A vertical deep ultraviolet LED with impedance matching

By optimizing the Al composition and structural design of the N-type semiconductor layer, and employing a combination of low-refractive-index thick layers and high-refractive-index thin layers, as well as a non-flat roughened surface, the problem of insufficient light extraction efficiency of vertical deep ultraviolet LEDs was solved, achieving efficient photoelectric impedance matching and high-power applications.

CN123076072APending Publication Date: 2026-11-10HUBEI YOUWEIXIN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611147706.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-30
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing vertical deep ultraviolet LEDs suffer from severe total internal reflection light loss due to interlayer refractive index mismatch, resulting in insufficient light extraction efficiency and failing to meet the needs of high-power applications.

Method used

By optimizing the Al composition and structural design of the N-type semiconductor layer, a combination of a low-refractive-index thick layer and a high-refractive-index thin layer is used, along with a roughened non-flat surface, to form a continuous refractive index gradient, reducing interface reflection and light absorption, and achieving photoelectric impedance matching.

Benefits of technology

It significantly improves the chip's light extraction efficiency and continuous light output power, adapting to the needs of high-power deep ultraviolet applications, while ensuring the reliability of high-current operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076072A_ABST
    Figure CN123076072A_ABST
Patent Text Reader

Abstract

This invention provides an impedance-matched vertical deep ultraviolet LED. By setting the first semiconductor layer near the light-emitting surface as a thick layer with low refractive index and the second semiconductor layer near the quantum well active layer as a thin layer with high refractive index, and combining it with a roughened surface with a peak-to-valley difference greater than 100 nm, a refractive index transition structure with a continuous increase from the air interface to the quantum well active layer is formed. This eliminates abrupt reflection loss between layers through the gradient refractive index design of the two semiconductor layers. Combined with the scattering effect of the roughened surface, large-angle light that was originally restricted by total internal reflection is converted into effective light that can be emitted normally, maximizing the anti-reflection advantage of the refractive index gradient. This enables impedance matching of the N-type semiconductor layer, and ultimately significantly reduces the total internal reflection light loss inside the device, effectively improving the light extraction efficiency and continuous emission power of the deep ultraviolet LED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronics, and more particularly to an impedance-matched vertical deep ultraviolet LED. Background Technology

[0002] Deep ultraviolet (DUV) light-emitting diodes (LEDs) have gradually replaced traditional mercury lamps as UV light sources in recent years due to their core advantages such as mercury-free environmental friendliness, compact size, fast response speed, and long lifespan. They have achieved large-scale applications in civilian fields such as surface disinfection, UV curing, and biochemical detection. With the continuous maturation of DUV chip technology, its application scope is rapidly expanding from low-power, small-scale static disinfection scenarios to high-end scenarios such as high-flow municipal water supply disinfection, medical high-purity water terminal treatment, deep purification of industrial wastewater, and large-space dynamic air disinfection. These scenarios generally require devices with higher continuous light output power, long-term operational reliability, and lower energy consumption per unit of light power. Light extraction efficiency, as the core factor determining the electro-optical conversion efficiency of DUV LEDs, directly determines the device's light output power and energy consumption level, thus placing extremely stringent requirements on the light extraction capabilities of vertical DUV LEDs.

[0003] Traditional in-cell / flip-chip deep ultraviolet (DUV) LEDs typically use heteroepitaxial sapphire substrates. However, due to the inherent insulating and low thermal conductivity of sapphire, these devices suffer from inherent defects such as vertical current blockage, long heat dissipation paths, and rapid junction temperature spikes under high current injection, making it difficult to meet the performance requirements of high-power applications. To overcome the performance bottleneck caused by the substrate, peeling off the back sapphire substrate and fabricating vertically structured DUV LEDs has become an industry-recognized technological direction for high-power devices. The vertical structure enables vertical current conduction, significantly shortening the heat dissipation path and structurally adapting to the long-term high-power operation requirements. However, existing vertical deep ultraviolet LEDs still have significant shortcomings in light extraction: On the one hand, high-Al-content P-type AlGaN materials are limited by the intrinsic characteristics of low Mg acceptor activation efficiency and poor hole mobility, resulting in insufficient lateral current expansion capability of the device. The current tends to concentrate in a local area directly below the electrode, causing problems such as current congestion, local hot spots, and uneven in-plane carrier injection. This not only increases the non-radiative recombination ratio but also causes poor in-plane light emission uniformity. On the other hand, the difference in Al composition between the N-type layer, quantum well, and P-type layer leads to a large refractive index difference. Light is prone to total internal reflection at the interlayer interface and is absorbed by the material and electrodes during repeated transmission within the device, making it difficult to emit effectively. This has become the core obstacle restricting further improvement in the light extraction efficiency of the device.

[0004] Current performance optimization solutions for vertical LEDs mostly follow the traditional current spreading layer design of flip chips, failing to fully consider the path characteristics of vertical current conduction and light extraction. These solutions generally suffer from problems such as strong deep-ultraviolet light absorption by the spreading layer material, large refractive index mismatch with adjacent layers, and numerous epitaxial lattice defects. This not only limits current spreading gain but also introduces additional interface reflection and light absorption losses, resulting in only a weak improvement in light extraction and failing to fully meet the high-performance requirements of vertical devices. As deep-ultraviolet LEDs increasingly target high-end applications such as high-flow-rate water treatment and large-space dynamic disinfection, the industry's requirements for device electro-optical conversion efficiency continue to rise. Fabricating vertical deep-ultraviolet LEDs by stripping sapphire substrates has become an inevitable technological route. Optimizing the interlayer refractive index characteristics of the vertical structure and further improving the chip's light extraction capability are currently core technical problems that urgently need to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to provide an impedance-matched vertical deep ultraviolet (DUV) LED to solve the technical problem of insufficient light extraction efficiency caused by severe total internal reflection light loss due to interlayer refractive index mismatch in existing vertical DUV LEDs. This invention achieves photoelectric impedance matching through Al composition and structural optimization of the N-type semiconductor layer, significantly improving chip light extraction efficiency while ensuring the reliability of high-current operation, thus meeting the requirements of high-power deep ultraviolet applications.

