A polycrystalline diamond composite heat dissipation substrate and its preparation method

By employing an ultra-high purity gas system, precise process parameters, and optimized interface design, the problems of low thermal conductivity, warpage, and interface thermal resistance of polycrystalline diamond heat dissipation substrates have been solved, resulting in the fabrication of high-performance polycrystalline diamond composite heat dissipation substrates suitable for high-power electronic devices.

CN123076237APending Publication Date: 2026-11-10SHENZHEN SHENGJING CALCIUM INTELLIGENT MANUFACTURING TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611263943.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

Existing polycrystalline diamond heat dissipation substrates suffer from problems such as low thermal conductivity, difficulty in controlling impurities, substrate warping, and high interface thermal resistance, making it difficult to meet the heat dissipation requirements of high power density electronic devices.

Method used

By employing an ultra-high purity gas system, precise process parameter control, optimized substrate processing and interface design, including the combined use of nanodiamond seed layers, microwave plasma deposition, chemical mechanical polishing and multi-layer metallization, combined with laser lift-off and micro-blind hole filling technology, a high-performance polycrystalline diamond composite heat dissipation substrate is formed.

Benefits of technology

A room temperature thermal conductivity of 1800 W/(m·K) was achieved for polycrystalline diamond substrates, reducing impurity concentration and warpage, and optimizing interface thermal resistance, making it suitable for packaging applications of high-power electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076237A_ABST
    Figure CN123076237A_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing a polycrystalline diamond composite heat dissipation substrate, comprising the following steps: substrate pretreatment and seed nucleation: after cleaning and surface roughening of the Si / Mo substrate, a nano-diamond seed layer is coated; preparation of an ultra-high purity gas system: hydrogen purified by a Pd-Ag alloy film purifier and methane with a purity ≥7N are used as the reaction gas source; microwave plasma ignition and parameter setting; CH4 introduction and diamond deposition; cooling and substrate separation: the deposited diamond film is separated from the substrate to obtain a freestanding polycrystalline diamond plate; chemical mechanical polishing: the freestanding polycrystalline diamond plate is polished on both sides. The high thermal conductivity polycrystalline diamond composite heat dissipation substrate and its preparation method provided by this invention can effectively solve the technical problems of low thermal conductivity of polycrystalline diamond, difficulty in controlling impurities, substrate warping, and high interfacial thermal resistance in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a polycrystalline diamond composite heat dissipation substrate and its preparation method, belonging to the field of semiconductor heat dissipation material technology. Background Technology

[0002] Currently, with the rapid development of electronic devices such as 5G mobile communication, artificial intelligence (AI) chips, power semiconductors, and high-power lasers towards high power density, miniaturization, and integration, heat dissipation has become a key bottleneck restricting device performance, lifespan, and reliability. Traditional heat dissipation substrate materials, due to limitations in thermal conductivity, matching coefficient of thermal expansion, and processing costs, are no longer sufficient to meet increasingly stringent heat dissipation requirements.

[0003] Existing materials thermal conductivity defect Aluminum (Al) substrate ~237 W / (m·K) Insufficient thermal conductivity means that the heat flux density of AI chips has exceeded their limits. Copper (Cu) heat sink ~400 W / (m·K) Density (8.9 g / cm³), CTE mismatch Si Aluminum nitride (AlN) ceramics ~170-200 W / (m·K) Difficulty in sintering, high cost, and brittleness Silicon carbide (SiC) substrate ~270-490 W / (m·K) High-temperature manufacturing process, difficulty in controlling surface roughness Single-crystal diamond (SCD) ~2200 W / (m·K) Size limitations, high cost, and difficulty in integrating heterogeneous materials Polycrystalline diamond (PCD) 800–1800 W / (m·K) Insufficient gas purity leads to impurity scattering and reduced thermal conductivity. As shown in the table above, although single-crystal diamond (SCD) has the highest theoretical thermal conductivity (approximately 2200 W / (m·K)), its size is limited (<10 mm) and its cost is extremely high, making it difficult to achieve large-scale industrial applications. Polycrystalline diamond (PCD) can theoretically combine the advantages of thermal conductivity and size, but existing preparation technologies have many defects, resulting in its actual thermal conductivity being far lower than the theoretical value.

[0004] Meanwhile, existing polycrystalline diamond chemical vapor deposition (CVD) preparation processes mainly suffer from the following technical defects: (1) Insufficient gas purity: Commercial H2 purity is often only 5N to 6N, and residual O2, N2 and other impurities are at the ppb to ppm level. These impurity atoms segregate at the grain boundaries during diamond growth, forming phonon scattering centers, resulting in a 20% to 40% loss in thermal conductivity.

[0005] (2) The CH4 concentration control is crude: the control precision of the CH4 / H2 volume ratio is insufficient. When the ratio exceeds the preferred range of 0.5% to 2%, non-diamond carbon phase (such as graphite phase or amorphous carbon) is easily formed. These non-diamond phases not only have extremely low thermal conductivity, but also act as phonon scattering sources to reduce the overall thermal conductivity and degrade the surface quality.

[0006] (3) Catalyst residue: Some CVD processes use transition metals (such as Fe, Co, Ni) as catalysts to promote nucleation, but the residue of such metal elements in the diamond lattice or grain boundaries will seriously scatter phonons and impair thermal conductivity.

