A method for recycling and repairing scrap materials from lithium-ion battery cathodes and its application.

By using alkaline treatment and lithium hydroxide solution to remove the binder, combined with hydrothermal calcination, the problem of binder reaction in NCM material recycling was solved, achieving efficient and environmentally friendly cathode material regeneration and restoration of electrochemical performance.

CN123073239APending Publication Date: 2026-11-10SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510600273.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing methods for recycling scrap materials from lithium-ion battery cathodes suffer from issues such as the reaction between binders and materials when processing NCM materials, which generates non-conductive substances that affect electrochemical performance. Furthermore, existing methods are time-consuming or cause significant environmental pollution.

Method used

The positive electrode material and current collector are separated by alkaline treatment, the binder is removed and lithium is added using lithium hydroxide solution, and then the material is regenerated by calcination under hydrothermal conditions.

Benefits of technology

It simplifies the process, reduces energy consumption, improves recycling efficiency, is environmentally friendly, and restores the electrochemical performance of cathode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123073239A_ABST
    Figure CN123073239A_ABST
Patent Text Reader

Abstract

This invention provides a method and application for recycling and repairing lithium-ion battery cathode waste. The recycling and repair method includes: pretreating lithium-ion battery cathode scraps with an alkaline solution to separate the cathode material from the current collector, obtaining recycled cathode material; directly mixing the recycled cathode material with lithium hydroxide and performing a hydrothermal reaction to replenish lithium and degrade the binder, obtaining an intermediate material; and calcining the intermediate material with a lithium source to obtain repaired cathode material. The method provided by this invention can simultaneously remove the binder from the surface of the cathode material crystals and replenish lithium in the crystals during the hydrothermal process, achieving direct hydrothermal-annealing recycling of cathode scraps. The structure and electrical properties of the recycled and repaired cathode material are comparable to commercially available materials, and the method has the advantages of simple process, high recovery rate, and environmental friendliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new energy technology, specifically relating to a method and application for recycling and repairing scrap materials from lithium-ion battery cathodes. Background Technology

[0002] The surge in demand for lithium-ion batteries from the electric vehicle sector has driven a massive expansion of the global battery manufacturing industry. According to the World Economic Forum, global battery demand is projected to reach 2,600 GWh by 2030. During these battery production processes, due to variations in factory process maturity and scale, electrode scrap is generated during electrode manufacturing and cutting, amounting to between 5% and 30% of the total output. Electrode production waste can be collected directly at different stages of battery manufacturing, as it is neither assembled into batteries nor in contact with the electrolyte. Therefore, battery manufacturers know its composition and do not need to disassemble batteries or perform other complex manual operations. Thus, electrode scrap is an readily available and high-value resource that needs to be recycled. Accelerating the direct recycling and reuse of electrode waste helps alleviate supply chain pressures and reduce battery costs by reintroducing recycled materials into battery production.

[0003] Currently, the mainstream recycling methods include pyrometallurgical recycling, hydrometallurgical recycling, and direct recycling. Among these three methods, the core purpose of pyrometallurgical and hydrometallurgical recycling is extraction—extracting valuable metal elements from spent batteries in the form of alloys or metal salts for subsequent utilization. Pyrometallurgical recycling requires high-temperature processing, resulting in high energy consumption and potentially generating harmful gases, leading to a significant environmental impact. Its recycling efficiency is limited; some metals are volatile or remain as slag, and it is difficult to recover specific metals alone, usually requiring combination with hydrometallurgical separation. Hydrometallurgical recycling typically requires large amounts of acid and alkali reagents, potentially causing secondary pollution and requiring wastewater treatment. It also involves multiple steps such as leaching, separation, and precipitation, making the process relatively complex. Direct recycling, on the other hand, aims at remediation, replenishing missing lithium and repairing phase transitions that occur during use or prolonged exposure to air without damaging the original crystal structure of the electrode material. Compared to energy-intensive pyrometallurgical recycling and environmentally unfriendly hydrometallurgical recycling, direct recycling has the simplest steps, requires the least pretreatment, and offers the highest recycling efficiency. Regeneration of failed electrode materials can be achieved using only separation, pretreatment, and lithium replenishment processes. Based on the characteristics of different cathode materials, direct regeneration methods can be further subdivided into hydrothermal methods, solid-state sintering methods, and molten salt methods. Compared to the hydrothermal regeneration of waste batteries, which requires manual disassembly and solvent removal of PVDF to separate aluminum foil and cathode powder, recycling electrode scraps eliminates the need for manual battery disassembly, reducing labor costs while improving safety.