[0006] The technical solution provided by this invention specifically includes the following: The present invention provides an impedance-matched vertical deep ultraviolet LED, which comprises, from the top surface of the chip downwards, an N-type semiconductor layer, a quantum well active layer, a P-type semiconductor layer and a P-type contact layer; The vertical deep ultraviolet LED also has an insulating layer and an N-type contact layer that are in contact with the N-type semiconductor layer; a part of the insulating layer is located on the lower surface of the P-type contact layer, and another part is located outside the sidewall of the P-type contact layer to the quantum well active layer and is attached to the sidewall of each corresponding layer; a part of the N-type contact layer is located on the lower surface of the insulating layer, and another part is located outside the outer sidewall of the insulating layer and is attached to the outer sidewall of the insulating layer. The N-type semiconductor layer includes a first semiconductor layer and a second semiconductor layer from the top of the chip downwards. The refractive index of the first semiconductor layer is less than that of the second semiconductor layer, and the thickness of the first semiconductor layer is greater than that of the second semiconductor layer. The surface of the first semiconductor layer facing away from the second semiconductor layer is a non-flat surface, and the maximum peak-to-valley difference of the non-flat surface is >100nm.

[0007] Specifically, this invention first employs a material design with a lower refractive index and greater thickness for the first semiconductor layer near the light-emitting top surface of the chip. This effectively reduces the refractive index difference between the light-emitting semiconductor material and air, widening the critical light-emitting angle. Simultaneously, the non-smooth, roughened structure on the top surface of the first semiconductor layer, with a maximum peak-to-valley difference greater than 100 nm, breaks interface total internal reflection, providing sufficient scattering transmission paths for light propagating at large angles, scattering light originally limited by total internal reflection into light capable of being emitted at small angles. Furthermore, the second semiconductor layer located below the first semiconductor layer employs a higher refractive index design, forming a continuous refractive index gradient with the first semiconductor layer. The transition between the two layers achieves optical impedance matching by progressively decreasing refractive index from the quantum well's light-emitting side to the N-type light-emitting surface. This avoids interface reflection within the N-type semiconductor layer and reduces the probability of light being ineffectively absorbed by the P-type semiconductor layer material during round-trip transmission within the device. Furthermore, the invention utilizes a vertical structure design between the bonded insulating layer and the N-type contact layer to ensure uniform longitudinal current expansion without introducing an additional high-absorption current extension layer. This significantly reduces total internal reflection light loss, greatly improves chip light extraction efficiency and continuous light output power, while also ensuring long-term operational reliability under high current injection, thus meeting the requirements of high-power deep ultraviolet applications.

[0008] More preferably, both the insulating layer and the N-type contact layer are in contact with the lower surface of the N-type semiconductor layer; or, both the insulating layer and the N-type contact layer penetrate a portion of the thickness of the N-type semiconductor layer and are in contact with it.

[0009] Specifically, the solution where both the insulating layer and the N-type contact layer are in contact with the lower surface of the N-type semiconductor layer does not require etching of the N-type semiconductor layer, thus avoiding etching damage, simplifying the process and increasing yield. The solution that embeds part of the thickness of the N-type semiconductor layer can shorten the lateral current transport distance of the high-resistivity N-type AlGaN and further improve the current uniformity within the active layer of the quantum well.

[0010] Preferably, the first semiconductor layer is a single layer of Al with a constant Al composition. a Ga 1-a The structure is N-type with a thickness of 500–8000 nm, and the Al component a is a constant value with parameters satisfying 40% ≤ a ≤ 100%.

[0011] Specifically, a monolayer of Al with a constant Al composition. a Ga 1-a With fewer defects and a clearer interface, the N-structure can stably achieve refractive index matching with the second semiconductor layer, resulting in high epitaxial yield. The 40%–100% Al composition ensures the material's low refractive index and high transparency in deep ultraviolet light, reducing the refractive index difference between the light-emitting surface and air, and minimizing self-absorption. The thickness of 500–8000 nm provides sufficient process windows and light scattering paths for surface roughening, avoiding stress and additional absorption caused by excessive thickness, fully leveraging the roughening effect to break total internal reflection, and stably improving light extraction efficiency.

[0012] Preferably, the first semiconductor layer is a single layer of Al with non-constant Al composition. b Ga 1-b The structure is an N-structure with a thickness of 1–1000 nm. Its Al composition b decreases linearly from b1 to b2 along the stacking direction from the top surface of the chip downwards. The parameters satisfy 60% ≤ b1 ≤ 100% and 40% ≤ b2 ≤ 80%.

[0013] Specifically, this preferred design can form a continuous refractive index gradient between air and the second semiconductor layer without the need for a multi-layer structure, eliminating Fresnel reflection at abrupt interfaces and achieving smoother optical impedance matching. The top surface of the first semiconductor layer maintains the advantage of a low refractive index difference with air, and the refractive index of the bottom surface of the first semiconductor layer is naturally connected to that of the second semiconductor layer. This does not increase the difficulty of material absorption and roughening processes, and can further reduce interlayer reflection loss and improve light extraction efficiency.

[0014] Preferably, the first semiconductor layer is Si-doped or unintentionally doped, with the Si doping concentration being 1E17 to 1E20 cm⁻¹. -3 .

[0015] Specifically, the aforementioned Si doping concentration range ensures the conductivity of the N-type semiconductor layer, improves longitudinal current spread, alleviates current congestion, and avoids severe free carrier absorption introduced by excessive doping. The unintentional doping mode results in fewer material defects and higher deep ultraviolet transmittance, allowing for flexible selection based on device performance requirements. In summary, neither of these doping modes disrupts the interlayer refractive index matching design and surface roughening effect, ensuring device electrical reliability without adding additional optical loss.