[0007] (4) Substrate warping and thermal stress: There is a significant difference in the coefficient of thermal expansion (CTE) between Si substrate and diamond (Si: 2.6 ppm / K, Diamond: 1.0 ppm / K). Thermal mismatch stress is easily generated during the cooling process after deposition, which leads to substrate warping or even cracking, seriously affecting the yield and reliability.

[0008] (5) Lack of interface thermal resistance management: In the existing composite structure design of PCD substrate and heat sink, there is a lack of systematic optimization scheme for interface thermal resistance. Problems such as insufficient adhesion of metallization layer and high porosity of solder layer lead to high interface thermal resistance, which weakens the high thermal conductivity advantage of diamond substrate.

[0009] Therefore, it is necessary to develop a new polycrystalline diamond composite heat dissipation substrate and its preparation method to overcome the above problems. Summary of the Invention

[0010] The purpose of this invention is to provide a high thermal conductivity polycrystalline diamond composite heat dissipation substrate and its preparation method, so as to solve the technical problems in the prior art such as low thermal conductivity of polycrystalline diamond, difficulty in controlling impurities, substrate warping, and high interface thermal resistance.

[0011] This invention is implemented as follows: This invention provides a method for preparing a polycrystalline diamond composite heat dissipation substrate, comprising the following steps: Step 1, Substrate pretreatment and seed nucleation: After cleaning and surface roughening the Si / Mo substrate, a nanodiamond seed layer is coated. Step 2, preparation of ultra-high purity gas system: use hydrogen purified by Pd-Ag alloy membrane purifier and methane with purity ≥7N as reaction gas source, and control the partial pressure of O2 and N2 impurities in the reaction chamber to be <10 ppb. Step 3, Microwave plasma ignition and parameter setting: Ignite hydrogen plasma in the microwave plasma CVD system and adjust the substrate surface temperature to 800℃ to 950℃. Step 4, CH4 introduction and diamond deposition: Control the CH4 / H2 volume ratio to 0.5% to 2% and grow a polycrystalline diamond film on the substrate surface to a thickness of 300 μm to 1000 μm. Step 5, Cooling and Separation from the Substrate: Separate the deposited diamond film from the substrate to obtain a free-standing polycrystalline diamond plate. Step 6, Chemical Mechanical Polishing: The free-standing polycrystalline diamond plate is polished on both sides to make the surface roughness Ra of the crystal-attached surface ≤ 5 nm.

[0012] Further, in step one: the cleaning process involves sequentially ultrasonic cleaning with acetone for 10 minutes, rinsing with isopropanol for 5 minutes, rinsing with deionized water, and drying with N2; the surface roughening treatment involves blasting with 120-mesh Al2O3 to control the Ra of the substrate surface to 0.8μm to 1.5μm; the nanodiamond seed layer uses ND@SiO2 composite particles with a particle size of 100 nm to 200 nm, dispersed in isopropanol at a concentration of 0.5 mg / mL to 2 mg / mL; the nucleation density is controlled to 1×10⁻⁶. 8 cm -2 Up to 1×10 10 cm -2 Surface contact angle < 30°.

[0013] Furthermore, in step two: the hydrogen source with a purity ≥6N is purified by a Pd-Ag alloy membrane purifier at 350℃ to 450℃, and the outlet purity reaches 7N; The gas delivery pipeline is made of electrolytically polished stainless steel or Monel alloy; the concentrations of O2 and N2 in the chamber are monitored in real time using an online gas chromatograph-mass spectrometer or a Fourier transform infrared spectrometer.

[0014] Furthermore, in step three: the absolute pressure of the cavity is set to 100 Torr to 200 Torr; the microwave power is gradually increased to 2 kW to 4 kW to ignite the plasma; the substrate surface temperature is 850°C to 900°C, and the temperature uniformity is controlled within ±15°C; after 10 to 15 minutes of stable operation, it is confirmed that the plasma is uniform and there is no local arcing.

[0015] Furthermore, in step four: the CH4 / H2 volume ratio is 0.8% to 1.5%; the deposition rate is 1 μm / h to 5 μm / h; online Raman spectroscopy is performed every 24 hours during the deposition process to control the sp³ / sp² peak intensity ratio to be >100:1; and the CH4 valve is closed after the target thickness is reached.

[0016] Further, in step five: after closing the CH4 valve, maintain the H2 plasma for 10 minutes to etch the non-diamond carbon on the surface; slowly reduce the microwave power at a rate of 50 W / min to 100 W / min, and cool the substrate with an H2 airflow of 500 sccm to 1000 sccm; after the substrate temperature drops below 200°C, turn off the microwave and purge the cavity with H2; separate the PCD film from the substrate using laser lift-off or chemical etching, and the resulting board warpage is <50 μm / 20 mm.

[0017] Furthermore, in step six: rough polishing is performed using 6μm diamond plaster at a pressure of 300 g / cm. 2 Up to 400 g / cm 2Rotation speed 80 rpm to 100 rpm, removing 10μm to 20μm particles; intermediate polishing using 1μm diamond paste, pressure 200 g / cm. 2 Up to 300 g / cm 2 Rotation speed 60 to 80 rpm, removing 3 to 5 μm particles; fine polishing using colloidal SiO2 polishing slurry with pH 9 to 10, pressure 100 g / cm. 2 Up to 150 g / cm 2 Rotation speed 40 rpm to 60 rpm to remove 1 μm to 2 μm; after polishing, ultrasonic cleaning with deionized water and drying with N2; back surface roughness controlled to Ra≤50 nm.

