Winded electrode body and secondary battery
By setting electrode films of different densities on different main surfaces of the current collector, the problem of easy cracking of electrode films in traditional vortex-wound electrode bodies is solved, thereby improving the reliability and lifespan of the battery.
Patent Information
- Application Number
- CN202610598949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-30
- Publication Date
- 2026-11-10
AI Technical Summary
In traditional vortex-wound electrode bodies, the electrode film has a greater degree of curvature on the innermost circumference, which leads to stress concentration, making it prone to cracks and affecting battery performance.
By setting electrode films with different densities on different main surfaces of the current collector, specifically with the inner main surface having a lower density than the outer main surface, stress concentration on the inner side is reduced, the flexibility of the electrode body is enhanced, thereby reducing cracks in the electrode film.
It effectively reduces cracks in the electrode film, improves battery reliability and lifespan, and enhances the durability of the electrode body.
Smart Images

Figure CN123073205A_ABST
Abstract
Description
Technical Field
[0001] This disclosure relates to wound electrode bodies and secondary batteries. Background Technology
[0002] As a conventional vortex-wound electrode, Japanese Patent Application Publication No. 11-144762 discloses an electrode in which active material layers are provided on both sides of a current collector. In this electrode, one side of the current collector is a rough surface, and the other side of the current collector is a smooth surface that is smoother than the rough surface, and the roughness difference between the rough surface and the smooth surface is 1.5 or more. Summary of the Invention
[0003] As the electrodes constituting the wound electrode body, electrodes with an electrode film attached to the current collector can be used. In the wound electrode body, by winding in a manner that reduces the radius of curvature at the innermost circumference, the capacity of the secondary battery can be increased. However, in this case, the curvature of the innermost electrode body is greater than that of the outermost electrode body, increasing the stress applied to the electrode film disposed on the current collector. Therefore, without any countermeasures, there is a concern that the electrode film may crack.
[0004] This disclosure was made in view of the above-mentioned problems, and the purpose of this disclosure is to provide a wound electrode body capable of reducing cracks in the electrode film, and a secondary battery having the wound electrode body.
[0005] The wound electrode body according to this disclosure includes: a current collector having a first main surface located at one end in the thickness direction and a second main surface located at the other end in the thickness direction; a first electrode film disposed on the first main surface; and a second electrode film disposed on the second main surface. The current collector is wound with the first main surface facing inward and the second main surface facing outward. The density of the first electrode film is lower than the density of the second electrode film.
[0006] In the wound electrode body, the stress on the first main surface facing inward is greater than the stress on the second main surface facing outward. As described above, by making the density of the first electrode film on the first main surface, which has a greater stress than the second main surface, lower than the density of the second electrode film on the second main surface, flexibility can be imparted to the wound electrode body. This reduces the likelihood of cracks in the electrode film.
[0007] The secondary battery based on this disclosure includes the aforementioned wound electrode body and a housing housing that accommodates the aforementioned wound electrode body.
[0008] Based on the above configuration, a secondary battery with a wound electrode body that can reduce cracking of the electrode film can be obtained.
[0009] The above and other objects, features, aspects and advantages of the present invention will become apparent from the following detailed description of the invention, which will be understood in conjunction with the accompanying drawings. Attached Figure Description
[0010] Figure 1 This is a simplified cross-sectional view of the secondary battery involved in the implementation method.
[0011] Figure 2 This is a simplified top view of the positive electrode plate of the wound electrode body according to the embodiment after it has been unfolded.
[0012] Figure 3 This is a simplified cross-sectional view of the positive electrode plate of the wound electrode body according to the embodiment.
[0013] Figure 4 This is a simplified top view of the negative electrode plate of the wound electrode body according to the embodiment after it has been unfolded.
[0014] Figure 5 This is a simplified cross-sectional view of the negative electrode plate of the wound electrode body according to the embodiment. Detailed Implementation
[0015] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. It should be noted that in the following embodiments, the same reference numerals are used to label the same or common parts in the drawings, and their descriptions are omitted.
[0016] (Secondary battery)
[0017] Figure 1 This is a simplified cross-sectional view of the secondary battery involved in the embodiment. (Refer to...) Figure 1 This describes the secondary battery 100 involved in the implementation method.
[0018] The secondary battery 100 is, for example, a lithium-ion battery installed in a vehicle. It should be noted that the uses and types of the secondary battery 100 are not limited to those illustrated above. The secondary battery 100 can be a battery that uses electrolyte or a battery that does not use electrolyte.
[0019] According to one embodiment of the present disclosure, the secondary battery 100 includes a wound electrode body 1, a housing 2, a positive terminal 3, a positive current collector 4, an outer gasket 5, an inner gasket 6, and a negative current collector 7.
[0020] The electrode body 1 is wound into a spiral shape. The wound electrode body 1 is housed in the housing 2. The housing 2 has a cylindrical shape. That is, the secondary battery 100 is a cylindrical battery.
[0021] The wound electrode body 1 includes a positive electrode plate 10, a negative electrode plate 20, and a separator 30. The positive electrode plate 10 and the negative electrode plate 20 are, for example, dried electrode films. The separator 30 is disposed radially R between the positive electrode plate 10 and the negative electrode plate 20 of the wound electrode body 1. The separator 30 separates the positive electrode plate 10 and the negative electrode plate 20. Furthermore, the separator 30 is configured to allow ions (e.g., lithium ions) to move back and forth between the positive electrode plate 10 (more precisely, the positive electrode active material) and the negative electrode plate 20 (more precisely, the negative electrode active material). The wound electrode body 1 is composed of an electrode assembly formed by winding the positive electrode plate 10 and the negative electrode plate 20 with the separator 30 in between.
[0022] The housing 2 has an upper surface 2a, a lower surface 2b, and a side surface 2c. The upper surface 2a is the side of the housing 2 located axially in the cylindrical shape. Viewed from the perspective of the wound electrode body 1, the upper surface 2a is located on one side Z1 along the axial direction Z of the wound electrode body 1. The lower surface 2b is the other side Z2 of the housing 2 located axially in the cylindrical shape. Viewed from the perspective of the wound electrode body 1, the lower surface 2b is located on the other side along the axial direction Z of the wound electrode body 1. The side surface 2c has a cylindrical shape. The side surface 2c connects the upper surface 2a and the lower surface 2b. The housing 2 is formed of copper or aluminum, etc.
[0023] It should be noted that the casing 2 also contains electrolyte (not shown). On the other hand, in the case where the wound electrode body 1 is an all-solid-state battery, the electrolyte can be omitted.