[0016] Preferably, the second semiconductor layer is a Si-doped monolayer Al. c Ga 1-c The structure is an N-structure with a thickness of 1–1000 nm and a Si doping concentration of 1E17–1E20 cm⁻¹. -3 ; Wherein, the Al component c of the second semiconductor layer is a constant value and the parameter satisfies 30%≤a≤80%; or, the Al component c of the second semiconductor layer is a non-constant value and decreases linearly from c1 to c2 along the stacking direction from the top surface of the chip downward; wherein the parameter satisfies 50%≤c1≤80% and 30%≤c2≤60%.

[0017] Specifically, thin monolayer structures of 1–1000 nm can minimize the intrinsic absorption of deep ultraviolet light by AlGaN materials, combined with 1E17–1E20 cm⁻¹ -3 The Si doping concentration can compensate for the insufficient conductivity of the first semiconductor layer with high Al composition, optimize the vertical current distribution, and avoid current congestion and local hot spots.

[0018] For different structures of the first semiconductor layer, the Al composition of the second semiconductor layer is designed to be matched: when the first semiconductor layer is a constant Al composition structure, the second semiconductor layer adopts a constant Al composition scheme, the refractive index difference between the two layers is precisely controllable, the interface is clear without additional defects, the epitaxial process is simple and has good mass production performance, and stable stepped optical impedance matching can be achieved; when the first semiconductor layer is a gradient Al composition structure, the second semiconductor layer adopts a linear gradient Al composition scheme in the same direction, which together with the upper layer forms a continuous refractive index gradient from the light-emitting surface to the inside of the device, completely eliminating Fresnel reflection at the abrupt interface between layers, and achieving smoother end-to-end optical matching.

[0019] Preferably, the N-type semiconductor layer further includes a third semiconductor layer located between the second semiconductor layer and the quantum well active layer, and both the insulating layer and the N-type contact layer are in contact with the lower surface of the third semiconductor layer; The third semiconductor layer is a single layer of Al with non-constant Al composition. e Ga 1-e In the N-structure, the Al composition of the second semiconductor layer near the third semiconductor layer is e1, and the Al composition of the quantum well active layer near the third semiconductor layer is e2. The Al composition e of the third semiconductor layer changes linearly from e1 to e2 along the stacking direction from the top of the chip downwards.

[0020] Specifically, the design that both the insulating layer and the N-type contact layer are in contact with the lower surface of the third semiconductor layer allows the N-type electrode to be located completely behind the light-emitting surface. This avoids blocking the light emission from the top surface and damaging the roughened structure of the first semiconductor layer, thus maximizing the light extraction efficiency. It also allows the etching depth to be controlled to the shallowest possible depth, requiring only the removal of the edge P-type semiconductor layer and the quantum well active layer to expose the contact surface without damaging the upper N-type epitaxial layer, resulting in a low risk of leakage. The linear gradient of the Al composition in the third semiconductor layer can eliminate the abrupt change in refractive index between the second semiconductor layer and the quantum well active layer, forming a continuous refractive index gradient across the entire chain with the first and second semiconductor layers. This reduces interface reflection loss and balances low contact resistance with high light extraction efficiency.

[0021] Preferably, the N-type semiconductor layer further includes a fourth semiconductor layer located between the first semiconductor layer and the second semiconductor layer, wherein the fourth semiconductor layer is a monolayer Al with non-constant Al composition. f Ga 1-f N-structure; The Al composition of the first semiconductor layer near the fourth semiconductor layer is f1, and the Al composition of the second semiconductor layer near the fourth semiconductor layer is f2. The Al composition f of the fourth semiconductor layer changes linearly from f1 to f2 along the stacking direction from the top of the chip downwards.

[0022] Specifically, the fourth semiconductor layer is a refractive index transition layer between the first and second semiconductor layers. It adopts a single-layer linearly graded Al composition design, and the Al composition at both ends is perfectly matched with the adjacent layers. This eliminates the abrupt refractive index change and Fresnel reflection caused by the difference in Al composition between the two layers, making the refractive index gradient from the light-emitting surface to the quantum well active layer more continuous and smooth, reducing the round-trip reflection and ineffective absorption of light inside the N-type semiconductor layer; at the same time, the single-layer Al... f Ga 1-f The N-structure has no additional heterogeneous interface defects, does not introduce additional resistance and optical loss, further optimizes the impedance matching effect of the entire link, and improves the light extraction efficiency.

[0023] Preferably, both the first semiconductor layer and the second semiconductor layer are single-layer Al. d Ga 1-d N-structure; the average Al composition of the first semiconductor layer is d1, the average Al composition of the second semiconductor layer is d2, and d1 - d2 ≥ 3%.

[0024] Specifically, both the first semiconductor layer and the second semiconductor layer are made of single-layer Al. d Ga 1-d The N-structure has fewer epitaxial defects and lower deep ultraviolet light absorption. By controlling the average Al composition difference between the two layers to d1-d2≥3%, a stable and controllable refractive index difference can be formed: the first semiconductor layer with high Al and low refractive index is close to the light-emitting surface to reduce the refractive index difference with air, while the second semiconductor layer with low Al and high refractive index is close to the inside of the device to connect with subsequent functional layers. This avoids insufficient refractive index difference and weak total internal reflection suppression due to too small a composition difference, and also avoids lattice mismatch defects and strong interface reflection due to too large a composition difference. It provides a stable basic stepped structure for refractive index matching throughout the entire process and effectively reduces total internal reflection loss on the light-emitting side.

[0025] Preferably, the N-type semiconductor layer further includes a fifth semiconductor layer located between the first semiconductor layer and the second semiconductor layer. The fifth semiconductor layer includes a first sub-layer and a second sub-layer sequentially from the top surface of the chip downwards. The first sub-layer is a single layer of Al. x Ga 1-x The N-structure has a second sublayer that is a single layer of Al. y Ga 1-y N structure; x=d1±10%, y=d2±10% and x>y.

[0026] Specifically, the fifth semiconductor layer is a mass-production-friendly stepped transition structure between the first and second semiconductor layers. Its Al composition deviation is controlled within ±10%. By setting x>y, two levels of refractive index steps are formed, which can significantly reduce the abrupt interface reflection between the two layers. Moreover, the fifth semiconductor layer does not require continuous control of Al composition, which makes epitaxial control easier, the process window wider, and the yield higher. The two single-layer sublayers have no additional heterogeneous defects and do not increase light absorption or series resistance. It achieves a refractive index matching effect close to that of a continuous gradient layer with lower process cost.