[0018] The present invention also provides a polycrystalline diamond heat dissipation substrate prepared by the above-described method, wherein the polycrystalline diamond heat dissipation substrate has the following characteristics: Thermal conductivity at room temperature ≥1800 W / (m·K); Nitrogen impurity concentration < 5 × 10 16 atoms / cm³; Metal catalyst residue was not detected. Surface roughness Ra of the laminated surface ≤ 5 nm; Plate warpage < 50 μm / 20 mm; The Raman spectrum sp³ / sp² peak intensity ratio is >100:1.

[0019] The present invention also provides a composite structure based on the above-mentioned polycrystalline diamond heat dissipation substrate, comprising: The polycrystalline diamond heat dissipation substrate; The metallization layer is deposited on the working surface (referring to the crystal-attached surface) of the polycrystalline diamond heat dissipation substrate by sputtering or electron beam evaporation. The metallization layer consists of a Ti adhesion layer, a Pt or W diffusion barrier layer, and an Au solderable layer from bottom to top. And a Cu / Mo heat sink that is bonded to the metallization layer by Au-Sn eutectic bonding or nano-Ag sintering paste; The composite structure has an interfacial shear strength ≥ 20 MPa and an interfacial thermal resistance < 5 × 10⁻⁶ MPa. -6 m 2 ·K / W.

[0020] Furthermore, the thickness of the Ti adhesive layer is 50 nm to 100 nm, the thickness of the Pt or W diffusion barrier layer is 100 nm or 200 nm, and the thickness of the Au solderable layer is 500 nm. The back side (opposite to the working surface) of the polycrystalline diamond heat sink substrate is coated with a Cu layer with a thickness of 1μm to 3μm. The substrate has a laser-processed positioning groove on its edge, with a groove width of 0.2 mm to 0.5 mm and a groove depth of 0.1 mm to 0.3 mm. The back of the substrate is provided with micro blind holes processed by femtosecond laser, with a hole diameter of 50μm to 100μm and a hole depth of 100μm to 200μm, and the holes are filled with nanodiamond composite thermal interface material. The substrate has a laser-etched brand logo intaglio mark on its edge or back.

[0021] The present invention has the following beneficial effects: Compared with the prior art, the present invention has the following outstanding advantages and beneficial effects: 1. Breakthrough improvement in thermal conductivity: By systematically controlling the purity of the gas source (H2≥7N, CH4≥7N), trace impurities in the cavity (O2 and N2 both <10 ppb), and precise process parameters (CH4 / H2 ratio 0.5% to 2%, temperature 850℃ to 900℃), the room temperature thermal conductivity of the prepared polycrystalline diamond substrate can reach ≥1800 W / (m·K), far exceeding the level of conventional PCD (800 W / (m·K) to 1500 W / (m·K)), and approaching the performance of single-crystal diamond, realizing a leap in the performance of polycrystalline diamond heat dissipation substrates.

[0022] Extremely low impurity and defect density: This invention controls the nitrogen impurity concentration to <5×10⁻⁶. 16 atoms / cm 3 (Tens of ppb) No metal catalyst residue was detected, effectively eliminating the scattering effect of impurity atoms on phonons and ensuring high thermal conductivity. At the same time, the high sp³ / sp² ratio (>100:1) ensures the intrinsic high crystallinity of the material.

[0023] Solving the problems of substrate warpage and thermal stress: By optimizing the cooling rate (50 W / min to 100 W / min), using progressive laser lift-off, and selecting Mo substrate (CTE is closer to diamond), thermal mismatch stress was effectively controlled, and the resulting board warpage was <50μm / 20mm, with no cracks or peeling damage.

[0024] Systematic optimization of interface thermal resistance: Through the design of Ti / Pt / Au or Ti / W / Au multilayer metallization system (adhesion layer + diffusion barrier layer + solderable layer), low thermal resistance bonding of Au-Sn eutectic bonding or nano-Ag sintering paste, and micro-blind via TIM filling scheme, the interface thermal resistance is reduced to <5×10⁻ 6 m²·K / W, fully leveraging the high thermal conductivity advantage of diamond substrates.

[0025] Complete industrial application solutions: This invention not only provides a method for preparing the core PCD substrate, but also designs a metallization layer system, a Cu / Mo gradient thermal expansion matching composite structure, a micro-blind via TIM filling scheme, and a laser marking process, forming a complete chain of technical solutions from material preparation to packaging applications. It can be directly connected to packaging production lines for high-power LEDs, 5G / 6G RF devices, AI computing chips, automotive power modules, etc.

[0026] Excellent process controllability and reproducibility: Each step has clear quality inspection standards and failure response mechanisms. Closed-loop quality control of the entire process is achieved through online GC-MS / FTIR, Raman spectroscopy and other monitoring methods, ensuring consistency and yield between batches. Attached Figure Description

[0027] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 A flowchart illustrating the preparation method of a polycrystalline diamond composite heat dissipation substrate provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the composite structure of the polycrystalline diamond heat dissipation substrate provided in an embodiment of the present invention. Detailed Implementation

[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] like Figure 1 and Figure 2 As shown, the present invention provides a method for preparing a polycrystalline diamond composite heat dissipation substrate, comprising the following steps: Step 1: Substrate pretreatment and seed nucleation: This step aims to provide high-density, uniform, and well-bonded nucleation sites for the heteroepitaxial growth of high-quality polycrystalline diamond.

