOP aggregation 1 The HNMR spectrum and NMR results show that TOP can undergo polymerization in the presence of the aforementioned lithium salts, demonstrating that the polymerization of TOP initiated by alkali metal salts has good versatility.
[0058] Comparative Example 1:
[0059] In an argon-atmospheric glove box, 37.4 mg of lithium bisfluorosulfonylimide (LiFSI) was dissolved in 200 μL of DOL monomer (concentration 1.0 M), and 20 mM Mg(TFSI)2 was added as an initiator. The mixture was stirred until completely dissolved to obtain a precursor solution. The precursor solution was injected into the assembled battery and allowed to stand at room temperature for 12 hours to obtain the PDOL gel polymer electrolyte.
[0060] Comparative Example 2:
[0061] The polymerization was carried out under the same conditions as in Polymerization Example 1, except that the monomer described in this invention was replaced with 1,3,5-trioxane (TXE). After the reaction, the polymerization reaction was carried out by... 1 The product was characterized by 1H NMR. Nuclear magnetic resonance spectrum (NMR spectrum) Figure 8 The results showed that only the characteristic peaks of the raw material monomers (δ [5.1] ppm) were detected in the product, and no broad peak signals of polymer segments were observed, indicating that the compound TXE did not undergo polymerization under these conditions.
[0062] To investigate the electrolyte performance of polymerization Example 2 and Comparative Example 1, they were used to prepare the same type of battery. The electrolytes in Example 2 and Comparative Example 1 contained Li||LiNi. 0.8 Co 0.1 Mn 0.1 The specific methods for fabricating and testing O2, Li||LiFePO4 button cells are as follows:
[0063] NCM811 Positive Electrode: 80 wt% of nickel-cobalt-manganese ternary (NCM811) active material powder, 10 wt% of acetylene black conductive agent, and 10 wt% of polyvinylidene fluoride binder are mixed evenly. Then, an appropriate amount of N-methylpyrrolidone is added to the mixed powder, and the mixture is homogenized for 1 hour to obtain the electrode slurry. The slurry is then evenly coated onto aluminum foil using a scraper, vacuum dried for 12 hours, and cut into 10 mm round pieces to obtain the NCM811 positive electrode.
[0064] LFP Positive Electrode: 80 wt% lithium iron phosphate (LFP) active material powder, 10 wt% acetylene black conductive agent, and 10 wt% polyvinylidene fluoride binder are mixed evenly. Then, an appropriate amount of N-methylpyrrolidone is added to the mixed powder, and the mixture is homogenized for 1 hour to obtain the electrode slurry. The slurry is then evenly coated onto aluminum foil using a scraper, vacuum dried for 12 hours, and cut into 10 mm round pieces to obtain the lithium iron phosphate positive electrode.
[0065] Li negative electrode: A 14 mm diameter lithium metal sheet is used.
[0066] Cu foil: 16 mm in diameter and approximately 8 μm thick smooth copper foil.
[0067] Diaphragm: Cut a glass fiber diaphragm disc with a diameter of 19 mm.
[0068] Al foil: 19 mm diameter Al foil is used.
[0069] Electrolytes: The electrolytes prepared in Polymerization Example 2 and Comparative Example 1 were used, respectively.
[0070] Battery assembly: In an argon atmosphere glove box (O2<0.01 ppm, H2O<0.01 ppm), coin cells were assembled in the following order: “aluminum-plated positive electrode shell-Al foil-positive electrode disc-separator disc-negative electrode disc-stainless steel disc-spring sheet-negative electrode shell”. Electrolytes prepared in polymerization example 2 and comparative example 1 were added respectively, and finally the cells were encapsulated to obtain test cells.
[0071] Battery Testing: Nickel-cobalt-manganese ternary cathode lithium (NCM811) (Li) batteries assembled in situ from the gel polymer electrolytes of Example 2 and Comparative Example 1 were subjected to room temperature cycle testing. A Blue Electric test system was used, with charge-discharge tests conducted at a current density of 1 C (1 C corresponds to a specific capacity of 210 mAh / g) within a voltage range of 2.8–4.3 V. Figure 9 As shown, the gel polymer electrolyte in Comparative Example 1 could not release its capacity normally, while the gel polymer electrolyte in Polymerization Example 2 could release a specific capacity of 198.8 mAh / g. Figure 10As shown, the electrolyte prepared in Polymer Example 2 exhibits a capacity retention rate of over 87% and an average coulombic efficiency of 99.59% (3-100 cycles) when assembled into a battery after 100 cycles, indicating that the electrolyte prepared in this invention has excellent cycling performance.