[0027] Preferably, the vertical deep ultraviolet LED further includes an N-type electrode, a P-type electrode, and a supporting substrate; the N-type electrode is disposed on the lower surface of the N-type contact layer; the P-type electrode is disposed on the sidewall of the P-type contact layer that is not covered by the insulating layer, and is attached to the sidewall; the supporting substrate is disposed on the lower surface of the N-type electrode.

[0028] Specifically, compared to the problems of traditional vertical P-side electrodes blocking light emission and poor heat dissipation paths, this preferred solution places the P-type electrode on the exposed sidewall of the P-type contact layer, which can increase the effective light emission area; the N-type electrode is placed on the lower surface of the N-type contact layer and combined with a high thermal conductivity support substrate, which not only ensures that the N-type electrode has sufficient contact area to reduce resistance, but also allows the heat generated by the device to be quickly dissipated through the support substrate, making it more suitable for high-end application scenarios with high-power continuous operation.

[0029] The beneficial effects of this invention are as follows: Unlike existing technologies, this invention provides an impedance-matched vertical deep ultraviolet LED. This invention sets the first semiconductor layer near the light-emitting surface as a thick layer with a low refractive index, while setting the second semiconductor layer near the quantum well active layer as a thin layer with a high refractive index. Combined with a roughened surface on the top surface of the first semiconductor layer with a peak-to-valley difference greater than 100 nm, a continuously increasing refractive index transition structure is formed from the air interface to the quantum well active layer. This gradient refractive index design of the two semiconductor layers eliminates abrupt reflection losses between layers. Furthermore, the scattering effect of the roughened surface converts large-angle light rays that were originally limited by total internal reflection into effective light rays that can be emitted normally, maximizing the anti-reflection advantage of the refractive index gradient. This allows the N-type semiconductor layer to achieve impedance matching without the need for additional heterogeneous anti-reflection films, avoiding the introduction of additional interface reflection and deep ultraviolet light absorption losses. Ultimately, this significantly reduces the total internal reflection light loss within the device, effectively improving the light extraction efficiency and continuous emission power of the deep ultraviolet LED. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the cross-sectional structure of the vertical deep ultraviolet LED provided in Embodiment 1; In the accompanying drawings: 101—N-type semiconductor layer; 1011—first semiconductor layer; 1012—second semiconductor layer; 102—quantum well active layer; 103—P-type semiconductor layer; 104—P-type contact layer; 105—insulating layer; 106—N-type contact layer; 107—N-type electrode; 108—supporting substrate. Detailed Implementation

[0031] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0032] To address the problems of existing technologies, this invention, based on the basic architecture of vertical deep ultraviolet LEDs, specifically designs an extended enhancement structure that is more adapted to the current transmission path of vertical chips. Through the synergistic optimization of Al composition gradient and doping concentration distribution, it enhances the lateral current expansion capability of the P-type doped region, improves the in-plane uniformity of carrier injection, and ultimately achieves an effective improvement in the luminous efficiency of deep ultraviolet LEDs, providing a feasible technical solution for the large-scale deployment of high-power deep ultraviolet devices in high-end disinfection and other scenarios.

[0033] The technical solution of this application will now be described in conjunction with specific embodiments.

[0034] Example 1 (including a double-layer AlGaN impedance matching structure): Please see Figure 1 , Figure 1 This is a schematic diagram of the cross-sectional structure of the vertical deep ultraviolet LED 100 provided in this embodiment 1; wherein, this embodiment 1 provides an impedance-matched vertical deep ultraviolet LED 100, which includes, from the top surface of the chip downwards, an N-type semiconductor layer 101, a quantum well active layer 102, a P-type semiconductor layer 103 and a P-type contact layer 104. Specifically, the vertical deep ultraviolet LED 100 is further provided with an insulating layer 105 and an N-type contact layer 106 that are in contact with the lower surface of the N-type semiconductor layer 101; a portion of the insulating layer 105 is disposed on the lower surface of the P-type contact layer 104, and another portion is located outside the sidewall of the P-type contact layer 104 to the quantum well active layer 102 on the same side and is attached to the sidewall of each corresponding layer; a portion of the N-type contact layer 106 is disposed on the lower surface of the insulating layer 105, and another portion is located outside the outer sidewall of the insulating layer 105 and is attached to the outer sidewall of the insulating layer 105.

[0035] In Example 1, the N-type semiconductor layer 101 includes a first semiconductor layer and a second semiconductor layer sequentially from the top surface of the chip downwards. The refractive index of the first semiconductor layer is less than that of the second semiconductor layer, and the thickness of the first semiconductor layer is greater than that of the second semiconductor layer. The N-type semiconductor layer 101 is epitaxially grown by metal-organic chemical vapor deposition (MOCVD) technology.

[0036] Specifically, the first semiconductor layer is a single layer of Al with a constant Al composition. 0.65 Ga 0.35 The structure is an N-type structure with a thickness of 3000 nm and a refractive index of approximately 2.26. The surface of the first semiconductor layer facing away from the second semiconductor layer is a non-flat surface with a maximum peak-to-valley difference of 500 nm.

[0037] Specifically, the second semiconductor layer is a single layer of Al doped with Si and having a constant Al composition. 0.6 Ga 0.4 The structure is an N-structure with a thickness of 500 nm and a Si doping concentration of 5E18cm⁻¹. -3 Its refractive index is approximately 2.28.

[0038] In this embodiment 1, the quantum well active layer 102 is located on the lower surface of the N-type semiconductor layer 101 and consists of 2 to 20 cycles of AlGaN quantum well / quantum barrier structures (5 cycles in this embodiment 1). The thickness of the AlGaN quantum well is 0.1 to 5 nm (approximately 3 nm in this embodiment 1), and the Al content is 0 to 80% (55% in this embodiment 1); the thickness of the AlGaN quantum barrier is 5 to 30 nm (approximately 10 nm in this embodiment 1), and the Al content is 20% to 100% (60% in this embodiment 1). By adjusting the mass percentage of Al content in the AlGaN quantum well, deep ultraviolet light emission in the 200 to 310 nm wavelength band can be achieved (the emission wavelength in this embodiment 1 is 275 nm).