[0031] Single-crystal silicon wafers (Si(100)) or molybdenum (Mo) wafers with (100) crystal plane orientation are selected as growth substrates. The substrate size is set according to the target product specifications, preferably a circular wafer with a diameter of 2 inches to 4 inches or a square wafer with a side length of 20 mm × 20 mm. The substrate thickness is controlled within the range of 0.5 mm to 1.0 mm. Before growth, the substrate is ultrasonically cleaned in acetone for 10 minutes to remove surface organic contaminants, then transferred to isopropanol for rinsing for 5 minutes, then thoroughly rinsed with deionized water, and finally dried with high-purity nitrogen gas (N2, purity ≥ 99.999%).

[0032] To improve the adhesion rate and nucleation density of diamond crystal nuclei, the cleaned substrate surface was physically roughened using 120-mesh alumina (Al2O3) blasting particles. By adjusting the blasting pressure and time, the arithmetic mean roughness (Ra) of the substrate surface was precisely controlled between 0.8 μm and 1.5 μm. This roughness range provides sufficient mechanical locking sites while avoiding excessive roughness that could degrade the surface smoothness of the subsequently deposited diamond film.

[0033] Nanodiamond particles (preferably core-shell structured ND@SiO2 composite particles) with a particle size of 100 nm to 200 nm were dispersed in isopropanol to prepare a seed suspension with a concentration of 0.5 mg / mL to 2 mg / mL. To ensure the monodispersity of the nanoparticles, the suspension was ultrasonically dispersed for 15 minutes before use. The suspension was then coated onto a roughened substrate surface using a spin-coating method with a spin speed of 3000 rpm and a coating time of 30 seconds; or a dip-coating method was used with a pull-up speed controlled at 1 mm / s to 5 mm / s. After coating, the substrate was dried in an oven at 80°C for 30 minutes to form a uniform and tightly bonded nanodiamond seed layer on the substrate surface.

[0034] The seed layer was characterized using field emission scanning electron microscopy (FE-SEM), and its nucleation density needed to reach 1×10⁻⁶. 8 cm -2 Up to 1×10 10 cm -2 Meanwhile, the activation level of the substrate surface is evaluated using a static contact angle meter. The contact angle of deionized water on its surface should be less than 30° to ensure good hydrophilicity.

[0035] Countermeasures for failure: If SEM observation shows that the seed particles have obvious agglomeration, polyvinylpyrrolidone (PVP) at 0.1% of the total mass of solute should be introduced into the seed suspension as a dispersant, and then ultrasonically dispersed before coating; if the nucleation density does not reach the lower limit of the standard, the concentration of the seed suspension should be increased to 2 mg / mL or the spin coating operation should be repeated 2 to 3 times to compensate until it passes the acceptance test.

[0036] Step 2: Preparation of the Ultra-High Purity Gas System This step aims to completely eliminate impurity atoms, especially nitrogen (N) and oxygen (O) and their compounds, from the gas source, providing a pure reaction atmosphere for subsequent deposition.

[0037] The hydrogen source uses high-purity hydrogen cylinders with a purity ≥6N (99.9999%), and its output pipeline is connected to a Pd-Ag alloy membrane purifier. This purifier operates at temperatures between 350℃ and 450℃, utilizing the selective permeation principle of the palladium-silver alloy membrane to effectively remove residual impurities such as O2, H2O, and N2 from the hydrogen, raising the purity of the output hydrogen to 7N (99.99999%). The methane source directly uses ultra-high-purity methane cylinders with a purity ≥7N (99.99999%), which are precisely metered by a mass flow controller (MFC) before entering the reaction chamber.

[0038] All gas delivery pipelines are made of electropolished stainless steel (EP-SS) or Monel alloy to avoid secondary contamination caused by gas escaping from the pipe walls. Before each batch of processes goes online, the chambers and pipelines are purged with high-purity helium (He) for 30 minutes, followed by evacuation to an absolute pressure ≤1×10⁻⁻. 5 Torr. During the deposition preparation stage, start the online gas chromatography-mass spectrometry (GC-MS) or Fourier transform infrared spectroscopy (FTIR) connected to the chamber to monitor the residual gas composition in the chamber in real time. Only after confirming that the partial pressure of O2 is <10 ppb and the partial pressure of N2 is <10 ppb can the next step be carried out.

[0039] Countermeasures for failure: If monitoring detects that the O2 concentration exceeds the standard, immediately check whether the operating temperature of the Pd-Ag purifier deviates from the set range and check the sealing of the pipeline joints; if the N2 concentration exceeds the standard, consider replacing the CH4 cylinder or installing a low-temperature adsorption trap in the gas pipeline for deep removal of nitrogen.

[0040] Step 3: Microwave plasma ignition and parameter setting This step aims to establish a stable and uniform microwave plasma, enabling the substrate to reach the temperature range required for diamond growth.

[0041] A microwave plasma chemical vapor deposition (MPCVD) system with a frequency of 2.45 GHz was used, equipped with a microwave power source (adjustable output power from 1.5 kW to 6 kW) and an infrared pyrometer for non-contact substrate surface temperature monitoring. Ultra-high purity H2, confirmed to be suitable in Example 2, was introduced into the cavity, and the cavity absolute pressure was set to 100 Torr to 200 Torr. The microwave source was activated using a step-by-step, slow power increase method, gradually increasing the power to 2 kW to 4 kW to ignite the H2 plasma. A typical blue-violet glow was observed at this point.

