An environmentally friendly solderable flexible circuit board and its manufacturing method

By using copper paste printing technology on PI film to manufacture flexible circuit boards, the complex and environmental problems of existing FPC processes have been solved, realizing a thin, foldable, environmentally friendly, solderable flexible circuit board, reducing costs and improving production efficiency.

CN123075802APending Publication Date: 2026-11-10SUZHOU SIPULANDI ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611162815.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-03
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The existing manufacturing process of single-sided FPC is complex, costly, and environmentally challenging, and it is difficult to achieve direct SMT soldering.

Method used

Flexible circuit boards are manufactured on PI films using copper paste printing technology. These boards include a substrate, adhesive layer, conductor layer, and protective layer. The process involves low-temperature sintering and printing additive manufacturing, avoiding wet chemical processes and achieving solderability and environmental friendliness of the conductor layer.

Benefits of technology

It reduces production costs, simplifies the process, enables thin and foldable circuit boards, possesses the high-temperature resistance of SMT technology, and improves environmental friendliness and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123075802A_ABST
    Figure CN123075802A_ABST
Patent Text Reader

Abstract

This invention relates to an environmentally friendly method for manufacturing a solderable flexible circuit board, comprising the following steps: S1: heat shrinking of the substrate layer; S2: adhesive application; S3: conductor layer printing; S4: copper paste sintering; S5: lamination and lamination; S6: die cutting. This invention utilizes low-temperature sintered printed copper paste to completely replace the production and processing of FCCL (Fused Crystal Disc Residue Coating) in the upstream manufacturing plant of FPC. This method directly forms conductors on the PI (polyimide) film, resulting in lighter, thinner, foldable, and bendable circuit boards. The use of additive manufacturing completely avoids the wet chemical process, making it more environmentally friendly. Manufacturing costs are reduced by more than 40% compared to traditional processes, making it more competitive. The heat-shrinkable and stabilized substrate and protective layer are more heat-resistant, enabling traditional SMT (Surface Mount Technology) processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to circuit boards, and more particularly to an environmentally friendly solderable flexible circuit board and its manufacturing method. Background Technology

[0002] Currently, single-sided FPCs in the electronics industry are all achieved using traditional etching methods. This process is complex, presenting significant challenges related to the environmental impact of chemical usage and wastewater discharge. The manufacturing process is also relatively long and costly. To address this, our company has developed a copper paste printing method to replace FCCL (Follicular Unit Cldextrose). This not only replaces the upstream copper foil processing but also saves substantial materials and manufacturing costs in the circuit production stage. Furthermore, the new flexible circuit board can simultaneously achieve direct SMT soldering, adding a new industrial track to "low-carbon production." Summary of the Invention

[0003] To address the shortcomings of existing technologies, the purpose of this invention is to provide an environmentally friendly weldable flexible circuit board and its manufacturing method.

[0004] The technical solution adopted by the present invention to solve its technical problem is: an environmentally friendly solderable flexible circuit board, comprising a substrate, an adhesive layer covering the top surface of the substrate, a conductor layer printed on the top surface of the adhesive layer, and a protective layer covering the top surface of the conductor layer. The adhesive layer is used to increase the adhesion between the conductor layer and the substrate. The conductor layer is made of printed sintered copper paste. The protective layer is used to isolate the conductor layer from the air. The substrate layer is a PI film.

[0005] As a further improvement to this design, the substrate layer is a heat-shrinkable PI film, and the substrate thickness is not less than 12.5 μm.

[0006] As a further improvement to this design, the adhesive layer is an ADH epoxy resin adhesive, and the copper paste is composed of copper powder mixed with epoxy resin.

[0007] As a further improvement to this design, the copper powder particle size in the copper paste is 1-10μm.

[0008] As a further improvement to this design, the protective layer is a PI film, and the protective layer has a window located above the solderable position of the conductor layer. The top surface of the solderable position of the conductor layer is provided with a gold plating layer.