[0039] In this embodiment 1, the P-type semiconductor layer 103 is located on the lower surface of the quantum well active layer 102. It is a P-type doped AlGaN layer, and its Al composition is typically lower than that of the quantum barrier. The thickness is 1–50 nm (approximately 50 nm in this embodiment 1). The P-type semiconductor layer 103 is also epitaxially grown using MOCVD technology, and the doping element is Mg with a doping concentration of 1 × 10⁻⁶. 18 ~1×10 19 cm -3 (This Example 1 is approximately 2 × 10) 18 cm -3 ).

[0040] In this embodiment 1, a P-type contact layer 104 is formed on the lower surface of the P-type semiconductor layer 103 to achieve good ohmic contact between the P-type semiconductor layer 103 and the external electrode. The material of the P-type contact layer 104 is selected from at least one of Rh, Ru, Pd, Ir, Al, Ni, Ti, Au, and Ag, and can be a single-layer structure or a multi-layer stacked structure, with a thickness of 5–70 nm (in this embodiment 1, a single-layer Rh structure with a thickness of approximately 30 nm is used). The Rh material has high reflectivity to deep ultraviolet light and can form good ohmic contact with the extended enhancement layer 104.

[0041] In this embodiment 1, the insulating layer 105 is used to isolate the P-type contact layer 104 and the N-type contact layer 106 to prevent short circuits between different metals. The material of the insulating layer 105 is selected from insulating dielectric materials such as silicon dioxide (SiO2) and silicon nitride (Si3N4), and the thickness is 50-2000nm (SiO2 is used in this embodiment 1, and the thickness is about 300nm).

[0042] In this embodiment 1, the material of the N-type contact layer 106 is selected from at least one of Cr, Al, Ti, Ni, and Au, and can be a single-layer structure or a multi-layer stacked structure, with a depth of 50 to 4000 nm (approximately 1 μm in this embodiment 1); in this embodiment 1, the N-type contact layer 106 adopts a Cr / Al / Ti / Au stacked structure, with a total thickness of 50 to 4000 nm (approximately 500 nm in this embodiment 1).

[0043] In this embodiment 1, the N-type electrode 107107 is formed below the N-type contact layer 106 and serves as the negative electrode of the chip. From top to bottom, it includes a reflective layer and a bonding layer. On the back side of the bonding layer away from the reflective layer, a support substrate 108 and a welding metal layer are disposed sequentially.

[0044] Specifically, the reflective layer is composed of a metallic material capable of reflecting deep ultraviolet light with wavelengths of 200–310 nm. The metallic material is selected from at least one of Rh, Ru, Pd, Ir, Al, Ni, Ti, Au, and Ag, and its thickness is 10–500 nm. The function of the reflective layer is to reflect downward-propagating light and lateral-propagating light from inside the chip back to the light-emitting surface, thereby improving light extraction efficiency. In this embodiment 1, the reflective layer adopts an Rh / Al stacked structure, wherein the Rh layer is approximately 50 nm thick and the Al layer is approximately 200 nm thick. Rh contacts the N-type contact layer 106, forming a good ohmic contact; the Al layer has a high reflectivity for deep ultraviolet light, effectively reflecting the light inside the chip.

[0045] Specifically, a bonding layer is formed between the reflective layer and the support substrate 108 to achieve bonding between the epitaxial wafer and the support substrate 108. The material of the bonding layer is selected from at least one of Cr, Ni, Pt, Ti, Au, Sn, Cu, Ag, and Ta, with Au-Sn alloy being preferred, and the thickness is 100–3000 nm (in this embodiment 1, Au-Sn alloy is used, with a thickness of approximately 1000 nm).

[0046] Specifically, the support substrate 108 is used to support the chip and conduct current. The material can be a doped semiconductor material (such as an N-type or P-type Si substrate) or a metal substrate with a thickness of 100 to 2000 μm (in this embodiment 1, an N-type Si substrate with a thickness of about 300 μm is used).

[0047] Specifically, a welding metal layer is formed on the lower surface of the support substrate 108 as the outermost layer of the support substrate 108 for subsequent welding or bonding. The material is usually Au, and the thickness is 1 to 5 μm (approximately 2 μm in this embodiment 1).

[0048] In this embodiment 1, as the positive electrode of the chip, the P-type electrode is disposed on the sidewall of the N-type contact layer 106 that is not covered by the insulating layer 105, and is attached to the sidewall; the P-type electrode is made of Au, with a thickness of 1 to 4 μm (2 μm in this embodiment 1).

[0049] In this embodiment 1, the fabrication method of the vertical deep ultraviolet LED 100 includes the following steps: Step (1) Surface Cleaning: The epitaxial wafer is placed in a cleaning basket and ultrasonically cleaned sequentially with acetone, isopropanol, and SPM solution to remove organic impurities from the surface of the epitaxial wafer; then rinsed with deionized water for 5 minutes to ensure no residual reagents remain on the surface; finally, it is placed in a spin dryer to obtain a clean epitaxial wafer. The epitaxial wafer, from bottom to top, comprises a sapphire substrate, an AlN intrinsic layer, a sacrificial layer, an N-type semiconductor layer 101, a quantum well active layer 102, and a P-type semiconductor layer 103, and is epitaxially grown using MOCVD technology. The SPM solution is a mixture of concentrated sulfuric acid and hydrogen peroxide, with a mixing ratio typically between 3:1 and 7:1 (4:1 in Example 1), which effectively removes organic matter and metallic impurities from the surface.

