A method for protecting semiconductor trenches and a semiconductor structure

By controlling the ratio of photoresist layer to trench depth and using dry etching technology, the problem of trench structure damage caused by photoresist thickness differences was solved, achieving reliable protection and efficient production of semiconductor trenches.

CN123076181APending Publication Date: 2026-11-10ZHEJIANG ICSPROUT SEMICONDUCTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611252694.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In semiconductor manufacturing processes, the thickness difference of photoresist between the trench region and the non-trench region means that the internal structure of the trench cannot be reliably protected during the etching process, resulting in structural damage or destruction. Existing technologies cannot effectively reduce this thickness difference.

Method used

By controlling the preset ratio between the initial thickness of the photoresist layer and the trench depth, the height difference is ensured to be within a specific range. The thickness of the photoresist layer is gradually adjusted using dry etching technology until the conditions are met, and then etching is performed to protect the internal structure of the trench.

Benefits of technology

This method achieves complete protection of the internal structure of the trench during the etching process, reduces process steps, lowers the risk of process deviation, improves production efficiency, and avoids structural damage to the trench sidewalls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076181A_ABST
    Figure CN123076181A_ABST
Patent Text Reader

Abstract

This invention discloses a method for protecting semiconductor trenches and a semiconductor structure. The method includes controlling a preset ratio between the initial thickness of the photoresist layer and the trench depth when forming a photoresist layer on the surface of the semiconductor substrate and within the trench; a height difference exists between the portion of the photoresist layer above the trench region and the portion above the dielectric stack. An etching step is performed when the height difference simultaneously satisfies a first condition and a second condition. The first condition is that the height difference is less than 20% of the thickness of the photoresist layer above the dielectric stack; the second condition is that the height difference is greater than or equal to the sum of the thicknesses of the second and third dielectric layers. If the height difference does not satisfy the first and second conditions, the photoresist layer is etched to remove the photoresist above the dielectric stack, and steps S2-S3 are repeated until the height difference simultaneously satisfies both the first and second conditions. Therefore, this invention can protect the trench sidewalls while improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing technology, and more specifically to a method for protecting semiconductor trenches and a semiconductor structure. Background Technology

[0002] In semiconductor manufacturing processes, some special products require the formation of intricate localized process patterns on the wafer surface. These patterns are relatively small, occupying less than 1% of the 12-inch wafer area, and are not located in the central region of the wafer. This area is a trench structure, and when etching the top structure of the trench using a dry + wet etching process, the internal structure must not be damaged. Therefore, photoresist is often used as a protective layer to cover the wafer surface.

[0003] However, when using photoresist to cover the surface of a wafer with a trench structure, the thickness of the photoresist in the trench area is lower than that in the non-trench area due to the height difference between the trench and non-trench regions. This thickness difference has a serious impact on subsequent processes: during the etching process at the same rate to remove the photoresist, when the photoresist in the non-trench area is completely removed, the photoresist inside the trench is too thin to continue protecting the internal structure of the trench. This causes subsequent etching processes to directly affect the inside of the trench, resulting in structural damage or even destruction.

[0004] However, under current conventional process conditions, the difference between H1 and H2 is typically 30% or more of H2, which cannot meet the requirements for protecting the internal structure of the trench. Therefore, there is an urgent need for a method that can effectively reduce the difference in photoresist thickness between the trench region and the non-trench region and reliably protect the internal structure of the trench during the etching process.

[0005] It should be noted that the information disclosed in this background section is intended only to enhance the understanding of the overall background of the present invention, and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention

[0006] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method and structure for protecting semiconductor trenches, so as to protect semiconductor trenches and improve production efficiency.

[0007] To achieve the above and other related objectives, the present invention provides a method for protecting semiconductor trenches, comprising:

[0008] S1: Provide a semiconductor substrate, the semiconductor substrate including a wafer and a dielectric stack covering the surface of the wafer, the dielectric stack including a first dielectric layer, a second dielectric layer and a third dielectric layer in sequence from the surface of the wafer, and a trench formed in the semiconductor substrate, the trench extending from the upper surface of the dielectric stack toward the wafer and penetrating the dielectric stack and a portion of the thickness of the wafer.

[0009] S2: A photoresist layer is formed on the surface of the semiconductor substrate and in the trench, and a preset ratio relationship is maintained between the initial thickness of the photoresist layer and the trench depth; the portion of the photoresist layer above the trench region has a height difference with the portion above the dielectric stack.

[0010] S3: When the height difference simultaneously meets the first condition and the second condition, proceed to step S5; when the height difference does not simultaneously meet the first condition and the second condition, proceed to step S4.

