Flexible film for secondary batteries and secondary batteries including the flexible film
By introducing a shear-thickening fluid shock-resistant layer into the soft-pack membrane of secondary batteries, the problem of insufficient shock resistance of soft-pack batteries is solved, achieving higher shock resistance and safety.
Patent Information
- Application Number
- CN202610612995.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-10
AI Technical Summary
Pouch batteries are less impact-resistant than prismatic or cylindrical batteries, and pouch films need to be developed to compensate for this deficiency.
The impact-resistant layer is made of shear-thickening fluid. The laminated structure includes a substrate layer, a stretching layer, a metal layer and a sealing layer, and an impact-resistant layer is selectively formed between each layer. The impact-resistant layer contains octopus and nano-silica or aramid fibers.
It improves the impact resistance of secondary batteries, protects them from external impacts and internal explosions, and enhances battery safety.
Smart Images

Figure CN123073286A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a soft-pack film for secondary batteries and a secondary battery including the soft-pack film. Background Technology
[0002] Rechargeable batteries are batteries that can be recharged and discharged repeatedly. With the development of the information communication and display industries, rechargeable batteries are widely used as power sources for portable electronic communication devices such as portable cameras, mobile phones, and laptops. In addition, in recent years, battery packs that include rechargeable batteries have been developed for use as power sources in environmentally friendly vehicles such as hybrid electric vehicles.
[0003] Secondary batteries can be categorized into lithium secondary batteries, nickel-cadmium batteries, and nickel-metal hydride batteries. Among them, lithium secondary batteries have high operating voltage and energy density per unit weight, and are advantageous for charging speed and lightweight design, so they are being actively developed and applied.
[0004] A lithium-ion secondary battery may include an electrode assembly and an electrolyte impregnating the electrode assembly, the electrode assembly including a positive electrode, a negative electrode, and a separator. The electrode assembly and electrolyte may be housed in an outer packaging material, for example, a pouch.
[0005] Compared to prismatic or cylindrical batteries, pouch cells are lighter and offer greater flexibility in terms of packaging space. However, pouch cells are less shock-resistant than prismatic or cylindrical batteries, necessitating the development of pouch films to compensate for this deficiency. Summary of the Invention
[0006] (a) Technical problems to be solved One technical problem of the present invention is to provide a soft-pack film for secondary batteries with improved stability.
[0007] One technical problem of the present invention is to provide a secondary battery including the soft-pack film.
[0008] (II) Technical Solution A flexible battery pack according to an exemplary embodiment of the present invention comprises: a substrate layer; a stretching layer formed on the substrate layer; a metal layer formed on the stretching layer; and a sealing layer formed on the metal layer. The flexible battery pack further comprises an impact-resistant layer containing a shear-thickening fluid, the impact-resistant layer being present at at least one of the following: between the substrate layer and the stretching layer; between the stretching layer and the metal layer; and between the metal layer and the sealing layer.
[0009] In an exemplary embodiment, the impact-resistant layer may be formed simultaneously between the substrate layer and the tensile layer, between the tensile layer and the metal layer, and between the metal layer and the sealing layer.
[0010] In an exemplary embodiment, the shear-thickening fluid may contain oobleck.
[0011] In an exemplary embodiment, the omega-3 may contain starch and water.
[0012] In an exemplary embodiment, the mass ratio of the starch to the water can be from 1:10 to 10:1.
[0013] In an exemplary embodiment, the impact-resistant layer may further comprise nano-silica or aramid fibers.
[0014] In an exemplary embodiment, the content of the nano-silica can be from 1% to 20% by weight relative to the weight of the impact-resistant layer.
[0015] In an exemplary embodiment, the content of the aramid fiber can be from 1% to 20% by weight relative to the weight of the impact-resistant layer.
[0016] In an exemplary embodiment, the thickness of the impact-resistant layer can be from 5 μm to 50 μm.
[0017] In an exemplary embodiment, the soft-pack film for secondary batteries may further include an adhesive layer between the layers.
[0018] A secondary battery according to an exemplary embodiment of the present invention includes: an electrode assembly comprising alternating positive and negative electrodes; and a soft-shell film for the secondary battery, the soft-shell film for the secondary battery housing the electrode assembly.
[0019] (III) Beneficial Effects The flexible film for secondary batteries according to an exemplary embodiment of the present invention may include an impact-resistant layer comprising a shear-thickening fluid. Therefore, the impact resistance of the secondary battery can be improved, thereby protecting the secondary battery from external impacts and impacts caused by internal explosions.