[0050] Specifically, the aforementioned MOCVD technology is mainly implemented in a Veeco K465i MOCVD equipment. High-purity H2, high-purity N2, or a mixture of high-purity H2 and high-purity N2 are used as the carrier gas, high-purity NH3 as the N source, trimethylgallium (TMGa) as the gallium source, trimethylindium (TMIn) as the indium source, silane (SiH4) as the N-type dopant, and magnesia dichotoma (CP2Mg) as the P-type dopant. The pressure in the reaction chamber of the MOCVD equipment is controlled between 20 and 100 torr.

[0051] Specifically, the epitaxial growth steps of the epitaxial wafer with the extended reinforcement layer 104 are as follows: Step (1.1): Place the sapphire substrate in the MOCVD equipment and grow an AlN low-temperature buffer layer on the sapphire substrate at 400℃~800℃ (800℃ in this embodiment 1), with a thickness of 10~50nm (50nm in this embodiment 1).

[0052] Step (1.2): Heat to 1200-1400℃ (1200℃ in this example 1) to grow an intrinsic AlN layer with a thickness of 500-4000nm (2000nm in this example 1).

[0053] Step (1.3): Cool down to 600℃~1100℃ (1100℃ in this example 1) and grow a sacrificial layer. The sacrificial layer is a single layer or multiple layers of AlGaN or GaN (AlGaN in this example 1); wherein, the Al composition of the sacrificial layer is 1%~95% (60% in this example 1) and the thickness is 1~100nm (100nm in this example 1).

[0054] Step (1.4): Cool down to 800-1200℃ (1000℃ in this embodiment 1) and grow an N-type semiconductor layer 101 (including a first semiconductor layer and a second semiconductor layer); wherein, the first semiconductor layer is a monolayer Al with a constant Al composition. 0.65 Ga 0.35 The structure is an N-type structure with a thickness of 3000 nm and a refractive index of approximately 2.26; the second semiconductor layer is a single layer of Al doped with Si and having a constant Al composition. 0.6 Ga 0.4 The structure is an N-structure with a thickness of 500 nm and a Si doping concentration of 5E18cm⁻¹. -3 Its refractive index is approximately 2.28.

[0055] Step (1.5): Cool down to 700℃~1100℃ (900℃ in this example 1) to grow a quantum well active layer 102, which consists of 5 periods of AlGaN quantum well / quantum barrier structure: the thickness of AlGaN quantum well is 3nm and the Al composition is 55%; the thickness of AlGaN quantum barrier is 10nm and the Al composition is 60%.

[0056] Step (1.6): Maintaining a constant temperature of 900℃, grow a P-type semiconductor layer 103, which is made of Mg-doped AlGaN with an Al composition of 55%, a thickness of 50 nm, and a Si doping concentration of 2 × 10⁻⁶. 18 cm -3 .

[0057] Step (2) Preparation of P-type contact layer 104: Using electron beam evaporation or sputtering technology, a P-type contact layer 104 is prepared on the surface of the extended reinforcement layer 104 away from the P-type semiconductor layer 103. The material includes, but is not limited to, single or stacked layers of Rh, Ru, Pd, Ir, Al, Ni, Ti, Au, Ag, etc., with a thickness of 5 to 70 nm (in this embodiment 1, a single Rh structure with a thickness of 30 nm is used), and the evaporation / sputtering rate is 0.1 to 10 nm / s (in this embodiment 1, the evaporation rate is 0.5 nm / s).

[0058] Step (3) Mesa fabrication: Positive photoresist is spin-coated onto the surface of the P-type contact layer 104 away from the extended reinforcement layer 104 at a spin speed of 3000-5000 r / min (4000 r / min in Example 1) for 30 s. The photoresist is then baked at 100°C for 30 s to cure. The photoresist is patterned using photolithography and developed with a developer to obtain a photoresist mask that matches the structure of the subsequent insulating layer 105. Using the patterned photoresist as a mask, inductively coupled plasma (ICP) is used to etch the surface of the P-type contact layer 104 away from the extended reinforcement layer 104, resulting in a mesa structure exposing part of the lower surface of the N-type semiconductor layer 101. After etching, the photoresist mask is removed to obtain an epitaxial wafer with a stepped structure; wherein the N-type semiconductor layer 101 and the quantum well active layer 102 form the aforementioned stepped structure.

[0059] Step (4) Preparation of insulating layer 105: Plasma-enhanced chemical vapor deposition (PECVD) is used to deposit an insulating layer 105 on the entire surface of the epitaxial wafer with a stepped structure. Part of the insulating layer 105 is located on the lower surface of the P-type contact layer 104, and another part is located outside the sidewall of the P-type contact layer 104 to the quantum well active layer 102 and is attached to the corresponding sidewall of each layer. The insulating layer 105 is made of SiO2 with a thickness of 300 nm. The deposition temperature is 200-400℃ (300℃ in this example 1) and the deposition pressure is 1-5 Pa (3 Pa in this example 1) to ensure that the insulating layer 105 is uniformly covered and free from defects such as pinholes and cracks.

[0060] Step (5) Preparation of N-type contact layer 106: An N-type contact layer 106 is prepared on the lower surface of insulating layer 105 using electron beam evaporation or sputtering technology. A portion of the N-type contact layer 106 is disposed on the lower surface of insulating layer 105, and another portion is located outside the outer wall of insulating layer 105 and adheres to the outer wall of insulating layer 105. The material of N-type contact layer 106 includes, but is not limited to, single or stacked layers of Cr, Al, Ti, Ni, Au, etc., with a thickness of 50-4000 nm (in Example 1, a Cr / Al / Ti / Au stacked structure with a total thickness of 500 nm) and an evaporation / sputtering rate of 0.1-10 nm / s (in Example 1, the evaporation rate is 1 nm / s). After preparation, rapid annealing is performed in an N2 atmosphere at a temperature of 500-1300℃ (800℃ in Example 1), an annealing time of 10 min, and an annealing rate of 150℃ / min. Rapid annealing can promote interdiffusion between metal and semiconductor, form good ohmic contact, reduce contact resistance, and improve the electrical performance of the device.