[0042] The substrate surface temperature is read in real time using an infrared pyrometer. The microwave power is fine-tuned to stabilize the substrate temperature within a process window of 800°C to 950°C, preferably 850°C to 900°C. Under these conditions, the plasma is maintained in stable operation for 10 to 15 minutes. Visual inspection confirms that the plasma spheres uniformly coat the substrate surface without localized arcing or abnormal discharge phenomena. The power-temperature-pressure steady-state curve under these conditions is recorded and saved as a batch process reference.

[0043] The quality inspection standards are: the temperature uniformity of the substrate surface is controlled within ±15℃, and the plasma color is uniform and free of impurities (no yellow N2 emission lines).

[0044] Troubleshooting: If plasma jitter or instability occurs, temporarily suspend CH4 introduction, reduce microwave power by 10%, and extend the stabilization time to 30 minutes; if the substrate temperature cannot reach the set value, check the microwave coupling antenna insertion depth and cavity resonant mode matching.

[0045] Step 4: CH4 Introduction and Diamond Deposition This step introduces a carbon source based on the aforementioned steady-state hydrogen plasma to achieve long-term growth of high-quality polycrystalline diamond films.

[0046] Based on the steady-state H2 plasma established in Example 3, the CH4 mass flow controller valve was opened at an extremely slow rate (approximately 0.5 sccm / min) to gradually increase the CH4 / H2 volume ratio to a target range of 0.5% to 2%, preferably 0.8% to 1.5%. Under these conditions, the diamond deposition rate was approximately 1 μm / h to 5 μm / h, and the total deposition time was calculated based on the target thickness (e.g., for a 500 μm thickness, approximately 167 hours at a rate of 3 μm / h).

[0047] During the deposition process, the following key parameters were continuously monitored: substrate surface temperature (infrared pyrometer), microwave forward and reflection power, cavity absolute pressure, CH4 / H2 flow ratio, and online readings of O2 and N2 impurities. Online Raman spectroscopy was performed every 24 hours through the cavity observation window to confirm the characteristic peak of sp³ diamond (1332 cm⁻¹). -1 The non-diamond carbon peak (1350 cm⁻¹) is dominant. -1 Up to 1550 cm -1 The concentration of ions is extremely low, with a peak intensity ratio of sp³ / sp² > 100:1, i.e., I(sp³) / I(sp²) > 100:1. After growing to the target thickness (300 μm to 1000 μm), the CH4 mass flow controller valve is slowly closed.

[0048] Countermeasures for failure: If Raman detection shows a significant non-diamond carbon phase (graphite phase), immediately reduce the CH4 / H2 ratio by 0.2% and appropriately increase the H2 flow rate to enhance the plasma etching effect; if the deposition rate is too low, the microwave power can be slightly increased (the increase should not exceed 5%), but the substrate temperature must be ensured not to exceed the upper limit of 950℃.

[0049] Step 5: Cooling and separating from the substrate (releasing the free-standing plate) This step aims to safely cool down and release the PCD film from the Si / Mo substrate to obtain a freestanding diamond plate.

[0050] After closing the CH4 valve, maintain pure H2 plasma for 10 minutes to etch away any remaining non-diamond carbon phase on the surface. Then, gradually reduce the microwave power from 50 W / min to 100 W / min while continuously cooling the substrate with an H2 gas flow from 500 sccm to 1000 sccm. Once the substrate temperature drops below 200°C, turn off the microwave power and continue purging the cavity with H2 for 10 minutes.

[0051] The deposited sample is removed, and the PCD film is separated from the substrate using either laser lift-off or chemical etching. For Si substrates, Si can be selectively removed using an HNA solution (a mixture of hydrofluoric acid, nitric acid, and acetic acid); for Mo substrates, FeCl3 solution can be used for etching. Laser lift-off is preferred, where a 248 nm or 355 nm excimer laser scans the back side of the substrate, causing the material at the interface to vaporize instantaneously and achieve separation. A free-standing PCD plate is obtained.

[0052] The quality inspection standards are: flatness of the board (warping < 50μm / 20mm); no cracks and no peeling damage.

[0053] Countermeasures for failures: If warping is severe, the temperature gradient should be reduced during the deposition process in Example 4, or a Mo substrate should be used instead (Mo has a CTE of 5.1 ppm / K, which is closer to diamond's 1.0 ppm / K than Si's 2.6 ppm / K, resulting in less thermal mismatch stress); if breakage occurs during separation, a progressive multi-channel laser ablation strategy (reducing the energy density of a single scan and increasing the number of scans) should be adopted to reduce thermal stress impact.

[0054] Step Six: CMP Double-Sided Polishing This step aims to obtain an ultra-smooth surface (Ra≤5 nm), suitable for direct chip bonding.

[0055] Double-sided polishing is performed using a chemical mechanical polishing (CMP) process. This process consists of three stages: Rough polishing: Using 6μm diamond paste, apply pressure of 300 g / cm² to 400 g / cm², and rotate the polishing pad at 80 rpm to 100 rpm to remove a thickness of about 10μm to 20μm, achieving rapid surface smoothing.

[0056] Medium polishing: Using 1μm diamond paste, apply a pressure of 200 g / cm² to 300 g / cm² and a rotation speed of 60 rpm to 80 rpm to remove a thickness of about 3μm to 5μm, further reducing surface roughness.