[0009] An environmentally friendly method for manufacturing a solderable flexible circuit board includes the following steps: S1: Heat shrinking of the substrate layer: Bake the substrate at a temperature of 170℃-190℃ for 50-70 minutes, and then cool it after baking. S2: Coating: Apply ADH epoxy resin adhesive to the top surface of the substrate treated in step S1, with a coating thickness of 13μm-15μm. Pre-bake the coated ADH epoxy resin adhesive for 18-20 minutes at a pre-baking temperature of 80℃. Place the pre-baked product into a curing device and maintain the curing device at 150℃ for 40 minutes. S3: Conductor layer printing: Print copper paste on the top surface of the substrate treated in step S2, and print the copper paste into the designed circuit shape, controlling the copper paste thickness to be 10-15μm; pre-bake the printed copper paste at 80℃ for 2-3 minutes, and then cool it to room temperature; S4: Copper paste sintering: After processing in step S3, the plates are stacked and pressed together at a pressure of 1400Pa. The copper paste is vacuum preheated at a temperature of 75-85℃ for 8-12 seconds. The preheated copper paste is then vacuum sintered at a low temperature of 180-220℃ for 110-130 seconds, and then cooled to room temperature. S5: Lamination and lamination: Open windows in the protective membrane material, clean the membrane material after opening the windows, attach the membrane material to the top surface of the substrate, pre-position the membrane material, and then heat-melt it at a temperature of 170-180℃ for 5 seconds. Pre-press the pre-melted membrane material at a temperature of 120℃ for 15 seconds and a pressure of 560Pa. Then heat-press the pre-pressed membrane material at a temperature of 150℃ for 80 seconds and a pressure of 1120Pa. S6: Punching: The substrate coated in step S5 is sent to the punching equipment for punching.

[0010] As a further improvement to this design, a copper paste pre-baking process is also included between step S3 and step S4, in which the printed copper paste is heated to 80°C and pre-baked for 2-3 minutes.

[0011] As a further improvement to this design, a gold plating process is also included between steps S5 and S6, wherein the gold plating process is to plate gold on the solderable parts of the conductor layer corresponding to the window.

[0012] As a further improvement to this design, an SMT assembly step is provided after step S6, in which electronic components are soldered to the surface of the substrate processed in step S6 using SMT equipment, and the pins of the electronic components are soldered to the solderable parts of the conductor layer.

[0013] The beneficial effects of this invention are as follows: This invention utilizes low-temperature sintering printed copper paste to completely replace the production and processing of FCCL in the upstream manufacturing plant of FPC. This solution directly forms conductors on the PI film, resulting in lighter, thinner, foldable, and flexible circuit boards. The use of printed additive manufacturing completely avoids the wet chemical process, making it more environmentally friendly. The manufacturing cost is reduced by more than 40% compared to traditional processes, making it more competitive. The heat-shrinkable and stabilized substrate and protective layer are more resistant to high temperatures, enabling traditional SMT processes. Attached Figure Description

[0014] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0015] Figure 1 This is an exploded view of the flexible circuit board of the present invention.

[0016] In the diagram: 1. Substrate, 2. Adhesive layer, 3. Conductor layer, 4. Protective layer, 5. Window, 6. Gold plating layer. Detailed Implementation

[0017] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments. The illustrative embodiments and descriptions are only used to explain the present invention and are not intended to limit the present invention.

[0018] Example: An environmentally friendly solderable flexible circuit board includes a substrate 1, an adhesive layer 2 covering the top surface of the substrate 1, a conductor layer 3 printed on the top surface of the adhesive layer 2, and a protective layer 4 covering the top surface of the conductor layer 3. The adhesive layer 2 is used to increase the adhesion between the conductor layer 3 and the substrate 1. The conductor layer 3 is made of printed and sintered copper paste. The protective layer 4 is used to isolate the conductor layer 3 from the air. The substrate 1 is a PI film with good high temperature resistance, which is convenient for subsequent high-temperature SMT processes.