[0061] Step (7) Preparation of the reflective layer: An electron beam evaporation or sputtering technique is used to prepare a reflective layer on the lower surface of the N-type contact layer 106. The material includes, but is not limited to, single or stacked layers of Rh, Al, Ag, Cr, Ti, Pt, Pd, Au, Ni, etc. Materials with high reflectivity for deep ultraviolet light of 200-320 nm (such as Rh and Al) are preferred. The thickness is 10-500 nm (in this embodiment 1, an Rh / Al stacked structure is used, with the Rh layer at 50 nm and the Al layer at 200 nm). The evaporation / sputtering rate is 0.2-20 nm / s (in this embodiment 1, the evaporation rate is 1 nm / s). The reflective layer makes good contact with the N-type contact layer 106, which can reflect the side light and reverse light inside the chip to the light-emitting surface, thereby improving the light extraction efficiency.

[0062] Step (8) Preparation of the bonding layer: A bonding layer is prepared simultaneously on the surface of the reflective layer and the surface of the support substrate 108 containing the welding metal layer using electron beam evaporation or sputtering technology. The material mainly includes at least one of Cr, Ni, Pt, Ti, Au, Sn, Cu, Ag, and Ta, with Au-Sn alloy preferred. The thickness is 100-3000 nm (Au-Sn alloy with a thickness of 1000 nm is used in Example 1), and the evaporation / sputtering rate is 0.1-5 nm / s (evaporation rate of 0.5 nm / s in Example 1). The support substrate 108 can be a doped semiconductor material (such as an N-type or P-type Si substrate) or a metal substrate. The thickness of the support substrate 108 is 100-2000 μm (N-type Si substrate with a thickness of 300 μm is used in Example 1) to support the chip and conduct current.

[0063] Step (9) Substrate stripping: Align the epitaxial chip with the bonding layer to the support substrate 108, and bond it in a vacuum environment at a temperature of 100-500℃ and a pressure of 1-5MPa (bonding in Example 1 was performed at 300℃ and 3MPa). The bonding time is 10-120min (60min in Example 1) to ensure a strong bond and no bubbles. After bonding, use a high-selectivity wet etching technique to remove the sacrificial layer in the epitaxial structure. Based on the separation interface released by the etching of the sacrificial layer, peel off the sapphire substrate, AlN low-temperature buffer layer, and AlN intrinsic layer used for epitaxial growth, exposing the surface of the N-type AlGaN layer. The etching solution used for wet etching is a mixture of hydrofluoric acid and nitric acid, the etching temperature is 10-150℃, and the etching time is 5-60min. After stripping, rinse thoroughly with deionized water and spin dry.

[0064] Step (10) Surface roughening: The roughening area is defined by a photolithography mask. The top surface of the N-type semiconductor layer 101 is roughened by Ar ion etching or wet etching to make the surface of the first semiconductor layer facing away from the second semiconductor layer a non-flat surface with a maximum peak-to-valley difference of 500 nm, thereby further improving the light extraction efficiency. The roughening parameters are as follows: If Ar ion etching is used, the etching power is 100-500 W (300 W in this example 1), and the etching time is 5-10 min (10 min in this example 1); if wet etching is used, KOH solution is used with a concentration of 5%-10%, the etching temperature is 20-100℃, and the etching time is 5-15 min. After roughening, the maximum peak-to-valley difference is controlled at 100-2000 nm (approximately 500 nm in this example 1), and then rinsed with deionized water and dried.

[0065] Step (11) Fabrication of the P-type electrode: Using negative photoresist photolithography, a P-pad pattern is defined at the N-side via (corresponding to the sidewall of the P-type contact layer 104 and N-type contact layer 106 not covered by the insulating layer 105). Negative photoresist is spin-coated at a speed of 3000–4000 r / min (3500 r / min in Example 1). After baking, exposure and development are performed to obtain the pad mask. An electron beam evaporation technique is used to deposit the P-type electrode at the mask window. Au is selected as the material, with a thickness of 1–4 μm (2 μm in Example 1), and an evaporation rate of 0.1–1 nm / s (0.5 nm / s in Example 1). After deposition, the photoresist mask is removed to obtain the P-type electrode.

[0066] Step (12) Chip dicing and testing: The prepared chip wafer is diced into individual chips using a dicing machine. The dicing width is 20-100μm (50μm in Example 1). After dicing, the individual chips are tested for electrical performance, optical performance and reliability. If the test is qualified, it is the finished vertical deep ultraviolet LED100 chip.

[0067] Comparative Example 1 (excluding the double-layer AlGaN impedance matching structure): Comparative Example 1 provides a vertical deep ultraviolet LED 100 without a double-layer AlGaN impedance matching structure. Its specific structural parameters and preparation method are largely the same as those of Example 1, except that the specific parameters of the N-type semiconductor layer 101 in Comparative Example 1 are set as follows: the N-type semiconductor layer 101 is a single layer of Al doped with Si. 0.6 Ga 0.45 N, thickness is 3000 nm, Si dopant element is 5E18cm -3 .

[0068] Comparative Example 2 (Traditional standard deep ultraviolet LED): Comparative Example 2 uses a standard, mass-produced, front-mounted deep ultraviolet LED structure, without sapphire substrate bonding and removal, and omits the impedance matching structure, insulating layer 105, vertical structure covering electrode, and back reflective structure proposed in this invention. To ensure the rigor of the single-variable comparison, except for the aforementioned structural differences, the entire process parameters of Comparative Example 2 from epitaxial growth to electrode fabrication are consistent with Comparative Example 1: all epitaxial layer material systems, Al composition, doping concentration, quantum well structure, and metal system are exactly the same. The only omissions in the fabrication process are the fabrication steps of insulating layer 105, back reflective layer, bonding layer, supporting substrate 108, and back welding metal. Substrate removal, N-plane roughening, and sidewall electrode-related processes are not performed. The remaining operating parameters, such as cleaning, thin film deposition, and rapid annealing, are matched with Comparative Example 1.