[0024] The height dimension (dimension along the Z-axis) of the housing 2 is, for example, 50 mm or more, 60 mm or more, 70 mm or more, or 80 mm or more. The larger the height dimension (dimension along the Z-axis) of the housing 2, the larger the battery capacity of the secondary battery 100. Conversely, the height dimension (dimension along the Z-axis) of the housing 2 is, for example, 150 mm or less, 100 mm or less, or 80 mm or less. The smaller the height dimension (height dimension) along the Z-axis of the housing 2, the lower the height of the module housing the secondary battery 100 can be.
[0025] The diameter (radial dimension R) of the housing 2 is, for example, 15mm or more, 20mm or more, 25mm or more, 30mm or more, 40mm or more, 45mm or more, or 46mm or more. The larger the diameter (maximum radial dimension R) of the housing 2, the larger the battery capacity of the secondary battery 100. The diameter (radial dimension R) of the housing 2 is, for example, less than 100mm, less than 75mm, less than 50mm, or less than 46mm. The smaller the diameter (radial dimension R) of the housing 2, the more compactly the secondary battery 100 can be arranged within the module.
[0026] The positive terminal 3 is located on one side Z1 in the axial direction Z relative to the wound electrode body 1. The positive terminal 3 includes a disc portion 3a and a riveting portion 3b. The riveting portion 3b is connected to the disc portion 3a. The riveting portion 3b is configured to extend from the center of the disc portion 3a toward the other side Z2 in the axial direction Z. It should be noted that the positive terminal 3 is made of aluminum. The disc portion 3a is disposed on the upper surface portion 2a of the housing 2. A through hole 2d is provided on the upper surface portion 2a of the housing 2. The riveting portion 3b extends from the disc portion 3a disposed on the outside of the housing 2 through the through hole 2d into the interior of the housing 2.
[0027] The positive current collector 4 is housed within the housing 2. The positive current collector 4 is positioned on one side Z1 in the Z-axis direction relative to the wound electrode body 1. The positive current collector 4 is welded to the composite material unformed portion 12a of the positive electrode plate 10. Thus, the positive current collector 4 is positively charged. The positive current collector 4 is welded to the end of the riveting portion 3b on the other side Z2 in the Z-axis direction. Thus, the positive terminal 3 is positively charged.
[0028] An external gasket 5 is disposed between the disk portion 3a of the positive terminal 3 and the upper surface portion 2a of the housing 2. Thus, the positive terminal 3 and the housing 2 are insulated from each other.
[0029] An internal gasket 6 is disposed inside the housing 2 between the housing 2 and the positive current collector 4. Thus, the housing 2 and the positive current collector 4 are mutually insulated. It should be noted that the riveting part 3b contacts the positive current collector 4 by passing through the internal gasket 6.
[0030] The negative electrode current collector 7 is housed within the housing 2. The negative electrode current collector 7 is located on the opposite side Z2 in the axial direction Z relative to the wound electrode body 1. The negative electrode current collector 7 is welded to the composite material unformed portion 22a of the negative electrode plate 20. Therefore, the negative electrode current collector 7 carries a negative charge. The negative electrode current collector 7 is in contact with the housing 2. Specifically, the negative electrode current collector 7 is in contact with the lower surface portion 2b and the side surface portion 2c. Therefore, the housing 2 carries a negative charge. Furthermore, the upper surface portion 2a carries a negative charge.
[0031] Figure 2 This is a simplified top view of the positive electrode plate of the wound electrode body according to the embodiment after it has been unfolded. Figure 3 This is a simplified cross-sectional view of the positive electrode plate of the wound electrode body according to the embodiment. It should be noted that... Figure 3 It is along Figure 2 The sectional view shown is taken along line III-III. (Refer to...) Figure 2 as well as Figure 3 The positive electrode plate 10 involved in the implementation method is explained.
[0032] In its unfolded state, the positive electrode plate 10 has a strip-like shape extending along the length direction D1. The length direction D1 is the direction in which the winding direction X is unfolded into a straight line. The positive electrode plate 10 has a first end 10a and a second end 10b in the length direction D1. The first end 10a is the end located on the inner circumferential side of the wound electrode body 1 (the inner circumferential end of the winding). The second end 10b is the end located on the outer circumferential side of the wound electrode body 1 (the outer circumferential end of the winding).
[0033] The positive electrode plate 10 includes a positive current collector 11, a first positive electrode film 13, and a second positive electrode film 14. The positive current collector 11 is made of a metal foil such as aluminum. The positive current collector 11 has a first main surface 11a and a second main surface 11b arranged along the thickness direction. In the state of winding the electrode body 1, that is, in the wound state after the positive electrode plate 10 is wound, the first main surface 11a faces the inner peripheral side, and the second main surface 11b faces the outer peripheral side.
[0034] The positive electrode plate 10 has a composite material unformed portion 12a and a composite material formed portion 12b. The composite material unformed portion 12a is the portion of the positive electrode current collector 11 exposed from both the first positive electrode film 13 and the second positive electrode film 14. The composite material formed portion 12b is the portion of the positive electrode plate 10 where both the first positive electrode film 13 and the second positive electrode film 14 are formed. The composite material unformed portion 12a extends from the composite material formed portion 12b toward one side in the width direction D2 of the positive electrode plate 10. It should be noted that the width direction D2 is the direction parallel to the axial direction Z in the wound electrode body 1. In the wound state, the composite material unformed portion 12a is exposed from the composite material formed portion 12b toward one side Z1 in the axial direction Z of the wound electrode body 1.
[0035] The first positive electrode film 13 is disposed on the first main surface 11a. The density of the first positive electrode film 13 is less than the density of the second positive electrode film 14. The first positive electrode film 13 is disposed on the first main surface 11a on one side of the width direction D2, which is orthogonal to the aforementioned length direction, with the end of the first main surface 11a exposed.
[0036] The second positive electrode film 14 is disposed on the second main surface 11b. The second positive electrode film 14 is disposed on one side of the second main surface 11b in the width direction D2, which is orthogonal to the aforementioned length direction, such that its end is exposed on the second main surface 11b. The second positive electrode film 14 is disposed in the thickness direction T of the positive electrode plate 10 (refer to...). Figure 3 The second positive electrode film 14 is configured to overlap with the first positive electrode film 13. The size of the second positive electrode film 14 is basically the same as that of the first positive electrode film 13.
[0037] The density of the second positive electrode film 14 is more than 1.1 times and less than 1.5 times the density of the first positive electrode film 13.
[0038] Both the first positive electrode film 13 and the second positive electrode film 14 have a first region R1 located on the first end 10a side of the inner circumference of the winding and a second region R2 located on the second end 10b side of the outer circumference of the winding in the winding direction X.