[0020] The secondary battery including the soft-pack film of this invention can be widely used in green technology fields such as electric vehicles using batteries, battery charging stations, and other battery-powered solar and wind power generation. Furthermore, the lithium secondary battery including the soft-pack film of this invention can be used in eco-friendly electric vehicles and hybrid vehicles, which prevent climate change by suppressing air pollution and greenhouse gas emissions. Attached Figure Description
[0021] Figure 1 This is a schematic diagram illustrating the laminated structure of a soft film according to an exemplary embodiment.
[0022] Figure 2 and Figure 3 These are a plan view and a cross-sectional view of a secondary battery according to an exemplary embodiment. Detailed Implementation
[0023] According to an exemplary embodiment of the present invention, a soft-pack film for secondary batteries (hereinafter, may be simply referred to as soft-pack film) selectively forms an impact-resistant layer between the layers.
[0024] The exemplary embodiments will be described in more detail with reference to the accompanying drawings. However, the drawings and embodiments in this specification serve to further understand the technical concept of the invention, and therefore the invention should not be construed as being limited to the contents described in these drawings and embodiments.
[0025] The terms "upper part," "lower part," "above," "below," "first," "second," etc., used in this invention do not specify absolute positions or orders, but are used in a relative sense. For example, the above terms are used relatively to specify other areas relative to a specific reference plane.
[0026] The terms "inner side" and "outer side" used in this invention do not specify absolute directions, but are used in a relative sense. For example, the above terms are used relatively to specify other directions relative to a particular structure.
[0027] Figure 1 This is a schematic diagram illustrating the laminated structure of a soft film according to an exemplary embodiment.
[0028] Reference Figure 1 The soft film 100 may include a structure in which a substrate layer 110, a stretching layer 120, a metal layer 130 and a sealing layer 140 are stacked in sequence.
[0029] In an exemplary embodiment, the substrate layer 110 may be formed on the outer surface of the flexible film 100, thereby protecting the secondary battery from friction and impact from the outside. For example, when the flexible film 100 houses the electrode assembly 350, the substrate layer 110 may be formed on the side not directly opposite the electrode assembly.
[0030] In an exemplary embodiment, the substrate layer 110 may be made of a polymer, thereby electrically isolating the electrode assembly housed inside the pouch from the outside.
[0031] For example, the polymer may include polyethylene (PE), polypropylene (PP), polycarbonate (PC), polyethylene terephthalate (PET), polyvinyl chloride (PVC), acrylic-based polymers, polyacrylonitrile (PAN), polyimide (PI), polyamide (PA), cellulose, aramid, nylon, polyester, poly-p-phenylenebenzobisoxazole (PBO), polyarylate (PAR), Teflon, glass fiber, etc. These can have a single-layer film structure formed from one material or a composite film structure formed by two or more materials forming layers. Therefore, the abrasion resistance, heat resistance, and insulation properties of the flexible film 100 can be improved.
[0032] For example, the substrate layer 110 may contain polyethylene terephthalate. Therefore, the durability and insulation properties of the flexible film 100 can be improved.
[0033] In an exemplary embodiment, the thickness of the substrate layer 110 can be 1 μm to 100 μm, 3 μm to 80 μm, or 5 μm to 50 μm. Within these ranges, a reduction in the abrasion resistance, heat resistance, and insulation of the flexible film 100, as well as a reduction in the energy density per unit volume of the secondary battery, can be prevented.
[0034] In an exemplary embodiment, the stretch layer 120 may be formed on the substrate layer 110, thereby improving the elasticity of the flexible film 100.
[0035] The stretch layer 120 may comprise polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymers, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, poly(p-phenylenebenzobisoxazole), polyarylate, polytetrafluoroethylene, glass fiber, etc. These may have a single-layer membrane structure formed from one material or a composite membrane structure formed by two or more materials forming separate layers.
[0036] For example, the stretch layer 120 may contain nylon. Therefore, the formability and insulation properties of the flexible film can be improved.
[0037] In an exemplary embodiment, the thickness of the stretch layer 120 can be 1 μm to 30 μm, 5 μm to 25 μm, or 10 μm to 20 μm. Within these ranges, a reduction in the abrasion resistance, heat resistance, and insulation of the soft film 100, as well as a reduction in the energy density per unit volume of the secondary battery, can be prevented.