[0069] Results and Analysis: The samples from Examples 1 and Comparative Examples 1-2 were tested for optical power and voltage at 100mA. The test results are shown in the table below: Table 1. Test results of Example 1 and Comparative Examples 1-2

[0070] As shown in Table 1, the performance test results at an injection current of 100mA indicate that, compared to Comparative Example 1, which has the same vertical architecture but lacks a double-layer AlGaN impedance matching structure, Example 1, employing a double-layer AlGaN impedance matching structure, achieves an optical power of 86.6mW at 100mA, an increase of approximately 10.5% compared to Comparative Example 1, while reducing the operating voltage to 5.54V. Compared to Comparative Example 2, which lacks an impedance matching structure and uses a conventional upright mounting structure, Example 1 shows an optical power increase of approximately 48.5% and a reduction in operating voltage of 0.2V. These test results verify that the refractive index matching design of the N-type semiconductor layer 101 in this invention can effectively reduce interlayer total internal reflection loss and decrease N-type contact resistance, thereby significantly improving the device's light output performance while increasing optical output power.

[0071] It should be noted that all the above embodiments belong to the same inventive concept, and the descriptions of each embodiment have different focuses. Where the description in a particular embodiment is not detailed, please refer to the description in other embodiments.

[0072] The above embodiments merely illustrate implementation methods of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. An impedance-matched vertical deep ultraviolet LED, characterized in that, From top to bottom, the chip consists of an N-type semiconductor layer, a quantum well active layer, a P-type semiconductor layer, and a P-type contact layer. The vertical deep ultraviolet LED is further provided with an insulating layer and an N-type contact layer that are in contact with the N-type semiconductor layer; a portion of the insulating layer is disposed on the lower surface of the P-type contact layer, and another portion is located outside the sidewall of the P-type contact layer to the quantum well active layer and is attached to the corresponding sidewall of each layer; a portion of the N-type contact layer is disposed on the lower surface of the insulating layer, and another portion is located outside the outer sidewall of the insulating layer and is attached to the outer sidewall of the insulating layer; The N-type semiconductor layer comprises a first semiconductor layer and a second semiconductor layer from the top surface of the chip downwards. The refractive index of the first semiconductor layer is less than that of the second semiconductor layer, and the thickness of the first semiconductor layer is greater than that of the second semiconductor layer. The surface of the first semiconductor layer facing away from the second semiconductor layer is a non-flat surface, and the maximum peak-to-valley difference of the non-flat surface is greater than 100 nm.

2. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The first semiconductor layer is a single layer of Al with a constant Al composition. a Ga 1-a The structure is N-type with a thickness of 500–8000 nm, and the Al component a is a constant value with parameters satisfying 40% ≤ a ≤ 100%.

3. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The first semiconductor layer is a single layer of Al with non-constant Al composition. b Ga 1-b The structure is an N-structure with a thickness of 1–1000 nm. Its Al composition b decreases linearly from b1 to b2 along the stacking direction from the top surface of the chip downwards. The parameters satisfy 60% ≤ b1 ≤ 100% and 40% ≤ b2 ≤ 80%.

4. The impedance-matched vertical deep ultraviolet LED according to claim 2 or 3, characterized in that, The first semiconductor layer is Si-doped or unintentionally doped, with a Si doping concentration of 1E17 to 1E20 cm⁻¹. -3 .

5. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The second semiconductor layer is a Si-doped monolayer Al. c Ga 1-c The structure is an N-structure with a thickness of 1–1000 nm and a Si doping concentration of 1E17–1E20 cm⁻¹. -3 ; Wherein, the Al component c of the second semiconductor layer is a constant value and the parameter satisfies 30%≤a≤80%; or, the Al component c of the second semiconductor layer is a non-constant value and decreases linearly from c1 to c2 along the stacking direction from the top surface of the chip downward; wherein the parameter satisfies 50%≤c1≤80% and 30%≤c2≤60%.

6. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The N-type semiconductor layer further includes a third semiconductor layer located between the second semiconductor layer and the quantum well active layer, and both the insulating layer and the N-type contact layer are in contact with the lower surface of the third semiconductor layer; The third semiconductor layer is a single layer of Al with non-constant Al composition. e Ga 1-e In the N-structure, the Al composition of the second semiconductor layer near the third semiconductor layer is e1, and the Al composition of the quantum well active layer near the third semiconductor layer is e2; the Al composition e of the third semiconductor layer changes linearly from e1 to e2 along the stacking direction from the top of the chip downwards.

7. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The N-type semiconductor layer further includes a fourth semiconductor layer located between the first semiconductor layer and the second semiconductor layer, wherein the fourth semiconductor layer is a monolayer Al with non-constant Al composition. f Ga 1-f N-structure; Wherein, the Al composition of the first semiconductor layer near the fourth semiconductor layer is f1, and the Al composition of the second semiconductor layer near the fourth semiconductor layer is f2; the Al composition f of the fourth semiconductor layer changes linearly from f1 to f2 along the stacking direction from the top surface of the chip downward.

8. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, Both the first semiconductor layer and the second semiconductor layer are single-layer Al. d Ga 1-d N-structure; the average Al composition of the first semiconductor layer is d1, the average Al composition of the second semiconductor layer is d2, and d1 - d2 ≥ 3%.

9. The impedance-matched vertical deep ultraviolet LED according to claim 8, characterized in that, The N-type semiconductor layer further includes a fifth semiconductor layer located between the first semiconductor layer and the second semiconductor layer. The fifth semiconductor layer includes a first sub-layer and a second sub-layer sequentially from the top surface of the chip downwards. The first sub-layer is a single layer of Al. x Ga 1-x The N-structure, with the second sublayer being a single layer of Al. y Ga 1-y N structure; x=d1±10%, y=d2±10% and x>y.

10. The impedance-matched vertical deep ultraviolet LED according to claim 1, characterized in that, The vertical deep ultraviolet LED further includes an N-type electrode, a P-type electrode, and a supporting substrate; the N-type electrode is disposed on the lower surface of the N-type contact layer; the P-type electrode is disposed on the sidewall of the P-type contact layer that is not covered by the insulating layer, and is in contact with the sidewall; the supporting substrate is disposed on the lower surface of the N-type electrode.