[0039] The first positive electrode film 13 and the second positive electrode film 14 have a first region R1 located on the side of the first end 10a, a second region R2 located on the side of the second end 10b, and an intermediate region R3 located between the first region R1 and the second region R2 in the length direction D1. That is, the first positive electrode film 13 and the second positive electrode film 14 have a first region R1 located on the side of the inner circumference end of the winding, a second region R2 located on the side of the outer circumference end of the winding, and an intermediate region R3 located between the first region R1 and the second region R2 in the wound state.
[0040] The densities of the first positive electrode film 13 and the second positive electrode film 14 increase sequentially in the first region R1, the intermediate region R3, and the second region R2.
[0041] Figure 4 This is a simplified top view of the negative electrode plate of the wound electrode body according to the embodiment after it has been unfolded. Figure 5 This is a simplified cross-sectional view of the negative electrode plate included in the wound electrode body according to the embodiment. (Refer to...) Figure 4 as well as Figure 5 The negative electrode plate 20 involved in the implementation method is described.
[0042] The negative electrode plate 20, in its unfolded state, has a strip-like shape extending along the length direction D1. The negative electrode plate 20 has a first end 20a and a second end 20b along the length direction D1. The first end 20a is the end located on the inner circumferential side of the wound electrode body 1 (the inner circumferential end). The second end 20b is the end located on the outer circumferential side of the wound electrode body 1 (the outer circumferential end).
[0043] The negative electrode plate 20 includes a negative electrode current collector 21, a first negative electrode film 23, and a second negative electrode film 24. The negative electrode current collector 21 is made of a metal foil such as copper. The negative electrode current collector 21 has a first main surface 21a and a second main surface 21b arranged along the thickness direction T. In the state of winding the electrode body 1, that is, in the wound state after the negative electrode plate 20 is wound, the first main surface 21a faces the inner peripheral side, and the second main surface 21b faces the outer peripheral side.
[0044] The negative electrode plate 20 has a composite material unformed portion 22a and a composite material formed portion 22b. The composite material unformed portion 22a is the portion of the negative electrode current collector 21 exposed from both the first negative electrode film 23 and the second negative electrode film 24. The composite material formed portion 22b is the portion formed by both the first negative electrode film 23 and the second negative electrode film 24 in the negative electrode plate 20. The composite material unformed portion 22a extends from the composite material formed portion 22b to the other side in the width direction. In the wound state, the composite material unformed portion 22a is exposed from the composite material formed portion 22b to the other side Z2 in the axial direction Z of the wound electrode body 1.
[0045] The first negative electrode film 23 is disposed on the first main surface 21a. The density of the first negative electrode film 23 is less than the density of the second negative electrode film 24. The first negative electrode film 23 is disposed on the first main surface 21a on the other side of the width direction D2, which is orthogonal to the aforementioned length direction D1, with the first main surface 21a exposed.
[0046] The second negative electrode film 24 is disposed on the second main surface 21b. The second negative electrode film 24 is disposed on the other side of the second main surface 21b in the width direction D2, which is orthogonal to the aforementioned length direction D1, with the second main surface 21b exposed. The second negative electrode film 24 is arranged to overlap with the first negative electrode film 23 in the thickness direction T of the negative electrode plate 20. The dimensions of the second negative electrode film 24 are substantially the same as the dimensions of the first negative electrode film 23.
[0047] The density of the second negative electrode film 24 is more than 1.1 times and less than 1.5 times the density of the first negative electrode film 23.
[0048] Both the first negative electrode film 23 and the second negative electrode film 24 have a first region R1 located on the first end 20a side of the inner circumference of the winding and a second region R2 located on the second end 20b side of the outer circumference of the winding in the winding direction.
[0049] The first negative electrode film 23 and the second negative electrode film 24 have a first region R1 located on the side of the first end 20a, a second region R2 located on the side of the second end 20b, and an intermediate region R3 located between the first region R1 and the second region R2 in the length direction. That is, the first negative electrode film 23 and the second negative electrode film 24 have a first region R1 located on the side of the inner circumference end of the winding, a second region R2 located on the side of the outer circumference end of the winding, and an intermediate region R3 located between the first region R1 and the second region R2 in the winding state.
[0050] The densities of both the first negative electrode film 23 and the second negative electrode film 24 increase sequentially in the first region R1, the intermediate region R3, and the second region R2.
[0051] It should be noted that the aforementioned positive electrode plate 10 is formed by attaching a first positive electrode film 13 to the first main surface 11a of the positive current collector 11 and attaching a second positive electrode film 14 to the second main surface 11b of the positive current collector 11. The first positive electrode film 13 is composed of the electrode film of the first positive electrode, and the second positive electrode film 14 is composed of the electrode film of the second positive electrode.
[0052] When the density is changed along the winding direction as described above, both the electrode film of the first positive electrode and the electrode film of the second positive electrode contain multiple electrode films with different densities, and each electrode film is attached to a corresponding region.
[0053] The density of the electrode film attached to the positive electrode in the first region R1 is less than the density of the electrode film attached to the positive electrode in the intermediate region R3, and less than the density of the electrode film attached to the positive electrode in the second region R2. The density of the electrode film attached to the positive electrode in the intermediate region R3 is less than the density of the electrode film attached to the positive electrode in the second region R2.
[0054] The density of the composite material in each electrode film can be adjusted during the manufacturing of each electrode film by changing conditions such as pressing pressure.
[0055] Similarly, the negative electrode plate 20 is formed by attaching a first negative electrode film 23 to the first main surface 21a of the negative electrode current collector 21 and attaching a second negative electrode film 24 to the second main surface 21b of the negative electrode current collector 21. The first negative electrode film 23 is composed of the electrode film of the first negative electrode, and the second negative electrode film 24 is composed of the electrode film of the second negative electrode.
[0056] When the density is changed along the winding direction as described above, the electrode film of the first negative electrode and the electrode film of the second negative electrode each contain multiple electrode films with different densities, and each electrode film is attached to a corresponding region.
[0057] The density of the electrode film attached to the negative electrode in the first region R1 is less than the density of the electrode film attached to the negative electrode in the intermediate region R3, and less than the density of the electrode film attached to the negative electrode in the second region R2. The density of the electrode film attached to the negative electrode in the intermediate region R3 is less than the density of the electrode film attached to the negative electrode in the second region R2.
[0058] The density of the composite material in each electrode film can be adjusted by changing conditions such as pressing pressure during the manufacturing of each electrode film.
[0059] As described above, an example is given where the density of both the first positive electrode film 13 and the second positive electrode film 14 increases as they approach the outer periphery of the winding on the positive electrode plate 10 side, but this is not the only example. As long as the density of the first positive electrode film 13 is less than the density of the second positive electrode film 14, the density of the composite material in both the first positive electrode film 13 and the second positive electrode film 14 can remain approximately constant as they approach the outer periphery of the winding.