[0011] The first condition is that the height difference is less than 20% of the thickness of the photoresist layer above the dielectric stack;

[0012] The second condition is: the height difference is greater than the sum of the thicknesses of the second dielectric layer and the third dielectric layer;

[0013] S4: If the height difference in step S3 does not meet the first and second conditions, the photoresist layer is etched to remove the photoresist located above the dielectric stack, and steps S2 to S3 are repeated until the height difference simultaneously meets the first and second conditions.

[0014] S5: Perform the second etching to remove the remaining photoresist layer and the first dielectric layer, exposing the sidewalls of the trench. The third dielectric layer is not etched laterally, and the structure of the trench inside the wafer remains intact.

[0015] Optionally, in step S2, the preset ratio is: the thickness difference between the thickness of the photoresist layer and the depth of the trench is controlled to be 10% to 50% of the trench depth.

[0016] Optionally, in step S2, the thickness deviation of the photoresist layer is less than 3% of the photoresist layer thickness.

[0017] Optionally, in step S2, forming the photoresist layer includes: wetting the surface of the semiconductor substrate with RRC reagent, applying the photoresist using a dynamic dispensing method, and performing soft baking after application.

[0018] Optionally, in step S4, steps S2 to S3 are repeated no more than 3 times.

[0019] Optionally, the first and second etching processes are dry etching.

[0020] Optionally, the sum of the thicknesses of the second dielectric layer and the third dielectric layer is 10% to 20% of the trench depth.

[0021] Optionally, the projected area of ​​the trench on the wafer surface is less than 1% of the total wafer area.

[0022] Alternatively, the trench may be located in the edge region or non-central region of the wafer.

[0023] According to one aspect of the present invention, a semiconductor structure is also provided, which is prepared by the above-described method for protecting semiconductor trenches.

[0024] Optionally, the top corner region of the trench located within the wafer is covered with a third dielectric layer of a certain thickness.

[0025] Compared with the prior art, the semiconductor trench protection method and semiconductor structure of the present invention have at least the following beneficial effects:

[0026] 1) This invention controls the thickness difference between the initial thickness of the photoresist layer and the trench depth to 10%~50% of the trench depth, ensuring a sufficient base for the photoresist thickness. This results in the absolute value of the height difference being greater than the sum of the thicknesses of the second and third dielectric layers after the first coating, satisfying the absolute protection thickness condition. Simultaneously, due to the increased base thickness of the photoresist layer, the percentage of the thickness difference to the photoresist layer thickness decreases to below 20% after the first coating or after no more than three cycles, satisfying the planarization condition. Achieving both conditions simultaneously avoids the side-cutting problem of the trench.

[0027] (2) Within the thickness range of this application, based on the values ​​of photoresist layer thickness and trench depth, only no more than three “coating-etching” cycles are needed to satisfy both conditions simultaneously. Compared with the thin-film solution, which requires multiple cycles but still cannot satisfy both conditions simultaneously, unnecessary process steps are reduced, the risk of process deviation accumulation introduced by multiple cycles is reduced, and process efficiency is improved.

[0028] (3) The present invention only needs to control the initial thickness in the photoresist coating process, without adjusting the global process parameters such as etching cavity and gas ratio. It is also applicable to local trench patterns with an area of ​​less than 1% on the wafer and located in the non-central region, and does not have any additional impact on the completed process structure in other areas of the wafer.

[0029] (4) In the semiconductor structure prepared by the method of the present invention, the third dielectric layer is not laterally etched, and the trench sidewalls located in the wafer remain intact, thus avoiding structural damage to the trench sidewalls caused by etching. Attached Figure Description

[0030] Figure 1 This is a top view of the semiconductor substrate in an embodiment of the present invention;

[0031] Figure 2 This is a schematic diagram of the cross-sectional structure of a semiconductor substrate after a photoresist layer has been formed on its surface, as shown in an embodiment of the present invention.

[0032] Figure 3 This is a schematic diagram of the cross-sectional structure after removing the first dielectric layer from the surface of a semiconductor substrate in the prior art.

[0033] Figure 4 This is a flowchart illustrating the steps of the semiconductor trench protection method in an embodiment of the present invention;

[0034] Figure 5 This is a SEM image of a semiconductor substrate after the first dielectric layer on the surface has been removed, as described in the prior art.

[0035] Figure 6 This is a SEM image of the semiconductor substrate after the first dielectric layer on the surface has been removed, according to an embodiment of the present invention.

