Anti-warpage packaging structure and its formation method
By introducing an anti-warping layer with a coefficient of thermal expansion between that of the bridging chip and the conductive plug on at least one side of the substrate, the warping deformation problem caused by the difference in coefficient of thermal expansion of the packaging structure is solved, and a packaging structure with high reliability and high-density interconnection is achieved.
Patent Information
- Application Number
- CN202611186673.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-10
AI Technical Summary
Existing packaging structures warp and deform due to differences in the coefficients of thermal expansion of materials, affecting product reliability and yield.
An anti-warping layer is introduced on at least one side of the substrate. Its coefficient of thermal expansion is between that of the bridging chip and the conductive plug, which optimizes the thermal stress distribution of the package structure. The anti-warping layer acts as a stress buffer between the bridging chip and the conductive plug, thereby reducing warping deformation.
It significantly reduces warpage caused by differences in the coefficients of thermal expansion of materials, improves the reliability and yield of the packaging structure, and supports high-density I/O fan-out and system-level integration.
Smart Images

Figure CN123076271A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor manufacturing technology, and in particular to an anti-warpage packaging structure and its formation method. Background Technology
[0002] With the rapid development of the semiconductor industry, chip manufacturing faces increasing challenges. At extremely small sizes, physical bottlenecks become more difficult to overcome, leading to rising R&D and production costs, declining product yields, and a gradual slowdown of Moore's Law, ushering in the post-Moore era for the semiconductor industry. Traditional packaging can no longer meet the new demands represented by artificial intelligence and high-performance computing. Leading companies in the semiconductor manufacturing field have begun to shift their focus from improving wafer manufacturing technology nodes to exploring innovations in system-in-package (SiP) technologies, giving rise to advanced packaging technologies.
[0003] Advanced packaging technologies have significantly improved chip performance by modifying packaging methods without shrinking process nodes. Fan-out packaging technologies, including Fan-Out Wafer Level Packaging (FOWLP) and Fan-Out Panel Level Packaging (FOPLP), have been a major driving force behind the advancement of advanced packaging. Emerging 2.5D and 3D packaging technologies further expand the application potential of flip-chip and wafer-level packaging processes by vertically stacking multiple chips, achieving more efficient input / output. Against the backdrop of the rapidly increasing computing power demands of artificial intelligence, these packaging technologies need to support higher frequencies and faster speeds of finer circuitry to shorten data transmission distances between chips, improve chip-to-die collaboration efficiency, thereby enhancing system performance and reducing overall power consumption.
[0004] However, there are still many problems with the packaging structure in the existing technology. Summary of the Invention
[0005] The technical problem solved by the present invention is to provide an anti-warping packaging structure and a method for forming the same, so as to improve the warping deformation of the packaging structure.
[0006] To address the aforementioned problems, the present invention provides an anti-warpage packaging structure, comprising: a substrate having a bridging chip and a plurality of conductive plugs therein, the conductive plugs penetrating the substrate, the substrate having a first side and a second side opposite to each other; an anti-warpage layer located at least on one side of the substrate, the anti-warpage layer having through holes exposing the corresponding end surfaces of the conductive plugs, the thermal expansion coefficient of the anti-warpage layer being greater than that of the bridging chip, and the thermal expansion coefficient of the anti-warpage layer being less than that of the conductive plugs; a first redistribution layer located on the first side of the substrate, and electrically connected to the conductive plugs and the bridging chip respectively; a second redistribution layer located on the second side of the substrate, and electrically connected to the conductive plugs and the bridging chip respectively; and a chip structure located on the first redistribution layer, and electrically connected to the first redistribution layer.
[0007] Optionally, the anti-warping layer is located on a first side of the substrate, and the anti-warping layer is located between the substrate and the first redistribution layer.
[0008] Optionally, the anti-warping layer is located on the second side of the substrate, and the anti-warping layer is located between the substrate and the second redistribution layer.
[0009] Optionally, the anti-warping layer is located on the first side and the second side of the substrate, and the anti-warping layer is located between the substrate and the second redistribution layer, and between the substrate and the second redistribution layer.
[0010] Optionally, the material of the anti-warping layer includes silicon oxide or silicon nitride.
[0011] Optionally, the wiring width and spacing of the second wiring layer are both greater than those of the first wiring layer.
[0012] Optionally, it may also include: a plurality of solder balls located on the second rewiring layer, the solder balls being electrically connected to the second rewiring layer.