[0060] In this case, the electrode film used as the first positive electrode is a single electrode film with a density that is approximately constant in the winding direction, and the electrode film used as the second positive electrode is also a single electrode film with a density that is approximately constant in the winding direction. The densities of the electrode films of the first and second positive electrodes can be adjusted by changing conditions such as pressing pressure during the manufacturing of each electrode film.
[0061] Similarly, an example is shown on the negative electrode plate 20 side where the densities of both the first negative electrode film 23 and the second negative electrode film 24 increase as they approach the outer periphery of the winding, but this is not the only example. As long as the density of the first negative electrode film 23 is less than the density of the second negative electrode film 24, the densities of both the first negative electrode film 23 and the second negative electrode film 24 can remain approximately constant as they approach the outer periphery of the winding.
[0062] In this case, the electrode film used as the first negative electrode is also a single electrode film with a density that is approximately constant in the winding direction, and the electrode film used as the second negative electrode is also a single electrode film with a density that is approximately constant in the winding direction. The densities of the electrode films of the first negative electrode and the second negative electrode can be adjusted by changing conditions such as pressing pressure during the manufacturing of each electrode film.
[0063] (Electrode film)
[0064] The electrode films of the first positive electrode and the second positive electrode can also be made of self-supporting films. Similarly, the electrode films of the first negative electrode and the second negative electrode can also be made of self-supporting films.
[0065] A self-supporting membrane is characterized by its ability to maintain its shape even without a support structure. For example, a self-supporting membrane possesses sufficient strength to withstand roller conveying even without a support structure such as a current collector (described later). The tensile strength range of a self-supporting membrane can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa, and 1.0 MPa, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The tensile strength range of a self-supporting membrane can be, for example, 0.1 MPa to 1.0 MPa. The tensile strength range of a self-supporting membrane can also be, for example, 0.5 MPa or higher. Having a tensile strength of 0.5 MPa or higher in a self-supporting membrane is expected to facilitate processes such as roll material handling.
[0066] The tensile strength of each of the above electrode films can be determined, for example, by the following method: A specimen is cut from the electrode film. The planar dimensions of the specimen are, for example, approximately 30 mm × 30 mm. A tensile test is performed on the specimen using a texture analyzer (e.g., manufactured by Eihong Seiki Co., Ltd.) at a speed of 2 mm / s. The maximum load during tension is measured. The tensile strength is calculated using the following formula. The tensile strength value is the arithmetic mean of three specimens.
[0067] Rm=(F×0.0098) / (t・W)
[0068] Rm: Tensile strength [MPa]
[0069] F: Maximum load [g]
[0070] t: Sample thickness [mm]
[0071] W: Sample width [mm]
[0072] The electrode film can have any planar shape. For example, the planar shape of the electrode film can be strip-shaped, rectangular, circular, etc. The dimensions of the electrode film (thickness, length, width, etc.) can be arbitrarily changed according to the electrode design. The thickness range of the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 5μm, 10μm, 25μm, 50μm, 75μm, 100μm, 150μm, 200μm, 250μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, and 1000μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The thickness range of the electrode film can be, for example, 5μm to 1000μm. The density range of the electrode film can be, for example, from 0.5g / cm³. 3 1.0g / cm 3 1.5g / cm 3 2.0g / cm 3 2.5g / cm 3 3.0g / cm 3 3.5g / cm 3 4.0g / cm 3 4.5g / cm 3 5.0g / cm 3 The range formed by selecting any one value can be a range with only an upper or lower limit, or a range with both an upper and lower limit can be obtained by selecting any two values. The range may or may not include endpoints. For example, the density range of the electrode film could be 0.5 g / cm³. 3 ~5.0g / cm 3 .
[0073] (composition)
[0074] The electrode membrane contains an electrode active material and a first binder. The first binder contains a fibrous binder. That is, the electrode membrane contains an electrode active material and a fibrous binder. The electrode membrane may further contain, for example, a second binder, a conductive material, a solid electrolyte, etc. For example, the electrode membrane contains, by mass fraction, 0.1% to 10% of the first binder, 0% to 10% of the second binder, 0% to 10% of the conductive material, 0% to 30% of the solid electrolyte, and the balance being the electrode active material.
[0075] (Electrode active material)
[0076] The electrode active material is a powder. The particle size distribution of the electrode active material can be, for example, a unimodal distribution. The particle size distribution can be a volume distribution or a number distribution. Volume distribution can be determined by laser diffraction. Number distribution can be determined by microscopy. "D50" represents the particle size at which the cumulative frequency reaches 50% in the cumulative distribution. The range of D50 for the electrode active material can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1 μm, 0.5 μm, 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, and 30 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the D50 range of the electrode active material can be 0.1 μm to 30 μm.
[0077] The particle size distribution of electrode active materials can be bimodal or multimodal. For example, in the case of a bimodal particle size distribution (frequency distribution), particles belonging to the peaks on the larger particle size side are called "large particles," and particles belonging to the peaks on the smaller particle size side are called "small particles." The mode particle size of each peak can be considered as the particle size of each particle. The "mode particle size" represents the particle size at the peak of the frequency distribution. The particle size of large particles is "D". L "Relative to the particle size of small particles" D S The ratio of "D" to " L / D S The range can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1.2, 1.5, 2.0, 3.0, 4.0, and 5.0, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, a range can satisfy "1.2 ≦ D". L / D S Relationships such as ≦5.0”.
[0078] Electrode active materials can be primary or secondary particles. They can have any particle shape, such as spherical, ellipsoidal, scaly, plate-like, columnar, blocky, or irregular shapes.
[0079] The electrode active material can be a granulated body. Granulated bodies can be formed by any method. For example, they can be formed by spray drying, stirring granulation, etc. By granulation, the sphericity of the granulated body (secondary particles) can be adjusted. "Sphericity" refers to the roundness in an SEM image (two-dimensional image). Sphericity (roundness) is calculated using the following formula. Sphericity can be taken as the arithmetic mean of 10 particles.
[0080] ψ=4πS / L 2
[0081] ψ: Sphericity (roundness)
[0082] π: Pi
[0083] S: Cross-sectional area of the particle (the area enclosed by the particle's outline)
[0084] L: The perimeter of the particle (the length of the particle's outline).
[0085] The range of sphericity "ψ" of the electrode active material can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1 ≤ ψ ≤ 1.0".