[0057] Fine polishing: Using colloidal silica (SiO2) polishing slurry with pH 9 to 10, apply a pressure of 100 g / cm² to 150 g / cm² and a rotation speed of 40 rpm to 60 rpm to remove a thickness of about 1 μm to 2 μm, so that the surface roughness Ra of the laminated surface is ≤5 nm.

[0058] After polishing, the PCD board is ultrasonically cleaned in deionized water for 10 minutes and then dried with high-purity N2. Depending on the application requirements, the surface for chip bonding (the side where the chip is bonded) requires Ra ≤ 5 nm, while the back surface can be relaxed to Ra ≤ 50 nm.

[0059] Quality inspection: Atomic force microscope (AFM) measurement of the surface Ra ≤ 5 nm; optical microscope (100×) observation of the surface showed no scratches.

[0060] Countermeasures for failure: If a hazy residue appears on the surface, extend the polishing time and replace with fresh polishing fluid; if the edges are cracked, use a protective ring to fix the PCD board before polishing.

[0061] Step 7: Metallization layer deposition and composite structure assembly To impart excellent solderability and interfacial thermal conductivity to the high thermal conductivity PCD substrate and achieve high reliability composite with the heat sink, this step involves constructing a metallization system on the surface of the PCD substrate and performing thermo-press bonding.

[0062] Metallization layer sputtering deposition: Multiple metal films are sequentially deposited on the working surface (crystal-mounted surface) of the PCD substrate using magnetron sputtering or electron beam evaporation. The structure is designed as follows: a titanium (Ti) adhesion layer, 50 nm to 100 nm thick, to enhance the chemical bonding between the diamond and the metal layers; a platinum (Pt) or tungsten (W) diffusion barrier layer, 100 nm or 200 nm thick, to suppress inter-diffusion between the solder and the substrate during subsequent soldering; and a gold (Au) solderable layer, 500 nm thick, providing excellent wettability and an oxidation-resistant surface. As a preferred option, an additional copper (Cu) layer, 1 μm to 3 μm thick, is electroplated or sputtered on the non-crystal-mounted surface (back side) of the PCD substrate to improve thermal expansion compatibility and solder wettability with the copper / molybdenum (Cu / Mo) composite substrate.

[0063] Hot-press composite bonding: The metallized PCD substrate is aligned and stacked with a pre-prepared Cu / Mo heat sink, using Au-Sn (gold-tin) eutectic solder (eutectic temperature 280℃) or nano-silver (Ag) sintering paste (sintering temperature 250℃) as the intermediate bonding layer. The bonding process is carried out in a hot-pressing device, applying an axial pressure of 0.5 MPa to 2.0 MPa and holding for 10 to 30 minutes to allow the solder to fully melt or sinter densely, forming a PCD-on-Carrier composite heat dissipation structure. After bonding, the substrate is cooled to room temperature in the furnace, and the surface is ultrasonically cleaned with anhydrous ethanol or a special cleaning agent to remove residual flux or organic matter.

[0064] Quality inspection: The interfacial shear strength is evaluated using a DAGE push-shear tester, and is required to be no less than 20 MPa; the interfacial thermal resistance is determined using the time-domain thermal reflectometry (TDTR) method, and the target value is less than 5 × 10⁻⁶ MPa. -6 m 2 ·K / W.

[0065] Countermeasures for failure: If the interface is found to have pores or voids, the bonding pressure can be increased to above 2 MPa, or the nano silver sintering paste can be replaced (which has higher sintering density and lower thermal resistance); if the metallization layer peels off, the thickness of the Ti adhesive layer can be increased to 100 nm to enhance the bonding force, and the ion cleaning process before sputtering can be optimized (Ar plasma bombardment for 5 minutes).

[0066] Step 8: Physical Structure Fabrication and Full Performance Verification This step aims to finalize the substrate dimensions, fabricate functional microstructures, and perform comprehensive performance characterization to ensure the product meets design specifications.

[0067] Positioning Structure and Micro-Blind Via Fabrication: Using a femtosecond laser micromachining system, positioning alignment grooves are fabricated on the edge of the PCD substrate. The groove width is 0.2 mm to 0.5 mm, and the groove depth is 0.1 mm to 0.3 mm to facilitate precise coating and encapsulation alignment of the subsequent thermal interface material (TIM). Subsequently, a diamond wire saw is used to cut the substrate to the target finished size (e.g., 20 mm × 20 mm square or custom specifications). Further, a micro-blind via array is fabricated on the back side of the substrate (non-crystal-mounted side) using a femtosecond laser. The via diameter is controlled to be 50 μm to 100 μm, and the via depth is 100 μm to 200 μm. The vias are filled with a high thermal conductivity nanodiamond composite thermal interface material (TIM) to significantly reduce device-level thermal resistance.

[0068] Brand logo laser etching: A low-power femtosecond laser is used to etch brand logos and product traceability codes on the edge or back non-functional area of ​​the PCD substrate, forming intaglio markings. By controlling the laser parameters (power < 1W, scanning speed > 100mm / s), the etching depth is ensured to be only 1μm to 5μm, without damaging the substrate's structure and mechanical properties.