[0038] In an exemplary embodiment, the metal layer 130 may be formed on the upper part of the stretch layer 120, thereby ensuring the mechanical strength of the soft package 100 and blocking the entry and exit of external factors (such as gas, moisture, etc.), and preventing electrolyte leakage of the electrode assembly contained inside the soft package.
[0039] The metal layer 130 may contain a metal, such as an aluminum (Al) alloy. Therefore, a lightweight, flexible film 100 with improved mechanical strength, heat resistance, and insulation can be provided.
[0040] The aluminum alloy may further contain elements other than aluminum, such as iron (Fe), copper (Cu), chromium (Cr), manganese (Mn), nickel (Ni), magnesium (Mg), silicon (Si), and zinc (Zn). The content of these other elements in the aluminum alloy may be from 0.5 wt% to 2.0 wt%, 0.7 wt% to 1.8 wt%, or 1.0 wt% to 1.5 wt%. Within these ranges, the aluminum alloy exhibits excellent mechanical strength, formability, and resistance to external factors.
[0041] In an exemplary embodiment, the thickness of the metal layer 130 can be 20 μm to 100 μm, 25 μm to 80 μm, 30 μm to 60 μm, or 40 μm to 50 μm. Within these ranges, a reduction in the sealing durability of the soft-pack membrane can be prevented, while a reduction in the energy density per unit volume of the secondary battery can also be prevented.
[0042] In an exemplary embodiment, the sealing layer 140 may be formed on the inner surface of the flexible membrane 100. For example, when the flexible membrane 100 accommodates the electrode assembly 350, the sealing layer 140 may be formed on the side directly opposite the electrode assembly 350.
[0043] In an exemplary embodiment, the sealing layer 140 may comprise a thermopolymerizable compound. Therefore, when the sealing layer 140 is heat-treated in a contact state, the contact portion can achieve a strong bond and seal through the polymerization or crosslinking reaction of the thermopolymerizable compound.
[0044] The sealing layer 140 may comprise polyethylene, polypropylene, polycarbonate, polyethylene terephthalate, polyvinyl chloride, acrylic polymers, polyacrylonitrile, polyimide, polyamide, cellulose, aramid, nylon, polyester, poly(p-phenylenebenzobisoxazole), polyarylate, polytetrafluoroethylene, glass fiber, etc. These may have a single-layer membrane structure formed from one material or a composite membrane structure formed by two or more materials forming separate layers.
[0045] For example, the sealing layer 140 may contain polyolefin-based resins such as polyethylene and polypropylene. Therefore, the mechanical and chemical strength of the sealing layer can be improved.
[0046] The polyolefin-based resin may include acid-treated polyolefin (acid-modified polyolefin)-based resins, such as maleic anhydride grafted polypropylene (MAH-g-PP). Therefore, adhesion to the metal layer 130 can be improved.
[0047] In some embodiments, the sealing layer 140 may be a composite film of polypropylene and acid-treated polypropylene (acid-modified polypropylene). The polypropylene has excellent processability and moldability, thus facilitating easy sealing with a flexible membrane. The acid-treated polypropylene has excellent adhesion, particularly to metals, thereby enabling stable adhesion between the sealing layer 140 and the metal layer 130, enhancing the durability and reliability of the flexible membrane 100.
[0048] In some embodiments, the thickness of the sealing layer 140 can be 50 μm to 100 μm, 60 μm to 90 μm, or 70 μm to 80 μm. Within these ranges, a reduction in seal durability and a reduction in the energy density per unit volume of the secondary battery can be prevented.
[0049] Reference Figure 1Optionally, impact-resistant layers 150 can be further formed between the layers. For example, impact-resistant layers (150a, 150b, 150c) can be formed at least one of the following: between the substrate layer 110 and the stretch layer 120, between the stretch layer 120 and the metal layer 130, or between the metal layer 130 and the sealing layer 140. Therefore, the impact resistance of the secondary battery can be improved, thereby protecting the internally housed electrode assembly 350 from external impacts. Furthermore, in the event of an explosion inside the pouch, the propagation of the impact to other cells can be suppressed.