[0086] In both the first and second negative electrode films, a negative electrode active material is used as the electrode active material. The negative electrode active material may contain at least one material selected from the group consisting of natural graphite (flake graphite, spherical graphite), artificial graphite, soft carbon, hard carbon, silicon, silicon oxide, silicon-based alloys, silicon-carbon composite material "Si-C", lithium silicate, tin, tin oxide, tin-based alloys, and lithium titanate. Spherical graphite may be coated with amorphous carbon, for example. For example, natural graphite, artificial graphite, soft carbon, and hard carbon can be collectively referred to as "carbon-based active materials". Silicon may contain any crystalline phase. Silicon may contain at least one material selected from the group consisting of cage-like type I phase, cage-like type II phase, and diamond phase. Si-C represents composite particles containing at least one of silicon and silicon oxide with carbon. For example, silicon may be loaded into the internal voids of carbon particles. The carbon particles may be graphite particles or amorphous carbon particles. For example, silicon, silicon oxide, silicon-based alloys, and silicon-carbon composites can be collectively referred to as "silicon-based active materials".
[0087] The negative electrode active material can be, for example, a mixture of natural graphite and artificial graphite. The range of the mass ratio "natural graphite:artificial graphite" can be, for example, a range with any two pairs of values selected from the groups consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1" as endpoints. For example, a mass ratio such as "natural graphite:artificial graphite = 1:9 to 9:1" can be satisfied.
[0088] The negative electrode active material can be, for example, a mixture of carbon-based and silicon-based active materials. The range of the mass ratio "carbon-based active material: silicon-based active material" can be, for example, a range with any two groups selected as endpoints from the groups consisting of "1:99", "5:95", "10:90", "20:80", "30:70", "40:60", "50:50", "60:40", "70:30", "80:20", "90:10", "95:5", and "99:1". For example, a mass ratio of "carbon-based active material: silicon-based active material = 1:99 to 99:1" can be satisfied.
[0089] In both the first and second positive electrode films, a positive electrode active material is used as the electrode active material. The positive electrode active material may contain at least one compound selected from the group consisting of layered compounds, rock salt compounds, spinel compounds, and olivine compounds. For example, the positive electrode active material may be a mixture of layered compounds and olivine compounds. The mass ratio of "layered compound: olivine compound" may, for example, be a range with any two groups selected from the group consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", and "9:1" as endpoints. For example, a mass ratio such as "layered compound: olivine compound = 1:9 to 9:1" may be satisfied.
[0090] The positive electrode active material may contain at least one selected from the group consisting of Li(NiCoMn)O2 (layered compound), Li(NiCoAl)O2 (layered compound), LiMnO2 (rock salt compound), Li(NiMn)2O4 (spinel compound), and Li(MnFe)PO4 (olivine compound). It should be noted that the use of terms such as (NiCoMn) indicates that the total composition ratio within parentheses is 1. As long as the total is 1, the composition ratio of each component within parentheses can be arbitrary. For example, it is also permissible for some components to have a composition ratio of 0.
[0091] Layered compounds, for example, can have the general formula "Li x Ni a Cob M c O y The formula represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1≦x≦1.5". The formula satisfies the relationship "a+b+c=1". As long as this relationship is satisfied, the ranges of "a", "b", and "c" can be independently obtained by selecting any one value from the group consisting of 0, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, each with only an upper or lower limit. This can be a range with upper and lower limits obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0≦a≦1", "0≦b≦1", "0≦c≦1", etc. Similarly, it can satisfy relationships such as "0.5≦a≦0.9", "0.05≦b≦0.5", "0.05≦c≦0.5", etc. In the formula, "M" can be, for example, a range selected from the group consisting of Mn and A1. One less. The range of "y" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, and 2.4, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "1.6 ≦ y ≦ 2.4".
[0092] Layered compounds, for example, can be derived from Li x NiO y Li x CoO y Li x MnO y Li x Ni 1 / 3 Co 1 / 3 Mn 1 / 3 O y Li x Ni 0.4 Co 0.3 Mn 0.3 O y Li x Ni 0.5 Co 0.2 Mn 0.3 Oy Li x Ni 0.5 Co 0.3 Mn 0.2 O y Li x Ni 0.5 Co 0.4 Mn 0.1 O y Li x Ni 0.5 Co 0.1 Mn 0.4 O y Li x Ni 0.6 Co 0.3 Mn 0.1 O y Li x Ni 0.6 Co 0.2 Mn 0.2 O y Li x Ni 0.6 Co 0.1 Mn 0.3 O y Li x Ni 0.7 Co 0.2 Mn 0.1 O y Li x Ni 0.7 Co 0.1 Mn 0.2 O y Li x Ni 0.8 Co 0.1 Mn 0.1 O y Li x Ni 0.8 Co 0.15 Al 0.05 O y and Li x Ni 0.9 Co 0.05 Mn 0.05 O y The selected group must be at least one of the following. For example, the formula can satisfy relationships such as "0.1≦x≦1.5" and "1.6≦y≦2.4".
[0093] Peridotite-type compounds may, for example, have a composition represented by the general formula "LiMPO4". In this formula, "M" may be at least one selected from the group consisting of Fe, Ni, Co, and Mn.
[0094] Peridotite-type compounds, for example, can have the general formula "Li x Mn 1-a Fe a PO y The formula represents the composition. The range of "x" can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, and 1.5, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not have endpoints. For example, it can satisfy relationships such as "0.1 ≦ x ≦ 1.5". The range of "a" can be, for example, a range obtained by selecting any one value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1.0. The range of values can be obtained by selecting any two values, which may or may not contain endpoints. For example, it can satisfy relationships such as "0 ≦ a ≦ 1.0" and "0.1 ≦ a ≦ 0.5". Similarly, the range of "y" can be obtained by selecting any value from the group consisting of 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, and 4.4, which may or may not contain endpoints. For example, it can satisfy relationships such as "3.6 ≦ y ≦ 4.4".
[0095] Peridotite-type compounds may, for example, contain compounds derived from Li x MnPO y Li x Mn 0.9 Fe 0.1 PO y Li x Mn 0.8 Fe 0.2 PO y Li x Mn 0.7 Fe 0.3 PO y Li x Mn 0.6 Fe 0.4 PO y Li x Mn 0.5 Fe 0.5 PO y Li x Mn 0.4 Fe0.6 PO y Li x Mn 0.3 Fe 0.7 PO y Li x Mn 0.2 Fe 0.8 PO y Li x Mn 0.1 Fe 0.9 PO y and Li x FePO y The selected group must be at least one of the following. For example, the expression can satisfy relationships such as "0.1≦x≦1.5" and "3.6≦y≦4.4".
[0096] Any dopant can be introduced into the positive electrode active material. The dopant can be interstitial or substitutional. For example, the dopant can include at least one element selected from the group consisting of B, C, N, halogens, Si, Na, Mg, Al, Mn, Co, Cr, Sc, Ti, V, Cu, Zn, Ga, Ge, Se, Sr, Y, Zr, Nb, Mo, In, Pb, Bi, Sb, Sn, W, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, and actinides. The molar fraction (doping amount) of the dopant can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01%, 0.1%, 1%, 3%, and 5%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The doping amount can range from, for example, 0.01% to 5%.