[0036] Illustration of reference numerals in the attached diagram:

[0037] 1. Process pattern area; 2. Area requiring protection; 3. Internal structure damaged; 10. Semiconductor substrate; 100. Substrate; 200. Dielectric stack; 210. First dielectric layer; 220. Second dielectric layer; 230. Third dielectric layer; 300. Trench; 400. Photoresist layer; 410. First part; 402. Second part; 500. Side-cutting phenomenon. Detailed Implementation

[0038] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of this application. It should be noted that, unless otherwise specified, the following embodiments and features in the embodiments can be combined with each other.

[0039] It should be understood that the illustrations provided in the embodiments of this invention are merely schematic representations of the basic concept of the invention. Although the illustrations only show components relevant to the invention and are not drawn according to the actual number, shape, and size of components in implementation, the shape, quantity, and proportion of each component can be arbitrarily changed in actual implementation, and the component layout may also be more complex. The structures, proportions, sizes, etc., shown in the accompanying drawings are only used to complement the content disclosed in the specification for those skilled in the art to understand and read, and are not intended to limit the conditions under which this application can be implemented. Therefore, they have no substantial technical significance. Any modifications to the structure, changes in the proportional relationships, or adjustments to the size, without affecting the effects and objectives that the invention can produce, should still fall within the scope of the technical content disclosed in this application.

[0040] Example 1

[0041] This embodiment provides a method for protecting semiconductor trenches, referring to... Figure 4 This method protects the trenches in the semiconductor substrate from damage during the etching process. The semiconductor trench protection method of this embodiment includes:

[0042] S1: Provide a semiconductor substrate, the semiconductor substrate including a wafer and a dielectric stack covering the surface of the wafer, the dielectric stack including a first dielectric layer, a second dielectric layer and a third dielectric layer in sequence from the surface of the wafer, and a trench formed in the semiconductor substrate, the trench extending from the upper surface of the dielectric stack toward the wafer and penetrating the dielectric stack and a portion of the thickness of the wafer.

[0043] S2: A photoresist layer is formed on the surface of the semiconductor substrate and in the trench, and a preset ratio relationship is maintained between the initial thickness of the photoresist layer and the trench depth; the portion of the photoresist layer above the trench region has a height difference with the portion above the dielectric stack.

[0044] S3: When the height difference simultaneously meets the first condition and the second condition, proceed to step S5; when the height difference does not simultaneously meet the first condition and the second condition, proceed to step S4.

[0045] The first condition is that the height difference is less than 20% of the thickness of the photoresist layer located above the dielectric stack;

[0046] The second condition is: the height difference is greater than or equal to the sum of the thicknesses of the second dielectric layer and the third dielectric layer.

[0047] S4: If the height difference in step S3 does not simultaneously satisfy the first condition and the second condition, then the photoresist layer is etched to remove part of the photoresist located above the dielectric stack, and steps S2~S3 are repeated until the height difference simultaneously satisfies the first condition and the second condition.

[0048] S5: Perform the second etching to remove the remaining photoresist layer and the first dielectric layer, exposing the sidewalls of the trench. The third dielectric layer is not etched laterally, and the structure of the trench inside the wafer remains intact.

[0049] Perform step S1, refer to Figure 2 A semiconductor substrate is provided, comprising a wafer 100 and a dielectric stack 200 covering the surface of the wafer 100. The dielectric stack 200 sequentially includes a first dielectric layer 210, a second dielectric layer 220, and a third dielectric layer 230 from the surface of the wafer 100. A trench 300 is formed within the wafer 100, extending from the upper surface of the dielectric stack 200 toward the wafer 100, sequentially penetrating the third dielectric layer 230, the second dielectric layer 220, and the first dielectric layer 210, and extending to a certain depth within the wafer 100. (Referring to...) Figure 2 The area 2 requiring protection is the sidewall formed between the wafer and the third dielectric layer 230. In the prior art, referring to... Figure 3 When etching away the photoresist layer 400 in the trench 300, it will damage the area 2 that needs to be protected, resulting in the destruction of the internal structure.

[0050] The materials of the first dielectric layer 210, the second dielectric layer 220, and the third dielectric layer 230 can be selected from one or more of silicon oxide, silicon nitride, and silicon oxynitride, but the present invention is not limited thereto. In this embodiment, the material of the first dielectric layer 210 is silicon dioxide, the material of the second dielectric layer 220 is silicon nitride, and the material of the third dielectric layer 230 is silicon dioxide. The thickness of the first dielectric layer 210 is 80 nm, the thickness of the second dielectric layer 220 is 50 nm, and the thickness of the third dielectric layer 230 is 20 nm. The sum of the thicknesses of the second dielectric layer 220 and the third dielectric layer 230 is 70 nm.