[0004] Existing methods for directly regenerating electrode scrap involve simple calcination to separate the cathode material from the aluminum foil, followed by annealing to replenish a measured amount of missing lithium. This technology is suitable for LFP (lithium iron phosphate) materials and is relatively mature. However, NCM (lithium nickel cobalt manganese oxide) materials have poor thermal stability and high reactivity with binders. During calcination, they react with HF generated from the cracking of binders (such as PVDF) to form non-conductive LiF, thus affecting the charge-discharge performance of the material. Some existing technologies for separating aluminum foil and removing binders from the crystal surface involve soaking the material in organic solvents that can dissolve the binders. However, this method is time-consuming, and the organic solvents cause significant environmental pollution. Summary of the Invention

[0005] To solve all or part of the above-mentioned technical problems, the present invention provides the following technical solutions:

[0006] One objective of this invention is to provide a method for recycling and repairing scrap materials from lithium-ion battery cathodes, comprising:

[0007] Alkaline solution is used to pretreat the positive electrode scraps of lithium-ion batteries to separate the positive electrode material from the current collector, thereby obtaining recycled positive electrode material;

[0008] The recycled cathode material is mixed with a lithium hydroxide solution to replenish lithium in the recycled cathode material and degrade the binder therein, thereby obtaining an intermediate material;

[0009] The intermediate material is mixed with a lithium source and then calcined to obtain the repaired cathode material.

[0010] The method provided by this invention involves soaking cathode scrap in an alkaline solution to separate the current collector from the cathode material. Subsequently, a lithium hydroxide solution is used to remove the binder from the cathode material while simultaneously replenishing lithium lost due to prolonged exposure to air. In the subsequent calcination process, the phase transition is repaired, achieving material regeneration. The restored electrochemical performance of the final cathode material demonstrates the effectiveness of the hydrothermal direct recovery method for scrap regeneration.

[0011] In some embodiments, the method specifically includes: immersing the scrap material of the lithium-ion battery positive electrode in an alkaline solution with a concentration of 0.1-1 mol / L for 2-10 minutes, thereby separating the positive electrode material from the current collector.

[0012] In some embodiments, the alkali contained in the alkaline solution includes one or a combination of potassium hydroxide, sodium hydroxide, and lithium hydroxide.

[0013] In some embodiments, the method specifically includes: mixing the recycled cathode material with a lithium hydroxide solution with a concentration of 0.1-7 mol / L, and subjecting the resulting mixture to a hydrothermal reaction at a temperature of 180-240°C.

[0014] In some embodiments, the hydrothermal reaction takes 2-4 hours.

[0015] In some embodiments, the method specifically includes: heating to 750-950°C in an oxygen-containing atmosphere at a heating rate of 1-10°C / min, and holding at that temperature for 3-6 hours to carry out the calcination.

[0016] In some embodiments, the lithium source includes lithium carbonate and / or lithium hydroxide.

[0017] In some embodiments, the positive electrode material includes lithium nickel cobalt manganese oxide, wherein the nickel content in the lithium nickel cobalt manganese oxide is 30wt%-90wt%.

[0018] In some embodiments, the current collector is made of aluminum, for example, aluminum foil.

[0019] In some embodiments, the adhesive comprises PVDF.

[0020] The second objective of this invention is to provide a lithium-ion battery cathode material, which is obtained by recycling and repairing using any of the recycling and repair methods described in the invention.

[0021] The third objective of this invention is to provide the application of the aforementioned lithium-ion battery cathode material in the preparation of lithium-ion battery cathodes or lithium-ion batteries.

[0022] The fourth objective of this invention is to provide a lithium-ion battery positive electrode, wherein the lithium-ion battery positive electrode comprises the aforementioned lithium-ion battery positive electrode material.