[0013] Accordingly, the present invention also provides a method for forming an anti-warpage packaging structure, comprising: forming a substrate having a bridging chip and a plurality of conductive plugs therein, the conductive plugs penetrating the substrate, the substrate having a first side and a second side opposite to each other; forming an anti-warpage layer on at least one side of the substrate, the anti-warpage layer having through holes, the through holes exposing the corresponding end surfaces of the conductive plugs, the coefficient of thermal expansion of the anti-warpage layer being greater than the coefficient of thermal expansion of the bridging chip, and the coefficient of thermal expansion of the anti-warpage layer being less than the coefficient of thermal expansion of the conductive plugs; forming a first redistribution layer, the first redistribution layer being located on a first side of the substrate, and the first redistribution layer being electrically connected to the conductive plugs and the bridging chip respectively; forming a second redistribution layer, the second redistribution layer being located on a second side of the substrate, and the second redistribution layer being electrically connected to the conductive plugs and the bridging chip respectively; and providing a chip structure, the chip structure being located on the first redistribution layer, and the chip structure being electrically connected to the first redistribution layer.
[0014] Optionally, the anti-warping layer is formed on a first side of the substrate, and the anti-warping layer is located between the substrate and the first redistribution layer.
[0015] Optionally, the anti-warping layer is formed on the second side of the substrate, and the anti-warping layer is located between the substrate and the second redistribution layer.
[0016] Optionally, the anti-warping layer is formed on the first side and the second side of the substrate, and the anti-warping layer is located between the substrate and the second redistribution layer, and between the substrate and the second redistribution layer.
[0017] Optionally, before forming the anti-warping layer, the method further includes: performing stress simulation on the packaging structure to obtain the stress distribution; and determining the formation location and thickness of the anti-warping layer based on the simulation results.
[0018] Optionally, thermal stress simulation of the packaging structure can be performed based on finite element analysis.
[0019] Optionally, the method for forming the anti-warping layer includes: forming an anti-warping material layer on one side of the substrate using a chemical vapor deposition process; and performing patterned etching on the anti-warping material layer until the end surface of the corresponding conductive plug is exposed, thereby forming the anti-warping layer.
[0020] Compared with the prior art, the technical solution of the present invention has the following advantages: In the anti-warpage packaging structure of the present invention, by introducing the anti-warpage layer on at least one side of the substrate, the thermal expansion coefficient of the anti-warpage layer, which is between that of the bridging chip and the conductive plug, is utilized to achieve optimized control of the thermal stress distribution of the packaging structure. Specifically, since the thermal expansion coefficient of the anti-warpage layer is greater than that of the bridging chip but less than that of the conductive plug, the anti-warpage layer can act as a stress buffer between the bridging chip and the conductive plug when the temperature changes. On the one hand, the expansion degree of the anti-warpage layer is higher than that of the bridging chip, which can moderately compensate for the low expansion trend of the bridging chip and avoid local stress concentration in the bridging chip area due to excessive contraction or expansion; on the other hand, the expansion degree of the anti-warpage layer is lower than that of the conductive plug, which can constrain the highly expanding conductive plug and suppress its displacement amplitude caused by thermal expansion and contraction. Based on the added anti-warpage layer, the warpage deformation caused by the large difference in the thermal expansion coefficients of the materials in each layer can be significantly reduced. In addition, the via design on the anti-warping layer ensures reliable exposure of the conductive plug end surface, providing a structural basis for the electrical connection between the first and second rewiring layers and the conductive plug and the bridging chip, respectively.
[0021] Furthermore, the wiring width and spacing of the second redistribution layer are both greater than those of the first redistribution layer. This double-sided redistribution layer design, with the wiring width and spacing of the second redistribution layer being greater than those of the first redistribution layer, enables the chip structure to achieve high-density I / O fan-out, meeting the fine interconnection requirements of advanced process chips and forming a smooth interconnection transition from chip to system level.
[0022] Furthermore, it also includes a plurality of solder balls located on the second overlay layer, the solder balls being electrically connected to the second overlay layer. The solder balls provide a standardized package interface, facilitating surface mount soldering to the PCB board, improving package manufacturability and system-level integration capabilities. Simultaneously, the solder ball array design supports higher I / O density, achieving reliable electrical connection between the package and external circuits, enhancing product application compatibility and assembly efficiency.