[0051] Optionally, refer to Figure 1 A patterned region 1 is formed on wafer 100, and a trench 300 is located within the patterned region 1. The patterned region 1 is located at the edge of the wafer. The projected area of ​​the trench 300 on the surface of wafer 100 is less than 1% of the total area of ​​wafer 100, and the trench 300 is located at the edge or non-central region of wafer 100. Optionally, the sum of the thicknesses of the second dielectric layer and the third dielectric layer is 10% to 20% of the trench depth.

[0052] Step S2 is performed to form a photoresist layer 400 on the surface of the semiconductor substrate and in the trench 300.

[0053] Specifically, the semiconductor substrate surface is first wetted with RRC reagent. RRC reagent is a photoresist diluent, whose main components are one or more of propylene glycol methyl ether (PGME) and propylene glycol methyl acetate (PGMEA). The wafer is fed into a spin coater, where it is adsorbed onto the vacuum chuck of the spin coater. The wafer is rotated at a certain speed, while RRC reagent is sprayed from the central area of ​​the wafer surface towards the edge, ensuring that the wafer surface is uniformly wetted.

[0054] Next, photoresist is applied using a dynamic dispensing method. During wafer rotation, photoresist is dispensed into the central area of ​​the wafer surface, and centrifugal force is used to evenly spread the photoresist across the entire wafer surface and inside the trenches. After coating, a soft bake is performed to remove some of the solvent from the photoresist and cure the photoresist layer. The temperature and time of the soft bake are determined based on the type of photoresist selected.

[0055] Optionally, in step S2, forming the photoresist layer includes the following specific operations:

[0056] First, the wafer is fed into a spin coater and adsorbed onto a vacuum chuck. The wafer is rotated at 30-500 rpm while RRC solvent is ejected from the spray nozzle onto the wafer surface for 0.1-5 seconds. Then, the wafer rotation speed is adjusted to 0-100 rpm, and RRC solvent is ejected from the spray nozzle again for 0.1-5 seconds. This two-step variable-speed RRC coating effectively reduces photoresist consumption and improves the process quality of the photoresist film on the wafer surface.

[0057] After RRC wetting, photoresist is applied using a dynamic dispensing method. The wafer rotation speed is increased to the coating speed, and the photoresist is dispensed into the central area of ​​the wafer surface. Centrifugal force is used to spread the photoresist evenly. After coating, the wafer is placed on a hot plate for soft baking. The baking temperature and time are determined according to the manufacturer's recommendations for the selected photoresist.

[0058] A preset ratio is maintained between the initial thickness of the photoresist layer 400 and the depth of the trench 300. Specifically, the thickness difference between the initial thickness H2 of the photoresist layer and the trench depth h is controlled to be 10% to 50% of the trench depth h, that is, satisfying: h × 10% ≤ H2 − h ≤ h × 50%. For example, when the trench depth h is 300 nm, the photoresist layer thickness can be selected as 345 nm; when the trench depth h is 450 nm, the photoresist layer thickness can be selected as 495 nm to 675 nm.

[0059] Simultaneously, the thickness uniformity of the photoresist layer 400 is controlled to meet a preset deviation range. Specifically, the thickness deviation (Range, i.e., the difference between the maximum and minimum values ​​of the photoresist thickness at different locations on the wafer surface) of the photoresist layer 400 is controlled to be less than 3% of the initial thickness. For example, when the photoresist layer thickness is 345nm, its Range needs to be less than 10nm.

[0060] After the above coating, the photoresist layer 400 includes a first portion 410 located within and above the trench 300 and a second portion 420 located above the dielectric stack 200. Due to the height difference between the trench region and the non-trench region, the thickness H1 of the first portion 410 above the trench 300 is lower than the thickness H2 of the second portion 420, and there is a height difference Δ = H2 − H1 between them.

[0061] Execute step S3. If the height difference simultaneously meets the first and second conditions, execute step S5. If the height difference does not simultaneously meet the first and second conditions, execute step S4.

[0062] The first condition is Δ < H2 × 20%, to achieve planarization of the photoresist layer and ensure uniform etching in the vertical direction. The second condition is Δ > the thickness of the second dielectric layer (220 nm) + the thickness of the third dielectric layer (230 nm). In this embodiment, Δ > 70 nm, to ensure that the third dielectric layer is not laterally etched during the removal of the first dielectric layer.

[0063] Taking a trench depth of h=450nm as an example:

[0064] When H2 = 675nm (H2−h = 225nm = h × 50%), Δ = 103nm, Δ / H2 ≈ 15.3% < 20%, Δ = 103nm > 70nm. Both conditions are met simultaneously, so step S5 is executed directly, and the number of loops is 0.