[0023] Compared with existing technologies, the present invention has at least the following technical advantages: The method provided by the present invention can simultaneously remove the binder (such as PVDF) on the surface of the cathode material crystal and perform preliminary lithium replenishment on the crystal in one step during the hydrothermal process, realizing direct hydrothermal-annealing recycling of cathode scraps. The structure and electrical properties of the recycled and repaired cathode material are comparable to those of commercially available materials. The method provided by the present invention shortens the regeneration process of lithium-ion battery cathode scraps, and compared with the direct calcination method, it lowers the reaction temperature, reduces energy consumption and operating costs, and is more environmentally friendly. Attached Figure Description

[0024] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0025] Figure 1 This is a schematic diagram of the hydrothermal-annealing direct regeneration process of NCM622 scrap in Embodiment 1 of the present invention;

[0026] Figure 2 This is the X-ray photoelectron spectrum of the NCM622 material after hydrothermal treatment in Example 4;

[0027] Figure 3 This is an X-ray electron diffraction pattern of the repaired cathode material R-NCM622 obtained in Example 4;

[0028] Figure 4 These are charge-discharge curves of the repaired cathode material R-NCM622 obtained in Example 4 and the commercial lithium nickel cobalt manganese oxide material C-NCM622;

[0029] Figure 5 The images show the cycle curves of the repaired R-NCM622 and the commercially available lithium nickel cobalt manganese oxide material C-NCM622 cathode material obtained in Example 4. Detailed Implementation

[0030] The technical solutions of the present invention will be described in detail below with reference to specific embodiments, so that those skilled in the art can better understand and implement the technical solutions of the present invention. The specific functional details disclosed herein should not be construed as limiting, but are merely intended to form the basis of the claims and to teach those skilled in the art to employ the representative basis of the invention in different ways in any suitable detailed embodiment.

[0031] In addition, unless otherwise specified, all raw materials used in the following embodiments can be purchased from the market or other sources, and all production and testing equipment used are known in the art, and the testing methods used are also methods conventionally used in the art.

[0032] Example 1

[0033] This embodiment provides a method for recycling and repairing NCM622 (lithium nickel cobalt manganese oxide) scrap. Figure 1 This is a schematic diagram of the process flow of this embodiment, which specifically includes the following steps:

[0034] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0035] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 0.1 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0036] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0037] Example 2

[0038] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0039] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 1 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured out, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0040] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0041] Example 3

[0042] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0043] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 3 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured out, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0044] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0045] Example 4

[0046] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0047] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0048] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace and held for 4 hours. Finally, it is cooled to room temperature to obtain the repaired cathode material, which is denoted as R-NCM622.

[0049] Figure 2The X-ray photoelectron spectrum of the NCM622 material (i.e., the product of step 2) after hydrothermal treatment in Example 4 illustrates that the present invention achieves one-step lithium replenishment and removal of the binder PVDF during the hydrothermal reaction. Figure 3 This is the X-ray electron diffraction pattern of R-NCM622 obtained in Example 4, illustrating the restoration of the layered structure of R-NCM622 using the method provided by this invention, and its compatibility with commercial materials. Figure 3 The consistency of C-NCM622 in the text.

[0050] Example 5

[0051] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: The NCM622 scrap was placed in a 1M KOH solution. The solution produced a large number of bubbles. After standing for 10 minutes, the aluminum foil was separated from the positive electrode material. Then, the aluminum foil was removed from the solution with tweezers. The positive electrode material was centrifuged, washed with water, and dried in a vacuum oven to obtain alkaline-treated lithium nickel cobalt manganese oxide, denoted as AD-NCM622.

[0052] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 7 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured out, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0053] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0054] Example 6

[0055] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0056] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0057] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 750°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0058] Example 7

[0059] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0060] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0061] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 950°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0062] Example 8

[0063] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: The NCM622 scrap was placed in a 1M KOH solution. The solution produced a large number of bubbles. After standing for 10 minutes, the aluminum foil was separated from the positive electrode material. Then, the aluminum foil was removed from the solution with tweezers. The positive electrode material was centrifuged, washed with water, and dried in a vacuum oven to obtain alkaline-treated lithium nickel cobalt manganese oxide, denoted as AD-NCM622.

[0064] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0065] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 1°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0066] Example 9

[0067] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: The NCM622 scrap was placed in a 1M KOH solution. The solution produced a large number of bubbles. After standing for 10 minutes, the aluminum foil was separated from the positive electrode material. Then, the aluminum foil was removed from the solution with tweezers. The positive electrode material was centrifuged, washed with water, and dried in a vacuum oven to obtain alkaline-treated lithium nickel cobalt manganese oxide, denoted as AD-NCM622.

[0068] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 220 °C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0069] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 10°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 4 hours and then cooled to room temperature to obtain the repaired cathode material.