[0097] (Conductive materials)
[0098] Conductive materials can form electron conduction pathways within the electrode film. Conductive materials may include, for example, at least one material selected from the group consisting of acetylene black, Ketjen black (registered trademark), thermal cracking carbon black, furnace black, carbon fibers, carbon nanotubes, graphene sheets, metal fibers, and metal powders. When the electrode active material is a positive electrode active material, the group of materials constituting the conductive material may further include, for example, natural graphite and artificial graphite.
[0099] The conductive material can be, for example, a powder. The conductive material can have a smaller D50 compared to the electrode active material. The range of the D50 of the conductive material can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 3 μm, and 5 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The D50 range of the conductive material can be, for example, 0.01 μm to 5 μm.
[0100] The mass fraction range of the conductive material in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the mass fraction range of the conductive material can be 0% to 10%.
[0101] (Solid electrolyte)
[0102] Solid electrolytes can form ion conduction pathways within the electrode film. Solid electrolytes may include at least one selected from the group consisting of sulfide solid electrolytes, halide solid electrolytes, oxide solid electrolytes, hydride solid electrolytes, and nitride solid electrolytes. Sulfide solid electrolytes may include at least one selected from the group consisting of amorphous phases, crystalline phases, and glass-ceramic phases (crystalline glass). Crystalline phases may include, for example, argentite-germanium sulfide type, LGPS type, etc. Sulfide solid electrolytes may contain, for example, LiI-LiBr-Li3PS4, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2O-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li2S-GeS2-P2S5, Li2S-P2S5, Li 10 GeP2S 12 Li4P2S6, Li7P3S 11At least one of the following groups must be selected: LiI, LiBr, and Li7PS6. For example, "LiI-LiBr-Li3PS4" indicates a sulfide solid electrolyte formed by mixing LiI, LiBr, and Li3PS4 in any molar ratio. For example, the sulfide solid electrolyte can be generated by a mechanochemical method. The mixing ratio can be determined by marking numbers before each raw material. For example, "10LiI-15LiBr-75Li3PS4" indicates a mixing ratio (molar ratio) of "LiI:LiBr:Li3PS4=10:15:75".
[0103] Sulfide solid electrolytes can, for example, have a composition represented by the general formula "yLiI-zLiBr-(100-yz)[xLi2S-(1-x)P2S5]". The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1, 0.2, 0.25, 0.3, 0.4, 0.5, 0.6, 0.7, 0.75, 0.8, and 0.9, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy relationships such as "0.1≦x≦0.9". The formula also satisfies the relationship "0<100-yz≦100". As long as this relationship is satisfied, the ranges of "y" and "z" can be independently obtained by selecting any one value from the group consisting of 0, 5, 10, 15, 20, 25, and 30, resulting in a range with only an upper or lower limit. Alternatively, they can be obtained by selecting any two values, resulting in a range with both an upper and lower limit. The range may or may not include endpoints. For example, relationships such as "0≦y≦30" and "0≦z≦30" can be satisfied.
[0104] Sulfide solid electrolytes, for example, can have the general formula "Li4-xM 1-x P x S4 represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, and 1, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy the relationship "0 < x < 1". "M" in the formula can, for example, contain at least one value selected from the group consisting of Al, Zn, In, Ge, Si, Sn, Sb, Ga, and Bi.
[0105] Sulfide solid electrolytes, for example, can have the general formula "Li 10+x Ge 1+x P2-x S 12 The formula represents the composition. The range of "x" in the formula can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, and 0.7, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, it can satisfy a relationship such as "0 < x ≤ 0.7". A sulfide solid electrolyte represented by this formula may, for example, contain an LGPS-type crystalline phase.
[0106] Halogenated solid electrolytes, for example, can have the general formula "Li 6-na M a The composition is represented by "X6". In the formula, "n" represents the oxidation number of "M". "M" may, for example, contain atoms with an oxidation number of +3. "M" may, for example, contain atoms with an oxidation number of +4. "M" may, for example, contain at least one element selected from the group consisting of Y, Al, Ti, Zr, Ca, and Mg. For example, it may satisfy the relationship "0 < a < 2". "X" may, for example, contain at least one element selected from the group consisting of F, Cl, Br, and I.
[0107] Solid electrolytes can be, for example, powders. Solid electrolytes can have a smaller D50 compared to electrode active materials. The range of D50 for solid electrolytes can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.01 μm, 0.05 μm, 0.1 μm, 0.5 μm, 1 μm, 3 μm, and 5 μm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The D50 range of solid electrolytes can be, for example, 0.01 μm to 5 μm.
[0108] The volume fraction of the solid electrolyte in the electrode membrane can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 1%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, and 70%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the volume fraction of the solid electrolyte can range from 0% to 70%.
[0109] (First adhesive)
[0110] The first binder includes a fibrous binder. The first binder may also be substantially composed of a fibrous binder. The fibrous binder can be fibrillated, for example, by applying shear force to the granular binder (aggregates). For example, by feeding a composite material containing a granular binder to be converted into a fibrous binder and an electrode active material into the roll gap, shear force can be applied to the granular binder. By forming the granular binder into a fibrous binder, an electrode film can be formed. The rolling process can be performed once or repeatedly. Before the rolling process, shear force can be applied to the composite material, for example, by using a jet mill or a mixing granulator. For example, heating to 30°C to 150°C on top of the shear force can promote fibrillation. The granular binder can be completely or partially fibrillated. That is, the first binder may also contain granular components.
[0111] "Fibrous" indicates an aspect ratio (the ratio of the major diameter to the minor diameter) of 10 or higher. Materials with an aspect ratio lower than 10 are considered "granular." The aspect ratio (the ratio of fiber length to fiber diameter) of fibrous materials can, for example, be 100 or higher. The minor diameter, major diameter, fiber diameter, and fiber length are determined by microscopy. The aspect ratio is the arithmetic mean of 10 measured samples. The length of the short side of the smallest bounding rectangle "MBR" of the measured sample is considered the minor diameter, and the length of the long side is considered the major diameter. The fiber diameter represents the dimension in the direction orthogonal to the axis of the measured sample. The fiber length represents the total length along the axial direction.