[0050] In an exemplary embodiment, impact-resistant layers (150a, 150b, 150c) may be simultaneously formed between the substrate layer 110 and the stretch layer 120, between the stretch layer 120 and the metal layer 130, and between the metal layer 130 and the sealing layer 140. When the impact-resistant layers are only disposed on the outer and / or inner surfaces of the flexible film 100, rather than between the layers of the flexible film 100, the impact resistance of the secondary battery may not be sufficiently improved.
[0051] The impact-resistant layer 150 may contain a shear-thickening fluid. For example, the shear-thickening fluid may contain Ohmic fluid. Therefore, the impact-resistant layer 150 may have the properties of a non-Newtonian fluid, thereby further improving the impact resistance of the secondary battery.
[0052] In an exemplary embodiment, the omelet may contain starch and water. For example, the mass ratio of starch to water in the omelet may be 1:10 to 10:1, 1:9 to 9:1, 1:8 to 8:1, 1:7 to 7:1, 1:6 to 6:1, or 1:5 to 5:1.
[0053] In an exemplary embodiment, the impact-resistant layer 150 may further comprise nanosilica, aramid fibers, etc. Therefore, the impact resistance of the secondary battery can be further improved.
[0054] For example, the content of the nano-silica may be 1% to 20% by weight, 1% to 15% by weight, or 1% to 10% by weight relative to the weight of the impact-resistant layer 150.
[0055] For example, the content of the aramid fiber may be 1% to 20% by weight, 1% to 15% by weight, or 1% to 10% by weight relative to the weight of the impact-resistant layer 150.
[0056] In an exemplary embodiment, the thickness of the impact-resistant layer 150 can be 5 μm to 50 μm, 7 μm to 40 μm, or 10 μm to 30 μm. Within these ranges, the reduction in the impact resistance of the secondary battery can be prevented, while the reduction in the energy density per unit volume of the secondary battery can also be prevented.
[0057] In an exemplary embodiment, the impact-resistant layer 150 may further comprise polymers such as polyurethane, ethylene-acrylic acid (EAA), polyamide, and polypropylene. Therefore, adhesive strength can be imparted to the impact-resistant layer.
[0058] In an exemplary embodiment, the impact-resistant layer 150 can be housed within a film made of polyethylene terephthalate (PET), polypropylene, or the like. Therefore, the impact-resistant layer corresponding to the fluid layer can be fixed inside the flexible packaging.
[0059] In an exemplary embodiment, the impact-resistant layer 150 may be further disposed on the outer and / or inner surfaces of the soft membrane 100.
[0060] In an exemplary embodiment, the impact-resistant layer 150 may not be provided on the outer surface of the flexible membrane 100. In an exemplary embodiment, the impact-resistant layer 150 may not be provided on the inner surface of the flexible membrane 100. Therefore, a decrease in the energy density per unit volume of the secondary battery can be prevented.
[0061] In an exemplary embodiment, the flexible film 100 may further include an adhesive layer for bonding the layers. For example, the adhesive layer may be formed between the stretch layer 120 and the metal layer 130. For example, the adhesive layer may be formed between the stretch layer 120 and the substrate layer 110.
[0062] There are no particular restrictions on the adhesive layer, as long as it can provide adhesion between the layers. For example, the adhesive layer can contain polyacrylate, etc.
[0063] In an exemplary embodiment, the thickness of the adhesive layer can be 1 μm to 10 μm, 1 μm to 8 μm, or 1 μm to 5 μm. Within these ranges, the layers of the flexible film can be stably stacked without reducing the energy density per unit volume of the secondary battery.
[0064] Figure 2 and Figure 3 These are, respectively, a plan view and a cross-sectional view of a secondary battery according to an exemplary embodiment. For example, Figure 3 It is along Figure 2 A cross-sectional view taken along the thickness direction of the I-I' line.
[0065] Figure 2 and Figure 3 The secondary battery shown is schematic for ease of explanation, and the structure of the secondary battery of the present invention is not limited to that shown. Figure 2 and Figure 3 The structure shown.
[0066] According to an exemplary implementation, a unit cell can be defined by a positive electrode 300, a negative electrode 330, and a separator 340, and an electrode assembly 350 can be formed by stacking multiple unit cells.
[0067] The positive electrode 300 may include a positive electrode current collector 305 and a positive electrode active material layer 310, which is formed by coating the positive electrode active material onto the positive electrode current collector 305. The positive electrode active material may contain compounds that allow lithium ions to be reversibly inserted and extracted. In this case, the secondary battery can be provided as a lithium secondary battery.