[0070] Example 10

[0071] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 0.1M KOH solution. The solution generates a large number of bubbles. After standing for 2 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0072] (2) Hydrothermal lithium replenishment and removal of binder PVDF: The obtained AD-NCM622 was mixed with 80 mL of 5 mol / L lithium hydroxide solution and reacted in a forced-air oven at 180 °C for 2 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum oven to dry.

[0073] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate (the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 5°C / min in an oxygen atmosphere in a tube furnace. The temperature is held for 6 hours and then cooled to room temperature to obtain the repaired cathode material.

[0074] The cathode material prepared in Example 10 is equivalent to that in Example 1.

[0075] Comparative Example 1

[0076] (1) Alkali treatment to separate aluminum foil from positive electrode material on NCM622 scrap: NCM622 scrap is placed in 1M KOH solution. The solution generates a large number of bubbles. After standing for 10 minutes, the aluminum foil is separated from the positive electrode material. Then, the aluminum foil is removed from the solution with tweezers. The positive electrode material is centrifuged, washed with water, and dried in a vacuum oven to obtain lithium nickel cobalt manganese oxide after alkali treatment, which is denoted as AD-NCM622.

[0077] (2) Hydrothermal lithium replenishment and PVDF binder removal: The obtained AD-NCM622 and 80mL pure water The mixture was mixed and reacted in a forced-air drying oven at 220°C for 4 hours. After the reaction was completed, the supernatant was poured off, the material was washed with water and centrifuged, and then placed in a vacuum drying oven to dry.

[0078] (3) Sintering process: The product obtained in step (2) is mixed with lithium carbonate evenly (the amount of the mixture is such that the molar ratio of transition metal element and lithium element is 1:1.05). Then the mixture is transferred to a corundum boat and heated to 850°C at a heating rate of 2°C / min in an oxygen atmosphere in a tube furnace and held for 4 hours. Finally, it is cooled to room temperature to obtain the cathode material.

[0079] The positive electrode materials recovered in the above embodiments and comparative examples were used to make batteries for performance testing. Specifically, lithium sheets were used as the negative electrode of the battery, the electrolyte was KELOD lithium battery electrolyte 1M LiPF6EC∶DEC=1∶1, the separator was a 25μm thick KELOD lithium battery separator, and the batteries were assembled into coin cells for battery testing.

[0080] Table 1 shows the relevant process parameters and battery-related performance of the recycling and repair methods in Examples 1-9 and Comparative Example 1.

[0081] Table 1

[0082]

[0083] In Comparative Example 1, when the failed cathode material containing PVDF is hydrothermally treated in pure water, PVDF is difficult to degrade. During the subsequent calcination process, PVDF decomposes at high temperature, producing HF, which reacts with the cathode material to generate LiF, destroying the crystal structure of the material and resulting in extremely poor electrochemical performance.

[0084] Comparing Examples 1-5, treating the material with a lithium hydroxide solution of 0.1–3 mol / L can reduce PVDF, but the degradation is incomplete. Treating the material with a lithium hydroxide solution of 5 mol / L or higher can completely degrade PVDF. Comparing Examples 4 and 5, when the lithium hydroxide concentration is 7 mol / L, the battery capacity retention rate decreases compared to the 5 mol / L solution, but is still significantly higher than Comparative Example 1. Excessively high lithium hydroxide concentrations may leave alkaline residue on the material surface, leading to gelation of the battery slurry.

[0085] Comparing Examples 4, 6, and 7, during the calcination stage, the initial capacity and capacity retention of the repair material were superior when the calcination temperature was 850℃. At 750℃, the initial capacity and cycle stability tended to decrease slightly, possibly due to the lower temperature making it difficult to strengthen the crystal structure. At 950℃, the specific capacity tended to decrease slightly, possibly due to the volatilization of lattice lithium. Considering the initial capacity and capacity retention of the repair material, a calcination temperature of 750-950℃ was optimal, while excessively low or high temperatures would lead to a decrease in performance.

[0086] Comparing Examples 4, 8, and 9, a low heating rate does not affect the electrochemical performance of the material, but results in low efficiency. If the heating rate is too fast, the material's cycle stability may slightly decrease because the crystals cannot be sufficiently strengthened. Considering all factors, a heating rate of 1-10 °C / min is preferable; excessively high heating rates will lead to a decrease in material performance.