[0019] The substrate 1 layer is a heat-shrinkable PI film, and the thickness of the substrate 1 layer is not less than 12.5 μm. Since the minimum PI thickness of 12.5 μm has a DK value that meets the insulation performance requirements after FPC assembly, the substrate 1 layer is suitable.

[0020] The adhesive layer 2 is an ADH epoxy resin adhesive, and the copper paste is composed of copper powder mixed with epoxy resin. The ADH epoxy resin undergoes a cross-linking reaction with the epoxy resin in the copper paste, enhancing the adhesion between the copper paste and the substrate 1. During the cross-linking reaction, the epoxy resin in the copper paste migrates to the adhesive layer 2, causing the copper powder in the conductor layer 3 to move closer together and be densely packed.

[0021] The copper powder in the copper paste has a particle size of 1-10μm. The finer copper powder makes it easier for the copper powder in the sintered copper paste to be arranged tightly, thus reducing the resistance.

[0022] The protective layer 4 is a PI film, and the protective layer 4 has a window 5 located above the solderable position of the conductor layer 3. The top surface of the solderable position of the conductor layer 3 is provided with a gold-plated layer 6. The PI film provides better protection for the conductor layer 3.

[0023] An environmentally friendly method for manufacturing a solderable flexible circuit board includes the following steps: S1: Heat shrinking of substrate layer: The PI film substrate is baked at a temperature of 170℃-190℃ for 50-70 minutes. After baking, it is cooled, which can be done by air cooling to increase the cooling speed. After heat shrinking, the substrate is less likely to shrink during subsequent production. S2: Coating: Apply ADH epoxy resin adhesive to the top surface of the substrate treated in step S1, with a coating thickness of 13μm-15μm. Pre-bake the coated ADH epoxy resin adhesive for 18-20 minutes at a pre-baking temperature of 80℃. Place the pre-baked product into a curing device and maintain the curing device at 150℃ for 40 minutes. S3: Conductor layer printing: Print copper paste on the top surface of the substrate treated in step S2, and print the copper paste into the designed circuit shape. Control the thickness of the copper paste to 10-15μm to ensure good conductivity. S4: Copper paste sintering: After processing in step S3, the copper paste is laminated at a pressure of 1400 Pa and preheated under vacuum at a temperature of 75-85°C for 8-12 seconds. The preheated copper paste is then sintered under vacuum at a temperature of 180-220°C for 110-130 seconds. The entire process is carried out under vacuum, which can both defoam and reduce the oxidation of copper powder. After cooling to room temperature, the copper paste is laminated and heated to promote the migration of epoxy resin to ADH epoxy resin, increase cross-linking, and make the copper powder in the conductor layer more compact and have stronger adhesion. S5: Lamination and Pressing: Open windows in the protective film material, clean the film material after opening windows (using an ion blower and rubber rollers), attach the film material to the top surface of the substrate, pre-position the film material, and then heat-melt it at a temperature of 170-180℃ for 5 seconds. Pre-press the pre-melted film material at a temperature of 120℃ for 15 seconds and a pressure of 560Pa. Then, heat-press the pre-pressed film material at a temperature of 150℃ for 80 seconds and a pressure of 1120Pa. Heating and pressurizing reduce air bubbles under the protective layer and improve the adhesion of the protective layer. S6: Punching: The substrate coated in step S5 is sent to the punching equipment for punching.

[0024] Between steps S3 and S4, there is also a copper paste pre-baking process step, in which the printed copper paste is heated to 80°C and pre-baked for 2-3 minutes to reduce the adhesion of the surface copper paste pre-stacked board during copper paste sintering.

[0025] Between steps S5 and S6, a gold plating process is also included, in which the solderable parts of the conductor layer corresponding to window 5 are plated with gold to improve solderability.

[0026] After step S6, there is an SMT assembly step where electronic components are soldered onto the substrate surface processed in step S6 using SMT equipment. The pins of the electronic components are soldered to the solderable parts of the conductor layer, which improves production efficiency and is low-carbon and environmentally friendly.