[0068] In an exemplary embodiment, the positive electrode active material may comprise lithium-transition metal composite oxide particles. For example, the lithium-transition metal composite oxide particles may comprise nickel (Ni), and may further comprise at least one of cobalt (Co) or manganese (Mn).
[0069] For example, the positive current collector 305 may include stainless steel, nickel, aluminum, titanium, copper, zinc or alloys thereof, preferably, the positive current collector 305 may include aluminum or aluminum alloy.
[0070] For example, the positive electrode active material can be mixed with a binder, conductive material and / or dispersant in a solvent and stirred to prepare a slurry. The slurry can be coated onto the positive electrode current collector 305 and then dried and calendered to manufacture a positive electrode 300 including a positive electrode active material layer 310.
[0071] The adhesive may include, for example, organic adhesives such as vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or water-based adhesives such as styrene-butadiene rubber (SBR), and may be used with thickeners such as carboxymethyl cellulose (CMC).
[0072] For example, PVDF-based binders can be used as positive electrode binders. In this case, the amount of binder used to form the positive electrode active material layer can be reduced, and the amount of positive electrode active material can be relatively increased, thereby improving the power and capacity of the secondary battery.
[0073] The conductive material may be included to facilitate electron migration between active material particles. For example, the conductive material may include carbon-based conductive materials such as graphite, carbon black, graphene, and carbon nanotubes, and / or metal-based conductive materials including perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0074] The negative electrode 330 may include a negative electrode current collector 325 and a negative electrode active material layer 320, which is formed by coating the negative electrode active material onto the negative electrode current collector 325.
[0075] The negative electrode active material can be any active material known in the art capable of adsorbing and desorbing lithium ions. For example, the negative electrode active material can be carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, and carbon fibers; lithium alloys; silicon (Si)-based active materials, etc.
[0076] Examples of amorphous carbon include hard carbon, coke, mesocarbon microbeads (MCMB), and mesophase pitch-based carbon fiber (MPCF).
[0077] Examples of crystalline carbon include natural graphite, artificial graphite, graphitized coke, graphitized mesophase carbon microspheres (MCMB), graphitized mesophase pitch-based carbon fibers (MPCF), and other graphite-based carbons.
[0078] Elements included in the lithium alloy may include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, or indium.
[0079] The negative electrode current collector 325 may comprise stainless steel, copper, nickel, aluminum, titanium, or alloys thereof. Preferably, the negative electrode current collector 325 may comprise copper or a copper alloy.
[0080] For example, the negative electrode active material can be mixed with the aforementioned binder, conductive material, thickener, etc., in a solvent and stirred to form a slurry. The slurry can be coated on at least one side of the negative electrode current collector 325 and then dried and calendered to manufacture a negative electrode 330 including a negative electrode active material layer 320.
[0081] The adhesive and conductive material may be substantially the same as or similar to the substances used in the positive electrode active material layer 310. In some embodiments, for example, for compatibility with carbon-based active materials, the adhesive used to form the negative electrode may include a water-based adhesive such as styrene-butadiene rubber (SBR) and may be used with a thickener such as carboxymethyl cellulose (CMC).
[0082] The separator 340 can be disposed between the positive electrode 300 and the negative electrode 330. The separator 340 may include a porous polymer membrane made of polyolefin-based polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer. The separator 340 may also include a nonwoven fabric formed of high-melting-point glass fiber, polyethylene terephthalate fiber, etc.
[0083] According to an exemplary embodiment, the electrode assembly 350 can be defined by alternately and repeatedly stacking a positive electrode 300, a negative electrode 330, and a separator 340 (the separator 340 is disposed between the positive electrode 300 and the negative electrode 330).
[0084] The electrode assembly 350 can be of the winding type, stacking type, z-folding type, or stack-folding type.
[0085] A secondary battery can be defined by housing the electrode assembly 350 together with the electrolyte within a housing 360 made of the aforementioned flexible membrane. According to an exemplary embodiment, the electrolyte can be a non-aqueous electrolyte.
[0086] Non-aqueous electrolytes may contain a lithium salt as the electrolyte and an organic solvent, wherein the lithium salt may be, for example, Li... + X - This indicates that the anion (X) of the lithium salt is... - ), can be exemplified by F - Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - PF6 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - CF3SO3 - CF3CF2SO3 - (CF3SO2)2N - (FSO2)2N - CF3CF2(CF3)2CO - (CF3SO2)2CH - (SF5)3C - (CF3SO2)3C- CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - wait.