[0069] Comprehensive Performance Testing and Acceptance Standards: Finished PCD substrates must pass the following comprehensive performance tests: Thermal conductivity measurement: Laser flash method (LFA) was used, and the test value at room temperature should reach ≥1800 W / (m·K); Impurity content analysis: Nitrogen impurity concentration was detected using secondary ion mass spectrometry (SIMS), with a target value below 5 × 10¹. 6 atoms / cm³ (corresponding to tens of ppb), and the residues of metallic elements (catalytic metals such as Fe, Co, and Ni) were at undetectable levels; Interface performance retest: TDTR method was used to verify the interface thermal resistance <5×10⁻ 6 m²·K / W, DAGE shear strength ≥20 MPa; Surface quality inspection: Atomic force microscopy (AFM) confirmed that the roughness of the surface to which the crystal is attached is Ra≤5 nm, and no scratches or chipping are visible to the naked eye under an optical microscope.

[0070] Countermeasures for failure: If the final thermal conductivity does not reach the standard of ≥1800 W / (m·K), the process backtracking mechanism should be activated immediately. The gas purity records, CH4 / H2 volume ratio control curves, and O2 / N2 impurity online monitoring data from Examples 2 to 4 should be carefully reviewed to identify any potential impurity introduction points during the growth process. If edge chipping occurs during the micro-blind hole fabrication, the femtosecond laser pulse energy should be further reduced and the scanning path optimized. The extremely short pulse width (<300 fs) generates a very small heat-affected zone (HAZ < 1 μm) to avoid thermal damage.

[0071] In summary, the present invention has the following outstanding advantages and beneficial effects: 1. Breakthrough improvement in thermal conductivity: By systematically controlling the purity of the gas source (H2≥7N, CH4≥7N), trace impurities in the cavity (O2 and N2 both <10 ppb), and precise process parameters (CH4 / H2 ratio 0.5% to 2%, temperature 850℃ to 900℃), the room temperature thermal conductivity of the prepared polycrystalline diamond substrate can reach ≥1800 W / (m·K), far exceeding the level of conventional PCD (800 W / (m·K) to 1500 W / (m·K)), and approaching the performance of single-crystal diamond, realizing a leap in the performance of polycrystalline diamond heat dissipation substrates.

[0072] Extremely low impurity and defect density: This invention controls the nitrogen impurity concentration to <5×10⁻⁶. 16 atoms / cm 3 (Tens of ppb) No metal catalyst residue was detected, effectively eliminating the scattering effect of impurity atoms on phonons and ensuring high thermal conductivity. At the same time, the high sp³ / sp² ratio (>100:1) ensures the intrinsic high crystallinity of the material.

[0073] Solving the problems of substrate warpage and thermal stress: By optimizing the cooling rate (50 W / min to 100 W / min), using progressive laser lift-off, and selecting Mo substrate (CTE is closer to diamond), thermal mismatch stress was effectively controlled, and the resulting board warpage was <50μm / 20mm, with no cracks or peeling damage.

[0074] Systematic optimization of interface thermal resistance: Through the design of Ti / Pt / Au or Ti / W / Au multilayer metallization system (adhesion layer + diffusion barrier layer + solderable layer), low thermal resistance bonding of Au-Sn eutectic bonding or nano-Ag sintering paste, and micro-blind via TIM filling scheme, the interface thermal resistance is reduced to <5×10⁻ 6 m²·K / W, fully leveraging the high thermal conductivity advantage of diamond substrates.

[0075] Complete industrial application solutions: This invention not only provides a method for preparing the core PCD substrate, but also designs a metallization layer system, a Cu / Mo gradient thermal expansion matching composite structure, a micro-blind via TIM filling scheme, and a laser marking process, forming a complete chain of technical solutions from material preparation to packaging applications. It can be directly connected to packaging production lines for high-power LEDs, 5G / 6G RF devices, AI computing chips, automotive power modules, etc.

[0076] Excellent process controllability and reproducibility: Each step has clear quality inspection standards and failure response mechanisms. Closed-loop quality control of the entire process is achieved through online GC-MS / FTIR, Raman spectroscopy and other monitoring methods, ensuring consistency and yield between batches.

[0077] The polycrystalline diamond heat dissipation substrate, its preparation method, and composite structure provided by this invention can be widely used in electronic devices that require efficient heat dissipation, such as high-power semiconductor lasers, 5G / 6G communication RF chips, GaN power amplifiers, data center CPUs / GPUs, and electric vehicle power modules (such as IGBTs and SiC MOSFETs). It has significant industrial application value and market promotion prospects.

[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a polycrystalline diamond composite heat dissipation substrate, characterized in that, Includes the following steps: Step 1, Substrate pretreatment and seed nucleation: After cleaning and surface roughening the Si / Mo substrate, a nanodiamond seed layer is coated. Step 2, preparation of ultra-high purity gas system: use hydrogen purified by Pd-Ag alloy membrane purifier and methane with purity ≥7N as reaction gas source, and control the partial pressure of O2 and N2 impurities in the reaction chamber to be <10 ppb. Step 3, Microwave plasma ignition and parameter setting: Ignite hydrogen plasma in the microwave plasma CVD system and adjust the substrate surface temperature to 800℃ to 950℃. Step 4, CH4 introduction and diamond deposition: Control the CH4 / H2 volume ratio to 0.5% to 2% and grow a polycrystalline diamond film on the substrate surface to a thickness of 300 μm to 1000 μm. Step 5, Cooling and Separation from the Substrate: Separate the deposited diamond film from the substrate to obtain a free-standing polycrystalline diamond plate. Step 6, Chemical Mechanical Polishing: The free-standing polycrystalline diamond plate is polished on both sides to make the surface roughness Ra of the crystal-attached surface ≤ 5 nm.

2. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 1, characterized in that, In step one: The cleaning process involves sequentially ultrasonic cleaning with acetone for 10 minutes, rinsing with isopropanol for 5 minutes, rinsing with deionized water, and drying with N2. The surface roughening treatment involves sandblasting with 120-mesh Al2O3 to control the Ra of the substrate surface to 0.8μm to 1.5μm. The nanodiamond seed layer consists of ND@SiO2 composite particles with a particle size of 100 nm to 200 nm, dispersed in isopropanol at a concentration of 0.5 mg / mL to 2 mg / mL. Nucleation density controlled at 1×10 8 cm -2 Up to 1×10 10 cm -2 Surface contact angle < 30°.

3. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 1, characterized in that, In step two: The hydrogen source has a purity of ≥6N and is purified by a Pd-Ag alloy membrane purifier at 350℃ to 450℃, resulting in an outlet purity of 7N. The gas delivery pipeline is made of electrolytically polished stainless steel or Monel alloy; the concentrations of O2 and N2 in the chamber are monitored in real time using an online gas chromatograph-mass spectrometer or a Fourier transform infrared spectrometer.

4. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 1, characterized in that, In step three: The absolute pressure of the cavity is set to 100 Torr to 200 Torr; the microwave power is gradually increased to 2 kW to 4 kW to ignite the plasma; the substrate surface temperature is 850℃ to 900℃, and the temperature uniformity is controlled within ±15℃; after 10 to 15 minutes of stable operation, the plasma is confirmed to be uniform without local arcing.

5. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 1, characterized in that, In step four: the CH4 / H2 volume ratio is 0.8% to 1.5%; the deposition rate is 1 μm / h to 5 μm / h; online Raman spectroscopy is performed every 24 hours during the deposition process to control the sp³ / sp² peak intensity ratio to be >100:1; the CH4 valve is closed after the target thickness is reached.

6. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 5, characterized in that, In step five: after closing the CH4 valve, maintain the H2 plasma for 10 minutes to etch the non-diamond carbon on the surface; slowly reduce the microwave power at a rate of 50 W / min to 100 W / min, and cool the substrate with an H2 airflow of 500 sccm to 1000 sccm; after the substrate temperature drops below 200°C, turn off the microwave and purge the cavity with H2; separate the PCD film from the substrate using laser lift-off or chemical etching, and the resulting board warpage is <50μm / 20mm.

7. The method for preparing the polycrystalline diamond composite heat dissipation substrate as described in claim 1, characterized in that, In step six: rough polishing is performed using 6μm diamond plaster at a pressure of 300 g / cm. 2 Up to 400 g / cm 2 Rotation speed 80 rpm to 100 rpm, removing 10μm to 20μm particles; intermediate polishing using 1μm diamond paste, pressure 200 g / cm. 2 Up to 300 g / cm 2 Rotation speed 60 to 80 rpm, removing 3 to 5 μm particles; fine polishing using colloidal SiO2 polishing slurry with pH 9 to 10, pressure 100 g / cm. 2 Up to 150 g / cm 2 Rotation speed 40 rpm to 60 rpm to remove 1 μm to 2 μm particles; after polishing, ultrasonic cleaning with deionized water and drying with N2; back surface roughness controlled to Ra≤50 nm.

8. A polycrystalline diamond heat dissipation substrate prepared by the preparation method according to any one of claims 1 to 7, wherein the polycrystalline diamond heat dissipation substrate has the following characteristics: Thermal conductivity at room temperature ≥1800 W / (m·K); Nitrogen impurity concentration < 5 × 10 16 atoms / cm³; Metal catalyst residue was not detected. Surface roughness Ra of the laminated surface ≤ 5 nm; Plate warpage < 50 μm / 20 mm; The Raman spectrum sp³ / sp² peak intensity ratio is >100:

1.

9. A composite structure based on the polycrystalline diamond heat dissipation substrate of claim 8, characterized in that, include: The polycrystalline diamond heat dissipation substrate; The metallization layer is deposited on the working surface of the polycrystalline diamond heat dissipation substrate by sputtering or electron beam evaporation. The metallization layer consists of a Ti adhesion layer, a Pt or W diffusion barrier layer, and an Au solderable layer from bottom to top. And a Cu / Mo heat sink that is bonded to the metallization layer by Au-Sn eutectic bonding or nano-Ag sintering paste; The composite structure has an interfacial shear strength ≥ 20 MPa and an interfacial thermal resistance < 5 × 10⁻⁶ MPa. -6 m 2 ·K / W.

10. The composite structure as described in claim 9, characterized in that: The thickness of the Ti adhesive layer is 50 nm to 100 nm, the thickness of the Pt or W diffusion barrier layer is 100 nm or 200 nm, and the thickness of the Au solderable layer is 500 nm. The back side of the polycrystalline diamond heat dissipation substrate is coated with a Cu layer with a thickness of 1μm to 3μm. The substrate has a laser-processed positioning groove on its edge, with a groove width of 0.2 mm to 0.5 mm and a groove depth of 0.1 mm to 0.3 mm. The back of the substrate is provided with micro blind holes processed by femtosecond laser, with a hole diameter of 50μm to 100μm and a hole depth of 100μm to 200μm, and the holes are filled with nanodiamond composite thermal interface material. The substrate has a laser-etched brand logo intaglio mark on its edge or back.