[0023] In the method for forming an anti-warpage packaging structure according to the technical solution of the present invention, an anti-warpage layer is formed on at least one side of the substrate. Utilizing the characteristic that the coefficient of thermal expansion of the anti-warpage layer is between that of the bridging chip and the conductive plug, optimized control of the thermal stress distribution of the packaging structure is achieved. Specifically, since the coefficient of thermal expansion of the anti-warpage layer is greater than that of the bridging chip but less than that of the conductive plug, the anti-warpage layer can act as a stress buffer between the bridging chip and the conductive plug when the temperature changes. On the one hand, the expansion degree of the anti-warpage layer is higher than that of the bridging chip, which can moderately compensate for the low expansion trend of the bridging chip and prevent local stress concentration in the bridging chip area due to excessive contraction or expansion. On the other hand, the expansion degree of the anti-warpage layer is lower than that of the conductive plug, which can constrain the highly expanding conductive plug and suppress its displacement caused by thermal expansion and contraction. Based on the added anti-warpage layer, warpage deformation caused by significant differences in the coefficients of thermal expansion of the various layers can be significantly reduced. In addition, the via design on the anti-warping layer ensures reliable exposure of the conductive plug end surface, providing a structural basis for the electrical connection between the first and second rewiring layers and the conductive plug and the bridging chip, respectively.
[0024] Furthermore, before forming the anti-warping layer, the process includes: performing stress simulation on the packaging structure to obtain the stress distribution; and determining the formation location and thickness of the anti-warping layer based on the simulation results. Through simulation-driven precise design, the anti-warping layer can be specifically placed in stress concentration areas to achieve optimal stress buffering, avoiding material waste and process redundancy caused by blindly adding layers. This allows for the prediction and mitigation of reliability risks during the product development stage, shortening the R&D cycle and reducing trial-and-error costs.
[0025] Furthermore, thermal stress simulation of the packaging structure is performed using finite element analysis. This method accurately simulates the thermal expansion and stress transfer processes of each material layer under temperature changes, precisely identifying stress concentration areas and warpage risk points. Attached Figure Description
[0026] Figures 1 to 11 This is a schematic diagram of the steps in the method for forming the anti-warping packaging structure in an embodiment of the present invention; Figure 12 This is a schematic diagram of the anti-warping packaging structure in another embodiment of the present invention; Figure 13 This is a schematic diagram of the anti-warping packaging structure in another embodiment of the present invention. Detailed Implementation
[0027] As described in the background section, existing packaging structures still have many problems. These will be explained in detail below.
[0028] In CoPoS (Chip-on-Panel-on-Substrate) packaging technology, epoxy resin molding material encapsulates the copper pillars and silicon chip. The coefficient of thermal expansion (CTE) of the copper pillars is approximately 17 ppm / ℃, while the silicon chip has an extremely low CTE of only 2.6 to 3.0 ppm / ℃. The epoxy resin molding material, however, has the highest CTE, reaching 30 to 45 ppm / ℃. This significant difference in CTE among the three materials leads to a substantial stress mismatch when the device experiences temperature changes due to varying degrees of expansion and contraction. This inherent stress can easily cause irregular warping deformation of the package, resulting in interlayer delamination or separation failure, severely impacting product reliability and yield.
[0029] Based on this, the present invention provides an anti-warpage packaging structure and its formation method. By forming the anti-warpage layer on at least one side of the substrate, the thermal expansion coefficient of the anti-warpage layer, which is between that of the bridging chip and the conductive plug, optimizes and controls the thermal stress distribution of the packaging structure. Specifically, since the thermal expansion coefficient of the anti-warpage layer is greater than that of the bridging chip but less than that of the conductive plug, the anti-warpage layer can act as a stress buffer between the bridging chip and the conductive plug when the temperature changes. On the one hand, the expansion degree of the anti-warpage layer is higher than that of the bridging chip, which can moderately compensate for the low expansion trend of the bridging chip and avoid local stress concentration in the bridging chip area due to excessive contraction or expansion. On the other hand, the expansion degree of the anti-warpage layer is lower than that of the conductive plug, which can constrain the highly expanding conductive plug and suppress its displacement caused by thermal expansion and contraction. Based on the added anti-warpage layer, the warpage deformation caused by the large difference in the thermal expansion coefficients of the materials in each layer can be significantly reduced. In addition, the via design on the anti-warping layer ensures reliable exposure of the conductive plug end surface, providing a structural basis for the electrical connection between the first and second rewiring layers and the conductive plug and the bridging chip, respectively.
[0030] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0031] Figures 1 to 11 This is a schematic diagram of the steps in the method for forming the anti-warping packaging structure in an embodiment of the present invention.