[0087] The organic solvents may include, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, γ-butyrolactone, propylene sulfite, and tetrahydrofuran. These may be used alone or in combination of two or more.
[0088] like Figure 2 As shown, the tabs (positive tab and negative tab) can protrude from the positive current collector 305 and negative current collector 325 belonging to each cell and extend to a side of the housing 360. The tabs can be fused to the side of the housing 360 to form electrode leads (positive lead 307 and negative lead 327) extending to or exposed outside the housing 360.
[0089] Figure 2 The diagram shows the positive electrode lead 307 and the negative electrode lead 327 protruding from the upper side of the housing 360 in the planar direction, but the position of the electrode leads is not limited to this. For example, the electrode leads may protrude from at least one of the two sides of the housing 360, or from the lower side of the housing 360. Alternatively, the positive electrode lead 307 and the negative electrode lead 327 may be formed to protrude from different sides of the housing 360, respectively.
[0090] The secondary battery according to an exemplary embodiment of the present invention includes the electrode assembly 350 and the soft film described above, thereby having improved impact resistance.
[0091] The following are embodiments provided to aid in understanding the present invention. However, these embodiments are merely illustrative and do not limit the scope of the claims. Various changes and modifications can be made to the embodiments within the scope of the present invention and its technical concept. This is obvious to those skilled in the art, and such variations and modifications are naturally within the scope of the claims.
[0092] Example 1 1) Preparation of Eulerene Starch and water are mixed in a 1:2 ratio based on mass to produce Oubuli.
[0093] 2) Manufacturing of flexible packaging A flexible film is prepared by sequentially stacking and pressing a polypropylene (PP) layer (thickness: 40 μm), an aluminum (Al) layer (thickness: 40 μm), an adhesive layer (thickness: 2 μm), a nylon layer (thickness: 20 μm), an adhesive layer (thickness: 2 μm), an octane-retaining layer (thickness: 20 μm), an adhesive layer (thickness: 2 μm), and a PET film (thickness: 12 μm).
[0094] (3) Manufacturing of secondary batteries LiNi will be used as the positive electrode active material 0.8 Co 0.1 Mn 0.1 O2, carbon black as a conductive material, and polyvinylidene fluoride (PVDF) as a binder are mixed in a mass ratio of 95:3:2 to prepare a positive electrode slurry. The positive electrode slurry is then coated on an aluminum substrate and dried and calendered to form a positive electrode active material layer (120 μm).
[0095] A negative electrode slurry was prepared using 92% by weight of artificial graphite as the negative electrode active material, 2% by weight of styrene-butadiene rubber (SBR) based binder, 1% by weight of carboxymethyl cellulose (CMC) as a thickener, and 5% by weight of flake-like amorphous graphite as a conductive material. This negative electrode slurry was coated onto a copper substrate and then dried and calendered to form a 140 μm negative electrode active material layer.
[0096] A polyethylene (PE) diaphragm (15 μm) is placed between the positive and negative electrodes prepared as described above to form a battery cell. The battery cells are then stacked to form an electrode assembly, and the tab portions of the positive and negative electrodes are then welded together.
[0097] The electrode assembly is placed in the flexible film, and the three sides except for the electrolyte injection section are sealed. At this time, the portion with the tabs is included in the sealed section. Electrolyte is injected through the remaining sides except for the sealed section, and the remaining sides are sealed. Then, the sample is immersed for more than 12 hours to obtain a lithium secondary battery sample.
[0098] Example 2 The lithium secondary battery sample was manufactured using the same method as in Example 1, except that a polypropylene (PP) layer (thickness: 40 μm), an aluminum (Al) layer (thickness: 40 μm), an adhesive layer (thickness: 2 μm), an omega-3 layer (thickness: 20 μm), an adhesive layer (thickness: 2 μm), a nylon layer (thickness: 20 μm), an adhesive layer (thickness: 2 μm), and a PET film (thickness: 12 μm) were sequentially stacked to obtain a soft-pack film.
[0099] Examples 3 to 5 Lithium-ion battery samples were manufactured using the same method as in Example 1, except that the thicknesses of the ohmic layers used were 25 μm, 15 μm, and 10 μm, respectively.
[0100] The location and thickness of the eutectic layer in the above embodiments are shown in Table 1 below.