[0072] The lithium iron phosphate (LFP) battery assembled in situ with the gel polymer electrolyte in Example 2 was subjected to room temperature cycling tests. A blue electric current testing system was used, and charge-discharge tests were conducted at a current density of 1 C (1 C corresponds to a specific capacity of 170 mAh / g) within a voltage range of 2.5–3.8 V. Figure 11 As shown, the electrolyte prepared in Example 2 exhibits a capacity retention rate of over 99% after 350 cycles and an average coulombic efficiency of 99.90% (3-350 cycles), indicating that the electrolyte prepared in this invention has excellent cycling performance.
[0073] In summary, the above embodiments are only for illustrating the relevant principles and implementation methods, and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made to the present invention without departing from the principles of the present invention should be included within the protection scope of the present invention.
Claims
1. An in-situ polymerized cyclic ether gel electrolyte, characterized in that, The gel electrolyte is prepared by in-situ ring-opening polymerization of a precursor solution. The precursor solution contains a cyclic ether monomer and an alkali metal salt; The cyclic ether monomer is 1,3,5-trioxepane; The alkali metal salt acts as an initiator to initiate the ring-opening polymerization of 1,3,5-trioxepane, and the precursor solution does not contain any additional polymerization initiator.
2. The in-situ polymerized cyclic ether gel electrolyte according to claim 1, characterized in that, The alkali metal salt is selected from one or more of MFSI, MTFSI, MOTf, MBF4, MClO4, MBOB, MTFA, MClO4, MPF6, or MDFOB, where M represents Li, Na, or K.
3. The in-situ polymerized cyclic ether gel electrolyte according to claim 1, characterized in that, The concentration of the alkali metal salt in the precursor solution is 0.1-10 mol / L.
4. The in-situ polymerized cyclic ether gel electrolyte according to claim 1, characterized in that, The mass percentage of 1,3,5-trioxepane in the precursor solution is 34% to 95%.
5. The in-situ polymerized cyclic ether gel electrolyte according to claim 1, characterized in that, The in-situ ring-opening polymerization reaction is carried out at room temperature for 12-72 hours.
6. A high-voltage alkali metal battery, characterized in that, It includes a positive electrode, a negative electrode, a separator, and the in-situ polymerized gel electrolyte as described in any one of claims 1 to 5.
7. The high-voltage alkali metal battery according to claim 6, characterized in that, The active material of the positive electrode is selected from one or more of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium-rich manganese-based materials, lithium nickel manganese oxide, nickel cobalt manganese ternary materials, sodium / potassium ion layered oxides, sodium / potassium ion polyanionic compounds, sodium / potassium Prussian blue compounds, or sodium / potassium organic materials. The active material of the negative electrode is selected from one or more of lithium, sodium, potassium, and carbon-based alloy materials; The diaphragm is one of glass fiber diaphragm, cellulose diaphragm or porous polyolefin diaphragm.
8. The high-voltage alkali metal battery according to claim 7, characterized in that, The alkali metal battery is a lithium metal battery, the active material of the positive electrode is a nickel-cobalt-manganese ternary material or lithium iron phosphate, and the negative electrode is lithium metal.
9. The high-voltage alkali metal battery according to claim 7, characterized in that, Under an inert atmosphere, an alkali metal salt was added to 1,3,5-trioxepane and stirred until homogeneous to obtain a precursor solution. The precursor solution is injected into a battery casing containing a positive electrode, a negative electrode, and a separator, and then undergoes an in-situ ring-opening polymerization reaction to form the in-situ polymerized gel electrolyte inside the battery.
10. The application of the high-voltage alkali metal battery according to any one of claims 7 to 9 in new energy vehicles, large-scale energy storage or electronic products.
Citation Information
Patent Citations
Preparation method and application of wide-temperature-range lithium battery gel electrolyte
CN121097192A