[0032] A substrate is formed, which includes a bridging chip and several conductive plugs that penetrate the substrate. The substrate has opposing first and second sides. Please refer to [reference needed for detailed formation process] for more information. Figures 1 to 4 .
[0033] Please refer to Figure 1 Provide the first temporary carrier board 100.
[0034] In this embodiment, the first temporary carrier board 100 serves as the basic support platform for subsequent panel-level packaging processes. Its surface flatness and thermal stability directly affect the forming accuracy of subsequent layer metal structures. The first temporary carrier board 100 adopts a square panel, which can process dozens to hundreds of individual packaging structures in parallel in a single process cycle, significantly improving manufacturing efficiency and equipment capacity utilization.
[0035] In this embodiment, the panel material of the first temporary carrier board 100 can be glass or stainless steel, which have low coefficient of thermal expansion (CTE) and good thermal compatibility with the metal layer. This effectively reduces warping and interlayer stress concentration caused by thermal mismatch in subsequent high-temperature processes, ensures the pattern fidelity of the redistribution layer and conductive plug layer formed later, and ensures the dimensional consistency and electrical performance uniformity of each individual package structure under large-area mass production conditions.
[0036] Please refer to Figure 2 An electroplating seed layer 101 is formed on the first temporary carrier plate 100; a photoresist layer 102 is formed on the electroplating seed layer 101, and the photoresist layer 102 has a plurality of plug holes 103.
[0037] In this embodiment, the electroplating seed layer 101 is typically formed into a titanium-copper composite structure using a sputtering process to provide a conductive substrate. Subsequently, a photoresist material layer is coated onto the surface of the electroplating seed layer 101, and a photolithography process is used to form a photoresist layer 102 containing the plug via 103. The plug via 103 within the photoresist layer 102 defines the position of the conductive plug.
[0038] Please refer to Figure 3 The conductive plug 104 is formed in the plug through hole 103 by electroplating; after the conductive plug 104 is formed, the photoresist layer 102 is removed.
[0039] In this embodiment, the conductive plug 104 is formed by filling the plug through hole 103 with copper metal through an electroplating process. The conductive plug 104 will constitute a vertically interconnected conductive channel in the substrate.
[0040] Please refer to Figure 4 After removing the photoresist layer 102, a bridging chip 105 is provided and disposed on the electroplating seed layer 101; a molding compound 106 is formed on the electroplating seed layer 101, and the molding compound 106 exposes one end surface of the conductive plug 104.
[0041] In this embodiment, the molding compound 106 covers the sidewalls and bottom area of the conductive plug 104, as well as the bridging chip 105, while precisely controlling the molding compound thickness to expose one end surface of the conductive plug 104. This structural design allows the molding compound 106 to provide mechanical support and insulating isolation, while the exposed end face of the conductive plug 104 is used to achieve a reliable electrical connection with the subsequently formed redistribution layer, together forming the core interconnect foundation of the package structure.
[0042] In this embodiment, the method for forming the molding layer 106 includes: forming a molding material layer (not shown) on the electroplating seed layer 101, the molding material layer covering the conductive plug 104 and the bridging chip 105; and grinding the molding material layer until the end surface of the conductive structure is exposed to form the molding layer 106.
[0043] In this embodiment, the molding compound 106 is made of epoxy molding compound (EMC). Epoxy molding compound has excellent mechanical strength, thermal stability, and insulation properties.
[0044] Thus, the substrate fabrication is complete, wherein the electroplating seed layer 101 is located on the first side of the substrate, and the side exposing the end surface of the conductive plug 104 is the second side of the substrate.
[0045] After forming the substrate, an anti-warping layer is formed on at least one side of the substrate. The anti-warping layer has through-holes that expose the corresponding end surfaces of the conductive plug 104. The coefficient of thermal expansion of the anti-warping layer is greater than that of the bridging chip 105, and less than that of the conductive plug 104. For a detailed formation process, please refer to [reference needed]. Figures 5 to 6 .
[0046] In this embodiment, the anti-warping layer is formed on the second side of the substrate as an example.
[0047] Please refer to Figure 5 An anti-warping material layer 107 is formed on the second side of the substrate.
[0048] In this embodiment, the anti-warping material layer 107 is formed using a chemical vapor deposition process.
[0049] Please continue to refer to this. Figure 5 In this embodiment, before forming the anti-warping material layer 107, the molding layer 106 is opened to expose the pins of the bridging chip 105; the holes in the molding layer 106 are filled with metal material to form chip leads 108, which are electrically connected to the pins of the bridging chip 105.