[0101] [Table 1] Comparative Example 1 The lithium secondary battery sample was manufactured using the same method as in Example 1, except that after laminating the PET film (thickness: 12 μm), an omega-3 layer (thickness: 20 μm) was laminated on the outer side of the soft-pack film to obtain the soft-pack film.
[0102] Comparative Example 2 The lithium secondary battery sample was manufactured using the same method as in Example 1, except that a soft film excluding the ohmic layer was manufactured.
[0103] Experiment Example 1: SLED Test The lithium secondary battery samples of the examples and comparative examples were charged to 50% SOC and then subjected to trolley tests.
[0104] The trolley test was conducted by applying an impact of 60G (G being the gravitational acceleration) to lithium secondary battery samples of the examples and comparative examples charged to 50% SOC for 45ms.
[0105] (1) Voltage After an impact was applied, the voltage change of the lithium secondary battery sample was measured.
[0106] No variation: There is no difference from the original voltage. Voltage drop: A change of more than 100mV compared to the original voltage. (2) Insulation resistance (Riso) (MΩ) After an impact was applied, the insulation resistance of the lithium secondary battery sample was measured.
[0107] Pass: Above 4000MΩ Failure: Less than 4000MΩ Experiment Example 2: Safety Evaluation (Drop Test) To measure battery safety, lithium secondary battery samples from the examples and comparative examples were dropped from a height of 1m to apply physical impact to the secondary batteries, and it was determined whether they were damaged, and the following distinctions were made.
[0108] In good condition: There is no obvious difference in overall appearance before and after the fall.
[0109] Good: No electrolyte leakage or smoke occurred, and no external physical damage occurred.
[0110] Damage: The battery experiences an internal short circuit due to physical damage, resulting in smoke or electrolyte leakage.
[0111] The results of the above trolley tests and safety evaluations are shown in Table 2 below.
[0112] [Table 2] Referring to Table 2, compared with the secondary battery of Comparative Example 1, which has an omega-3 layer with a thickness of 20 μm on the outer side of the pouch, and the secondary battery of Comparative Example 2, which does not have an omega-3 layer, the secondary battery of the embodiment with an omega-3 layer with a thickness of 15 μm or more on the inside of the pouch exhibited superior performance in the trolley test.
[0113] Furthermore, embodiments with a non-cracked layer thickness of 20 μm or more exhibited superior performance in trolley tests.
Claims
1. A soft-pack film for secondary batteries, comprising: Substrate layer; A stretch layer formed on the substrate layer; A metal layer formed on the stretched layer; as well as A sealing layer, the sealing layer being formed on the metal layer, The flexible film for secondary batteries further includes an impact-resistant layer comprising a shear-thickening fluid, the impact-resistant layer being located at at least one of the following: between the substrate layer and the stretching layer, between the stretching layer and the metal layer, and between the metal layer and the sealing layer.
2. The soft-pack film for secondary batteries according to claim 1, wherein, The impact-resistant layer is formed simultaneously between the substrate layer and the tensile layer, between the tensile layer and the metal layer, and between the metal layer and the sealing layer.
3. The soft-pack film for secondary batteries according to claim 1, wherein, The shear-thickening fluid contains Eulerene.
4. The soft-pack film for secondary batteries according to claim 3, wherein, The omega-3 contains starch and water.
5. The soft-pack film for secondary batteries according to claim 4, wherein, The mass ratio of starch to water is 1:10 to 10:
1.
6. The soft-pack film for secondary batteries according to claim 1, wherein, The impact-resistant layer further comprises nano-silica or aramid fibers.
7. The soft-pack film for secondary batteries according to claim 6, wherein, The content of the nano-silica is from 1% to 20% by weight relative to the weight of the impact-resistant layer.
8. The soft-pack film for secondary batteries according to claim 6, wherein, The content of the aramid fiber is from 1% to 20% by weight relative to the weight of the impact-resistant layer.
9. The soft-pack film for secondary batteries according to claim 1, wherein, The thickness of the impact-resistant layer is 5 μm to 50 μm.
10. The soft-pack film for secondary batteries according to claim 1, wherein, The soft-pack film for the secondary battery further includes an adhesive layer between the layers.
11. A secondary battery, comprising: An electrode assembly, the electrode assembly comprising alternately arranged positive and negative electrodes; as well as The soft-pack film for secondary batteries according to claim 1, wherein the soft-pack film for secondary batteries accommodates the electrode assembly.