[0087] As a comparison, the present invention also prepared a control battery by replacing the above-mentioned R-NCM622 with commercial lithium nickel cobalt manganese oxide material (C-NCM622). Figure 4 These are charge / discharge curves of a battery assembled using the recycled and repaired R-NCM622 cathode material from Example 4, and a battery assembled using commercial C-NCM622. Figure 5 These are cycle curves of the batteries assembled with R-NCM622 and C-NCM622 in Example 4. From... Figure 4 , Figure 5 It is known that the method provided by the present invention can restore the electrochemical performance of NCM cathode scraps after regeneration, and the charge-discharge capacity and cycle stability are comparable to those of commercial lithium nickel cobalt manganese oxide materials.

[0088] In summary, the method provided by this invention can remove current collectors (e.g., aluminum foil) in the initial alkaline treatment process, and simultaneously remove binders (e.g., PVDF) and replenish lithium in the subsequent hydrothermal process. It has the advantages of simple process, high recovery rate and environmental friendliness.

[0089] All aspects, embodiments, features, and examples of this invention are to be regarded as illustrative in all respects and are not intended to limit the invention, the scope of which is defined only by the claims. Other embodiments, modifications, and uses will become apparent to those skilled in the art without departing from the spirit and scope of the invention as claimed.

[0090] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.

[0091] Although the invention has been described with reference to illustrative embodiments, those skilled in the art will understand that various other changes, omissions, and / or additions can be made without departing from the spirit and scope of the invention, and that elements of the embodiments can be substituted with substantially equivalents. Furthermore, many modifications can be made without departing from the scope of the invention to adapt particular situations or materials to the teachings of the invention. Therefore, this invention is not intended to be limited to the specific embodiments disclosed for carrying out the invention, but rather is intended to encompass all embodiments falling within the scope of the appended claims. Moreover, unless specifically stated otherwise, any use of the terms first, second, etc., does not indicate any order or importance, but is used to distinguish one element from another.

Claims

1. A method for recycling and repairing scrap materials from lithium-ion battery cathodes, characterized in that, include: Alkaline solution is used to pretreat the positive electrode scraps of lithium-ion batteries to separate the positive electrode material from the current collector, thereby obtaining recycled positive electrode material; The recycled cathode material is mixed with a lithium hydroxide solution to replenish lithium in the recycled cathode material and degrade the binder therein, thereby obtaining an intermediate material; The intermediate material is mixed with a lithium source and then calcined to obtain the repaired cathode material.

2. The recycling and repair method according to claim 1, characterized in that, Specifically, it includes: The scrap material of the positive electrode of the lithium-ion battery is immersed in an alkaline solution with a concentration of 0.1-1 mol / L for 2-10 minutes to separate the positive electrode material from the current collector.

3. The recycling and repair method according to claim 2, characterized in that: The alkaline solution contains one or more of the following bases: potassium hydroxide, sodium hydroxide, and lithium hydroxide.

4. The recycling and repair method according to claim 1, characterized in that, Specifically, it includes: The recovered cathode material is mixed with a lithium hydroxide solution with a concentration of 0.1-7 mol / L, and the resulting mixture is subjected to a hydrothermal reaction at a temperature of 180-240°C.

5. The recycling and repair method according to claim 4, characterized in that: The hydrothermal reaction takes 2-4 hours.

6. The recycling and repair method according to claim 1, characterized in that, Specifically, it includes: In an oxygen-containing atmosphere, the temperature is increased to 750-950℃ at a heating rate of 1-10℃ / min and held for 3-6 hours to carry out the calcination. And / or, the lithium source includes lithium carbonate and / or lithium hydroxide.

7. The recycling and repair method according to claim 1, characterized in that: The positive electrode material includes lithium nickel cobalt manganese oxide, wherein the nickel content in the lithium nickel cobalt manganese oxide is 30wt%-90wt%; And / or, the material of the current collector includes aluminum; And / or, the adhesive comprises PVDF.

8. A lithium-ion battery cathode material, characterized in that: It is recovered and repaired by the recovery and repair method described in any one of claims 1-7.

9. The application of the lithium-ion battery cathode material according to claim 8 in the preparation of lithium-ion battery cathodes or lithium-ion batteries.

10. A lithium-ion battery positive electrode, characterized in that, Including the lithium-ion battery cathode material as described in claim 8.