[0112] The fibrous adhesive may, for example, comprise a polymer composition. The polymer composition may be a homopolymer, copolymer, polymer blend, or polymer alloy. The fibrous adhesive may, for example, comprise polytetrafluoroethylene (PTFE). The fibrous adhesive may also contain any additives in addition to PTFE. Additives may include, for example, at least one selected from the group consisting of polyolefins, cellulose, polyethers, and polysiloxanes. The additives and PTFE may form at least one selected from the group consisting of polymer blends, polymer alloys, and copolymers. The range of the mass fraction of PTFE in the fibrous adhesive, or the range of the mass fraction of the tetrafluoroethylene (TFE) derivative, may be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 0%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 95%, 99%, and 100%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The mass fraction of PTFE in fibrous binders can range from, for example, 0% to 100%.
[0113] The number-average molecular weight "Mn" of the polymer constituting the fibrous binder can, for example, be in the range of 10 × 10⁻⁶. 4 50×10 4 100×10 4 150×10 4 200×10 4 300×10 4 400×10 4 500×10 4 1000×10 4 2000×10 4 3000×10 4 The range formed by selecting any one value can be a range with only an upper or lower limit, or a range with both an upper and lower limit can be obtained by selecting any two values. The range may or may not include endpoints. For example, the range for number-average molecular weight could be 10 × 10⁻⁶. 4 ~3000×10 4 Number-average molecular weight can be obtained, for example, from standard specific gravity. Test samples are prepared according to ASTM D-4895 98. Standard specific gravity is determined using the water displacement method according to ASTM D-792.
[0114] The range of fiber diameter (fiber diameter) of the fibrous adhesive can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 1nm, 5nm, 10nm, 15nm, 20nm, 50nm, 100nm, 200nm, 500nm, and 1000nm, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. For example, the fiber diameter range can be 1nm to 1000nm.
[0115] Fibrous binders can form a fibrous matrix. For example, the fibrous matrix can be used to hold the electrode active material (powder) in place, thus maintaining the shape of the electrode membrane. The fibrous matrix can be evaluated, for example, by fiber density. Fiber density can be determined, for example, by the following method: Prepare a cross-sectional SEM image of the electrode membrane. In the cross-sectional SEM image, mark a 20 μm straight line at any location. Calculate the fiber density (unit: strands / 20 μm) by counting the fibrous portions intersecting this line. Measure the fiber density at at least three locations within the cross-sectional SEM image. Use the arithmetic mean of the three or more locations as the fiber density. The range of fiber density can be, for example, a range with only an upper or lower limit obtained by selecting any one value from the group consisting of 1, 2, 5, 10, 20, 40, 60, 80, and 100, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of fiber density can be, for example, 1 to 100.
[0116] The range of the mass fraction of the first binder in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of the mass fraction of the first binder in the electrode film can be, for example, 0.1% to 10%.
[0117] (Second adhesive)
[0118] The form of the second adhesive is arbitrary. For example, the second adhesive can be granular, film-like, fibrous, etc. For example, the second adhesive can have a greater adhesive force than the first adhesive. For example, the electrode film can be fixed to the current collector by the second adhesive. The second adhesive may contain at least one component selected from the group consisting of polyvinylidene fluoride (PVdF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyethylene oxide (PEO), styrene-butadiene rubber (SBR), nitrile rubber (NBR), polyethylene (PE), polypropylene (PP), polyacrylonitrile (PAN), polyoxyethylene alkyl ether, polyimide (PI), polyamide-imide (PAI), and derivatives thereof.
[0119] The range of the mass fraction of the second binder in the electrode film can be, for example, a range with only an upper or lower limit obtained by selecting any value from the group consisting of 0%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, and 10%, or a range with both an upper and lower limit obtained by selecting any two values. The range may or may not include endpoints. The range of the mass fraction of the second binder in the electrode film can be, for example, 0% to 10%.
[0120] The range of the mass ratio "first adhesive: second adhesive" can be, for example, a range with any two pairs of pairs selected from the groups consisting of "1:9", "2:8", "3:7", "4:6", "5:5", "6:4", "7:3", "8:2", "9:1", and "10:0" as endpoints. For example, a mass ratio of "first adhesive: second adhesive = 1:9 to 10:0" can be satisfied.
[0121] (Added ingredients)
[0122] The electrode film can contain any additives. These additives may include, for example, inorganic fillers, organic fillers, surface modifiers, dispersants, lubricants, flame retardants, protective agents, fluxes, coupling agents, and adsorbents. Other additives may include, for example, polyoxyethylene allyl phenyl ether phosphate, zeolite, silane coupling agents, molybdenum sulfide, and tungsten oxide.
[0123] (Summarize)
[0124] As described above, in this embodiment, on both the positive electrode plate 10 side and the negative electrode plate 20 side, the density of the first composite material layer disposed on the first main surface of the current collector is lower than the density of the second composite material layer disposed on the second main surface of the current collector.
[0125] Generally, in a wound electrode body, the stress on the first main surface facing inward is greater than the stress on the second main surface facing outward. In this embodiment, as described above, on both the positive electrode plate 10 side and the negative electrode plate 20 side, the density of the first composite material layer provided on the first main surface, which has a greater stress than the second main surface facing outward, is lower than the density of the second composite material layer provided on the second main surface, thereby enabling the wound electrode body to be flexible. This reduces cracking in the composite material layers on both the positive electrode plate 10 side and the negative electrode plate 20 side.
[0126] It should be noted that, in this embodiment, an example is shown where the density of the first composite material layer disposed on the first main surface of the current collector is lower than the density of the second composite material layer disposed on the second main surface of the current collector on both the positive electrode plate 10 side and the negative electrode plate 20 side, but it is not limited to this.
[0127] On at least one side of the positive electrode plate 10 and the negative electrode plate 20, the density of the first composite material layer disposed on the first main surface of the current collector is lower than the density of the second composite material layer disposed on the second main surface of the current collector. In this case, the wound electrode body 1 can also be given flexibility, which can reduce cracking of the composite material layer on at least one side of the positive electrode plate 10 and the negative electrode plate 20. In this case, on the other side of the positive electrode plate 10 and the negative electrode plate 20, the density of the first composite material layer disposed on the first main surface of the current collector and the density of the second composite material layer disposed on the second main surface of the current collector can be the same.
[0128] Furthermore, in this embodiment, by setting the density of the second composite material layer to be at least 1.1 times and less than 1.5 times the density of the first composite material layer, appropriate flexibility can be imparted to the wound electrode body. For example, when the density of the second composite material layer is more than 1.5 times the density of the first composite material layer, the rigidity of the wound electrode body increases, making it difficult to wind. On the other hand, when the density of the second composite material layer is less than 1.1 times the density of the first composite material layer, the density difference between the first and second surfaces is small, making it difficult to impart sufficient flexibility to the wound electrode body.
[0129] Furthermore, as described above, by increasing the density of each region from the inside to the outside of the winding direction, the density of the composite material in regions subjected to greater stress can be reduced. This, in turn, can suppress cracking in the composite material layer.