[0065] When H2 = 540nm (H2−h = 90nm = h × 20%), Δ = 103nm, Δ / H2 ≈ 19.1% < 20%, Δ = 103nm > 70nm. Both conditions are met simultaneously, so step S5 is executed directly, and the number of loops is 0.

[0066] When H2 = 495nm (H2−h = 45nm = h × 10%, lower limit), Δ = 103nm, Δ / H2 ≈ 20.8% > 20%, Δ = 103nm > 70nm, the first condition is not met, the second condition is met, and step S4 is executed.

[0067] Execute step S4. If the height difference in step S3 does not simultaneously satisfy the first condition and the second condition, then etch the photoresist layer to remove the photoresist located above the dielectric stack. Repeat steps S2 to S3 until the height difference simultaneously satisfies the first condition and the second condition.

[0068] Specifically, the photoresist layer 400 is first etched to remove the photoresist located above the dielectric stack 200. A dry etching process is used to perform isotropic etching of the photoresist layer, with the photoresist in the flat regions (second portion 420) and the trench regions (first portion 410) being removed simultaneously at the same rate. Optionally, after the photoresist above the dielectric stack 200 is removed, some photoresist may remain inside the trenches.

[0069] Then, repeat steps S2-S3 to reform the photoresist layer on the surface of the dielectric stack after the first etching and within the trenches. Similarly, measure the height difference between the surface of the photoresist above the dielectric stack and the surface of the photoresist in the trenches until the height difference Δ simultaneously satisfies both the first and second conditions. The repetition should not exceed three times. Preferably, the repetition should be at most once.

[0070] Taking H2=495nm (h×10% lower limit) as an example: After the first cycle, Δ shrinks from 103nm to 70nm. At this time, Δ=70nm is equal to the sum of the thicknesses of the second and third dielectric layers (critical value), Δ / H2=70 / 495≈14.1%<20%, both conditions are met simultaneously (critical state), and the cycle stops.

[0071] After one or more cycles, the height difference between the photoresist layer 400 in the trench region and the flat region is further reduced to meet the requirements.

[0072] Step S5 is executed to perform the second etching, which removes the remaining photoresist layer and the first dielectric layer, exposing the sidewalls of the trench. The third dielectric layer is not laterally etched, and the structure of the trench located inside the wafer remains intact.

[0073] Specifically, a second etching is performed to remove the remaining photoresist layer and the first dielectric layer 210 (i.e., an 80nm thick SiO2 layer), exposing the sidewalls of the trench 300.

[0074] Since Δ has simultaneously met the two conditions of Δ<20%×H2 and Δ>70nm in step S3 or S4, during the etching process to remove the first dielectric layer 210:

[0075] Vertical direction: Because Δ<20%×H2, the photoresist in the flat area and the trench area is removed relatively uniformly, avoiding the uneven state where one side is etched through and the other side is still too thick;

[0076] Lateral (sidewall direction): Because Δ>70nm, the photoresist coating layer on the trench sidewall has sufficient lateral thickness. The third dielectric layer 230 will not be exposed to the etching environment prematurely during the removal of the first dielectric layer 210, and the etchant cannot attack the third dielectric layer 230 from the side.

[0077] Ultimately, the third dielectric layer 230 was not laterally etched and remained completely covered on the surface of the corner region 301 at the top of the trench, thus blocking the side-cutting path; the sidewall of the trench 300 located inside the wafer 100 was not etched or damaged, and the structure remained intact.

[0078] Example 2

[0079] This embodiment provides a semiconductor structure prepared using the semiconductor trench protection method as described in Embodiment 1.

[0080] Reference Figure 2 and Figure 6The semiconductor structure includes a wafer 100 and a dielectric stack 200 covering the surface of the wafer 100. The dielectric stack 200 includes a first dielectric layer 210, a second dielectric layer 220 and a third dielectric layer 230 sequentially from the surface of the wafer 100, wherein the first dielectric layer 210 has been completely removed, and the second dielectric layer 220 and the third dielectric layer 230 remain on the surface of the wafer 100.

[0081] A trench 300 is formed within the wafer 100. The trench 300 extends from the upper surface of the dielectric stack 200 toward the wafer 100, sequentially penetrating the third dielectric layer 230, the second dielectric layer 220, and the first dielectric layer 210, and extends to a certain depth inside the wafer 100. The sidewalls of the trench 300 are exposed to the external environment.