[0027] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. An environmentally friendly, solderable flexible circuit board, characterized in that, The device includes a substrate, an adhesive layer covering the top surface of the substrate, a conductor layer printed on the top surface of the adhesive layer, and a protective layer covering the top surface of the conductor layer. The adhesive layer is used to increase the adhesion between the conductor layer and the substrate. The conductor layer is made of printed sintered copper paste. The protective layer is used to isolate the conductor layer from the air. The substrate layer is a PI film.

2. The environmentally friendly weldable flexible circuit board according to claim 1, characterized in that, The substrate layer is a heat-shrinkable PI film, and the substrate thickness is not less than 12.5 μm.

3. The environmentally friendly weldable flexible circuit board according to claim 1, characterized in that, The adhesive layer is an ADH epoxy resin adhesive, and the copper paste is composed of copper powder mixed with epoxy resin.

4. The environmentally friendly weldable flexible circuit board according to claim 3, characterized in that, The copper powder in the copper paste has a particle size of 1-10 μm.

5. The environmentally friendly weldable flexible circuit board according to claim 1, characterized in that, The protective layer is a PI film, and the protective layer has a window located above the solderable position of the conductor layer. The top surface of the solderable position of the conductor layer is provided with a gold plating layer.

6. A method for manufacturing an environmentally friendly weldable flexible circuit board, characterized in that, Includes the following steps: S1: Heat shrinking of substrate layer: Bake the PI film substrate at a temperature of 170℃-190℃ for 50-70 minutes, and then cool it after baking. S2: Coating: Apply ADH epoxy resin adhesive to the top surface of the substrate treated in step S1, with a coating thickness of 13μm-15μm. Pre-bake the coated ADH epoxy resin adhesive for 18-20 minutes at a pre-baking temperature of 80℃. Place the pre-baked product into a curing device and maintain the curing device at 150℃ for 40 minutes. S3: Conductor layer printing: Print copper paste on the top surface of the substrate treated in step S2, and print the copper paste into the designed circuit shape, controlling the copper paste thickness to be 10-15μm; pre-bake the printed copper paste at 80℃ for 2-3 minutes, and then cool it to room temperature; S4: Copper paste sintering: After processing in step S3, the plates are stacked and pressed together at a pressure of 1400Pa. The copper paste is vacuum preheated at a temperature of 75-85℃ for 8-12 seconds. The preheated copper paste is then vacuum sintered at a low temperature of 180-220℃ for 110-130 seconds, and then cooled to room temperature. S5: Lamination and lamination: Open windows in the protective membrane material, clean the membrane material after opening the windows, attach the membrane material to the top surface of the substrate, pre-position the membrane material, and then heat-melt it at a temperature of 170-180℃ for 5 seconds. Pre-press the pre-melted membrane material at a temperature of 120℃ for 15 seconds and a pressure of 560Pa. Then heat-press the pre-pressed membrane material at a temperature of 150℃ for 80 seconds and a pressure of 1120Pa. S6: Punching: The substrate coated in step S5 is sent to the punching equipment for punching.

7. The method for manufacturing an environmentally friendly weldable flexible circuit board according to claim 6, characterized in that, Between steps S3 and S4, there is also a copper paste pre-baking process step, in which the printed copper paste is heated to 80°C and pre-baked for 2-3 minutes.

8. The method for manufacturing an environmentally friendly weldable flexible circuit board according to claim 6, characterized in that, Between steps S5 and S6, a gold plating process is also included, in which the solderable portion of the conductor layer corresponding to the window is plated with gold.

9. A method for manufacturing an environmentally friendly weldable flexible circuit board according to claim 8, characterized in that, Between steps S6 and S5, there is an SMT assembly step where electronic components are soldered onto the substrate surface after step S5 using SMT equipment, and the pins of the electronic components are soldered to the solderable parts of the conductor layer.