[0130] (Other variations)
[0131] It should be noted that, in this embodiment, the first positive electrode film 13 and the second positive electrode film 14 are illustrated as each having three regions in the winding direction, but this is not a limitation. Alternatively, the first positive electrode film 13 and the second positive electrode film 14 may each have only a first region R1 located on the inner periphery end side of the winding and a second region R2 located on the outer periphery end side of the winding. In this case, the density of the first region R1 in the composite material layer of at least one of the first positive electrode film 13 and the second positive electrode film 14 may be lower than the density of the second region R2.
[0132] Furthermore, the first positive electrode film 13 and the second positive electrode film 14 each have four or more regions in the winding direction. In this case, the density of the multiple regions in at least one of the positive electrode films 13 and 14 increases as it approaches the outer periphery of the winding from the inner periphery end side.
[0133] It should be noted that, in the first negative electrode film 23 and the second negative electrode film 24, the number of regions in the winding direction and the density of each region can be appropriately set, just like in the first positive electrode film 13 and the second positive electrode film 14, as described above.
[0134] The above description illustrates the case where both the first positive electrode film 13 and the second positive electrode film 14 are composed of self-supporting films, but it is not limited to this. Alternatively, one of the first positive electrode film 13 and the second positive electrode film 14 may be composed of a self-supporting film.
[0135] Furthermore, the above description illustrates a case where a positive electrode film is provided on both sides of the positive current collector 11, but it is not limited to this. Alternatively, a positive electrode film may be provided on one side of the positive current collector 11, and a positive electrode composite material layer may be provided on the other side. In this case, the positive electrode composite material layer may be formed by coating a slurry, as has been done previously.
[0136] Similarly, although the example given is that both the first negative electrode film 23 and the second negative electrode film 24 are composed of self-supporting films, it is not limited to this. It is also possible that one of the first negative electrode film 23 and the second negative electrode film 24 is composed of a self-supporting film.
[0137] Furthermore, the above description illustrates a case where negative electrode films are provided on both sides of the negative electrode current collector 21, but it is not limited to this. Alternatively, a negative electrode film may be provided on one side of the negative electrode current collector 21, and a negative electrode composite material layer may be provided on the other side. In this case, the negative electrode composite material layer can be formed by coating a slurry as in the conventional manner.
[0138] In addition, at least one of the positive current collector 11 and the negative current collector 21 may have a waveform shape that meanders in the thickness direction relative to the winding direction.
[0139] Alternatively, either the positive electrode plate 10 or the negative electrode plate 20 can be formed by coating the current collector with a slurry.
[0140] (Postscript)
[0141] As described above, this implementation method includes the following disclosures.
[0142] [Component 1]
[0143] A wound electrode body, comprising:
[0144] A current collector having a first main surface located at one end in the thickness direction and a second main surface located at the other end in the thickness direction;
[0145] A first electrode film, disposed on the first main surface; and
[0146] A second electrode film is disposed on the second main surface.
[0147] The current collector is wound with the first main surface facing inward and the second main surface facing outward.
[0148] The density of the first electrode film is lower than that of the second electrode film.
[0149] [Component 2]
[0150] According to the wound electrode body described in configuration 1, wherein...
[0151] At least one of the first electrode film and the second electrode film is composed of a self-supporting film.
[0152] The electrode film of at least one of them contains active material powder and fibrillated binder.
[0153] [Component 3]
[0154] According to the wound electrode body described in 1 or 2, wherein...
[0155] The density of the second electrode film is more than 1.1 times and less than 1.5 times the density of the first electrode film.
[0156] [Composition 4]
[0157] According to the wound electrode body comprising any one of 1 to 3, wherein...
[0158] The first electrode film and the second electrode film comprise multiple regions along the winding direction of the current collector.
[0159] The density of at least one of the first electrode film and the second electrode film in the plurality of regions gradually increases from the inner peripheral side to the outer peripheral side from the winding direction.
[0160] [Component 5]
[0161] According to the wound electrode body described in configuration 4, wherein...
[0162] The first electrode film and the second electrode film, in the winding direction, include a first region located on the inner peripheral end side of the winding and a second region located on the outer peripheral end side of the winding.
[0163] The density of the electrode film of at least one of the electrodes in the first region is lower than the density of the electrode film of at least one of the electrodes in the second region.
[0164] [Composition 6]
[0165] According to the wound electrode body described in configuration 5, wherein...
[0166] The first electrode film and the second electrode film have an intermediate region located between the first region and the second region in the winding direction.
[0167] The density of the electrode film of at least one of them increases sequentially in the first region, the intermediate region, and the second region.
[0168] [Component 7]
[0169] A secondary battery, comprising:
[0170] The wound electrode body constitutes any one of 1 to 6; and
[0171] A housing that houses the wound electrode body.
[0172] The embodiments of the present invention have been described above. However, it should be understood that the embodiments disclosed herein are illustrative in all respects and are not intended to limit the invention. The scope of the invention is set forth in the claims and is intended to include all modifications that are equivalent to and within the scope of the claims.
Claims
1. A wound electrode body, comprising: A current collector having a first main surface located at one end in the thickness direction and a second main surface located at the other end in the thickness direction; A first electrode film is disposed on the first main surface; as well as A second electrode film is disposed on the second main surface. The current collector is wound with the first main surface facing inward and the second main surface facing outward. The density of the first electrode film is lower than that of the second electrode film.
2. The wound electrode body according to claim 1, wherein, At least one of the first electrode film and the second electrode film is composed of a self-supporting film. The electrode film of at least one of them contains active material powder and fibrillated binder.
3. The wound electrode body according to claim 1 or 2, wherein, The density of the second electrode film is more than 1.1 times and less than 1.5 times the density of the first electrode film.
4. The wound electrode body according to any one of claims 1 to 3, wherein, The first electrode film and the second electrode film comprise multiple regions along the winding direction of the current collector. The density of at least one of the first electrode film and the second electrode film in the plurality of regions gradually increases from the inner peripheral side to the outer peripheral side from the winding direction.
5. The wound electrode body according to claim 4, wherein, The first electrode film and the second electrode film, in the winding direction, include a first region located on the inner peripheral end side of the winding and a second region located on the outer peripheral end side of the winding. The density of the electrode film of at least one of them is lower in the first region than in the second region.
6. The wound electrode body according to claim 5, wherein, The first electrode film and the second electrode film have an intermediate region located between the first region and the second region in the winding direction. The density of the electrode film of at least one of them increases sequentially in the first region, the intermediate region, and the second region.
7. A secondary battery, comprising: The wound electrode body according to any one of claims 1 to 6; and A housing that houses the wound electrode body.
Citation Information
Patent Citations
Spiral lithium ion battery electrode and spiral lithium ion battery using the same
JP1999144762A