[0082] The third dielectric layer 230 covers the second dielectric layer 220, and at the top corner region 301 of the trench 300, the third dielectric layer 230 continuously covers the corner surface without being laterally etched. Specifically, the thickness of the third dielectric layer 230 at the top corner region 301 of the trench is not significantly thinned due to lateral etching compared to the initial deposition thickness, the dielectric layer at the corner is continuous without breakage, and the etchant does not penetrate into the trench along the corner.

[0083] The sidewall surface of trench 300 inside wafer 100 is smooth and structurally intact, with no traces of sidewall damage, and its sidewall morphology is consistent with the expected morphology before etching. The internal space of trench 300 was not invaded by etchant, and the wafer material at the bottom of the trench was not etched and damaged.

[0084] In this embodiment, the first dielectric layer 210 is a SiO2 layer with an initial thickness of 80 nm, which has been completely removed during the process; the second dielectric layer 220 is a silicon nitride layer with a final remaining thickness of 50 nm; and the third dielectric layer 230 is a silicon oxide layer with a final remaining thickness of 20 nm. The total thickness of the second dielectric layer 220 and the third dielectric layer 230 is 70 nm, completely covering the surface of wafer 100 and the top corner region 301 of the trench. It should be noted that the materials and thicknesses of the above dielectric layers are only illustrative examples, and the present invention is not limited thereto. In other embodiments, other dielectric materials and other thickness combinations can be used for each dielectric layer, as long as the total thickness of the second and third dielectric layers can be matched with the photoresist height difference Δ to achieve anti-poke protection.

[0085] The projected area of ​​trench 300 on the surface of wafer 100 is less than 1% of the total area of ​​wafer 100, and trench 300 is located in the edge region or non-central region of wafer 100. This structural feature indicates that the present invention is particularly suitable for semiconductor devices with localized, small-area, non-central trench patterns on the wafer surface.

[0086] The present invention will now be described in detail with reference to specific embodiments.

[0087] Implementation Method 1

[0088] This embodiment provides process guidelines for selecting the initial thickness of the photoresist, explaining the number of "coating-etching" cycles required to meet the first condition (height difference Δ is less than 20% of the photoresist thickness H2 in the flat area) and the second condition (height difference Δ is greater than the sum of the thicknesses of the second and third dielectric layers, i.e., greater than 70nm) under different photoresist thickness values.

[0089] The trench depth is set to h = 450 nm, the second dielectric layer thickness is 50 nm, and the third dielectric layer thickness is 20 nm, with the sum of the thicknesses of the second and third dielectric layers being 70 nm. After photoresist coating, an initial height difference Δ0 will be generated between the trench area and the flat area. It should be noted that the specific value of Δ0 will fluctuate due to factors such as photoresist material characteristics (e.g., viscosity, solid content), spin coating process parameters (e.g., spin coating speed, acceleration, drop volume), and trench morphology, and is not a fixed value. Generally speaking, the larger the initial photoresist thickness H2, the slightly larger Δ0 will be. The following explanation uses Δ0 values ​​under representative process conditions to illustrate the process window provided by the thickness range settings of this application.

[0090] Interval 1: H2 − h ≥ h × 20% (i.e. H2 ≥ 540nm, the amount by which the initial thickness of the photoresist exceeds the trench depth is greater than or equal to 20% of the trench depth)

[0091] When H2 falls within this range, due to the sufficiently large base of H2, the Δ0 / H2 ratio after the initial coating is compressed to below 20%, satisfying the first condition. Simultaneously, because H2 is sufficiently thick, the absolute value of Δ0 is typically greater than 70 nm, satisfying the second condition. Both conditions are met simultaneously after the initial coating, allowing for direct execution of the final etching step without any further cycling. The cycle count for this range is 0.

[0092] For example, when H2 = 540 nm (the thickness difference is 20% of the trench depth, the lower limit of this range), if Δ0 is approximately 103 nm, then Δ0 / H2 ≈ 19.1% < 20%, and Δ0 = 103 nm > 70 nm. Both conditions are met simultaneously, and the number of cycles is 0. When H2 is larger (e.g., H2 = 675 nm, the thickness difference is 50% of the trench depth), the Δ0 / H2 ratio will further decrease (approximately 15.3%), and again, 0 cycles are sufficient to meet the standard.

[0093] Interval 2: h × 10% ≤ H2 − h < h × 20% (i.e. 495nm ≤ H2 < 540nm, the amount by which the initial thickness of the photoresist exceeds the trench depth is between 10% and 20% of the trench depth).

[0094] When H2 falls within this range, the Δ0 / H2 ratio after the initial coating is slightly higher than 20%, and the first condition is not yet met, requiring a cycle to be executed. After one "coating-etching" cycle, the height difference Δ decreases from Δ0 to Δ1, and the Δ1 / H2 ratio drops below 20%, satisfying the first condition. Simultaneously, because H2 still has a sufficient base, the absolute value of Δ1 remains around 70nm (critical value) or above, satisfying the second condition. The number of cycles corresponding to this range is 1.

[0095] For example, when H2 = 495 nm (the thickness difference is 10% of the trench depth, the lower limit of this range), if Δ0 is approximately 103 nm, then Δ0 / H2 ≈ 20.8% > 20%, and the first condition is not met. After one cycle, Δ1 shrinks to 70 nm, Δ1 / H2 ≈ 14.1% < 20%, and Δ1 = 70 nm is equal to the sum of the thicknesses of the second and third dielectric layers (critical value). Both conditions are met simultaneously, and the cycle count is 1. At this point, the final etching step can be performed.

[0096] It should be noted that in the above example, Δ0 = 103nm is a representative value. If, in the actual process, Δ0 is 95nm or 115nm due to differences in equipment or materials, under interval two (H2 = 495nm), Δ0 / H2 would be approximately 19.2% or 23.2%, respectively. If Δ0 = 95nm, both conditions are satisfied after the first coating (95 / 495 ≈ 19.2% < 20%, and 95 > 70), and the cycle count is 0. If Δ0 = 115nm, after one cycle, Δ1 shrinks to approximately 80~85nm, still greater than 70nm, and Δ1 / H2 ≈ 16%~17% < 20%, requiring one cycle. Therefore, even if Δ0 fluctuates within a reasonable range, the cycle count corresponding to the thickness conditions of this application remains 0~1.

[0097] Interval 3: H2 − h < h × 10% (i.e., H2 < 495nm, which does not fall within the scope of protection of this application)

[0098] When H2 falls within this range, the initial photoresist thickness is insufficient, and the Δ0 / H2 ratio is too high, requiring multiple cycles to reduce Δ / H2 below 20%. However, after multiple cycles, the absolute value of Δ has simultaneously decreased to below 70nm, and the second condition is no longer met. This range cannot simultaneously satisfy both conditions and is therefore not within the scope of this invention. See Embodiment Two for details.

[0099] Implementation Method 2

[0100] This comparative example is used to demonstrate the process effect when the initial thickness of the photoresist does not fall within the protection scope of this invention.

[0101] The trench depth is set to h = 450 nm, and the dielectric stacking parameters are the same as in Implementation Method 1: the thickness of the first dielectric layer is 80 nm, the thickness of the second dielectric layer is 50 nm, the thickness of the third dielectric layer is 20 nm, and the sum of the thicknesses of the second and third dielectric layers is 70 nm. The operator selects an initial photoresist thickness H2 = 225 nm. At this time, H2 − h = 225 − 450 = −225 nm, that is, the photoresist thickness is less than the trench depth, and the thickness difference is negative, which does not meet the condition of this invention that "the thickness difference between the initial photoresist thickness and the trench depth is 10% to 50% of the trench depth" (that is, H2 − h should be between 45 nm and 225 nm, and the corresponding H2 should be between 495 nm and 675 nm).

[0102] After the first coating, the height difference Δ0 = 103 nm, Δ0 / H2 ≈ 45.8%, which is much greater than 20%, so the first condition is not met; Δ0 = 103 nm is greater than 70 nm, so the second condition is met. After the first cycle, Δ1 = 70 nm, but Δ1 / H2 ≈ 31.1%, still greater than 20%, so the first condition is still not met. After the second cycle, Δ2 = 41 nm, Δ2 / H2 ≈ 18.2% < 20%, so the first condition is met, but Δ2 = 41 nm < 70 nm, so the second condition is no longer met. After the third cycle, Δ3 = 30 nm, Δ3 / H2 ≈ 13.3%, so the first condition is met to a higher degree, but Δ3 = 30 nm is much less than 70 nm, so the second condition is even less met.

[0103] Therefore, it is evident that the first and second conditions cannot be simultaneously satisfied in this comparative example. After the first cycle, the second condition is satisfied, but the first condition is not; after the second and third cycles, the first condition is satisfied, but the second condition is not. If the operator performs the final etching after the second or third cycle to remove the first dielectric layer (SiO2, 80nm), since Δ < 70nm, the third dielectric layer is prematurely exposed to the etching environment during the etching process of removing the first dielectric layer. The etchant attacks the third dielectric layer laterally, causing it to be almost completely etched away, resulting in a significant "side-cut" defect. The etchant penetrates into the trench along the side-cut path, damaging the trench sidewalls and internal structure within the wafer, failing to provide effective protection for the trench within the wafer. If the operator performs the final etching after the first cycle, although Δ = 70nm satisfies the critical value of the second condition, Δ / H2 = 31.1% is much greater than 20%, severely failing to meet the first condition. The etching is uneven in the vertical direction, and the reliability of the process cannot be guaranteed.

[0104] This comparative example illustrates that when the initial thickness of the photoresist does not fall within the range defined in this application, even after multiple cycles, the two conditions cannot be met simultaneously, making it impossible to effectively protect the third dielectric layer and the sidewalls of the inner trench of the wafer.

[0105] Figure 5The comparative example of Embodiment 2 shows a semiconductor structure obtained without the method of the present invention, in which the third dielectric layer 230 is laterally etched away at the corner region 301 at the top of the trench, resulting in a side-penetration phenomenon 500. The etchant penetrates into the trench along the side-penetration path, causing the sidewall of the trench 300 located inside the wafer 100 to be etched and damaged, resulting in a rough surface and uneven morphology. The internal space of the trench is irregularly expanded, which seriously affects the device performance.

[0106] Figure 6 The semiconductor structure obtained by the method of the present invention in section one of Embodiment 1 is shown. In this semiconductor structure, the third dielectric layer 230 remains intact and continuous in the top corner region 301 of the trench, and the sidewalls of the trench inside the wafer are smooth and undamaged.

[0107] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A method for protecting semiconductor trenches, characterized in that, include: S1: A semiconductor substrate is provided, the semiconductor substrate including a wafer and a dielectric stack covering the surface of the wafer, the dielectric stack including a first dielectric layer, a second dielectric layer and a third dielectric layer in sequence from the surface of the wafer, and a trench is formed in the semiconductor substrate, the trench extending from the upper surface of the dielectric stack toward the wafer and penetrating the dielectric stack and a portion of the thickness of the wafer; S2: A photoresist layer is formed on the surface of the semiconductor substrate and in the trench, and a preset ratio relationship is controlled between the initial thickness of the photoresist layer and the depth of the trench. The portion of the photoresist layer above the trench region has a height difference from the portion above the dielectric stack; S3: When the height difference simultaneously satisfies the first condition and the second condition, proceed to step S5; when the height difference does not simultaneously satisfy the first condition and the second condition, proceed to step S4. The first condition is that the height difference is less than 20% of the thickness of the photoresist layer above the dielectric stack; The second condition is that the height difference is greater than or equal to the sum of the thicknesses of the second dielectric layer and the third dielectric layer; S4: If the height difference in step S3 does not simultaneously satisfy the first condition and the second condition, then the photoresist layer is first etched to remove the photoresist located above the dielectric stack, and steps S2 to S3 are repeated until the height difference simultaneously satisfies the first condition and the second condition. S5: Perform a second etching to remove the remaining photoresist layer and the first dielectric layer, exposing the sidewalls of the trench. The third dielectric layer is not laterally etched, and the structure of the trench located inside the wafer remains intact.

2. The method for protecting semiconductor trenches according to claim 1, characterized in that, In step S2, the preset ratio is: the thickness difference between the thickness of the photoresist layer and the depth of the trench is controlled to be 10% to 50% of the trench depth.

3. The method for protecting semiconductor trenches according to claim 1, characterized in that, In step S2, the thickness deviation of the photoresist layer is less than 3% of the thickness of the photoresist layer.

4. The method for protecting semiconductor trenches according to claim 1, characterized in that, In step S2, forming the photoresist layer includes: wetting the surface of the semiconductor substrate with RRC reagent, applying photoresist using a dynamic dispensing method, and performing soft baking after application.

5. The method for protecting semiconductor trenches according to claim 1, characterized in that, In step S4, the number of times steps S2 to S3 are repeated shall not exceed 3.

6. The method for protecting semiconductor trenches according to claim 1, characterized in that, The first etching and the second etching are dry etching methods.

7. The method for protecting semiconductor trenches according to claim 1, characterized in that, The sum of the thicknesses of the second dielectric layer and the third dielectric layer is 10% to 20% of the trench depth.

8. The method for protecting semiconductor trenches according to claim 1, characterized in that, The projected area of ​​the trench on the wafer surface is less than 1% of the total area of ​​the wafer.

9. The method for protecting semiconductor trenches according to claim 1, characterized in that, The trench is located in the edge region or non-central region of the wafer.

10. A semiconductor structure, characterized in that, It is prepared by the method for protecting semiconductor trenches as described in any one of claims 1 to 9.

11. The semiconductor structure according to claim 10, characterized in that, The top corner region of the trench located within the wafer is covered with a third dielectric layer of a certain thickness.