[0050] It should be noted that, since the size of the bridging chip 105 is smaller than that of the conductive plug 104, when the conductive plug 104 is exposed on the second side of the substrate, the bridging chip 105 is still completely covered by the molding compound 106 and cannot be directly accessed. Therefore, the molding compound 106 needs to be perforated to expose the pins of the bridging chip 105, and the holes are filled with metal material to form the chip leads 108. The chip leads 108 extend the pins of the bridging chip 105 outward, thereby establishing an electrical connection channel between the bridging chip 105 and the subsequently formed second rewiring layer, ensuring that the interconnection function of the bridging chip 105 is realized, and avoiding the problem of the bridging chip 105 being buried and failing due to size difference.
[0051] Please refer to Figure 6 The anti-warping material layer 107 is patterned and etched until the end surface of the corresponding conductive plug 104 is exposed, forming the anti-warping layer 109, which has a plurality of through holes 115.
[0052] By forming the anti-warping layer 109 on at least one side of the substrate, and utilizing the characteristic that the coefficient of thermal expansion of the anti-warping layer 109 is between that of the bridging chip 105 and the conductive plug 104, the thermal stress distribution of the package structure can be optimized and controlled. Specifically, since the coefficient of thermal expansion of the anti-warping layer 109 is greater than that of the bridging chip 105 but less than that of the conductive plug 104, the anti-warping layer 109 can act as a stress buffer between the bridging chip 105 and the conductive plug 104 when the temperature changes. On the one hand, the expansion degree of the anti-warping layer 109 is higher than that of the bridging chip 105, which can moderately compensate for the low expansion trend of the bridging chip 105 and avoid local stress concentration in the area of the bridging chip 105 due to excessive contraction or expansion; on the other hand, the expansion degree of the anti-warping layer 109 is lower than that of the conductive plug 104, which can constrain the highly expanded conductive plug 104 and suppress its displacement caused by thermal expansion and contraction. Based on the added anti-warping layer 109, warping deformation caused by the significant difference in the coefficients of thermal expansion of the materials in each layer can be significantly reduced. In addition, the through-hole 115 design on the anti-warping layer 109 can ensure reliable exposure of the end surface of the conductive plug 104, providing a structural basis for the electrical connection between the first rewiring layer and the second rewiring layer and the conductive plug 104 and the bridging chip 105, respectively.
[0053] In this embodiment, the method for patterning the anti-warping material layer 107 includes: forming a patterned layer on the anti-warping material layer 107, the patterned layer exposing a portion of the top surface of the anti-warping material layer 107; performing dry etching on the anti-warping material layer 107 using the patterned layer as a mask to form the anti-warping layer 109; and removing the patterned layer after forming the anti-warping layer 109.
[0054] In this embodiment, the purpose of patterning and etching openings in the anti-warping material layer 107 is to expose the end surface of the conductive plug 104, ensuring that the subsequent second wiring layer can form a reliable electrical connection with the conductive plug 104, thereby achieving electrical conductivity between the two sides of the substrate. Simultaneously, since the chip lead 108 has already led the pins of the bridging chip 105 out from the molding layer 106, the via 115 on the anti-warping layer 109 also needs to expose the end face of the chip lead 108 so that the subsequent second wiring layer can electrically connect with the chip lead 108, thereby connecting the bridging chip 105 to the overall circuit and ensuring that the interconnection function of the bridging chip 105 is realized.
[0055] In this embodiment, the anti-warping layer 109 is made of silicon oxide.
[0056] In other embodiments, the anti-warping layer may also be made of silicon nitride.
[0057] In this embodiment, before forming the anti-warping layer 109, the method further includes: performing stress simulation on the packaging structure to obtain the stress distribution; and determining the formation location and thickness of the anti-warping layer 109 based on the simulation results. Through simulation-driven precise design, the anti-warping layer 109 can be specifically placed in stress concentration areas to achieve optimal stress buffering, avoiding material waste and process redundancy caused by blindly adding layers. This allows for the prediction and avoidance of reliability risks during the product development stage, shortening the R&D cycle and reducing trial-and-error costs.
[0058] In this embodiment, thermal stress simulation of the packaging structure is performed based on finite element analysis. Using finite element analysis to simulate thermal stress in the packaging structure can accurately simulate the thermal expansion and stress transfer process of each layer of material under temperature changes, and accurately identify stress concentration areas and warping risk points.
[0059] Please refer to Figure 7 A second rewiring layer 110 is formed, which is located on the second side of the substrate and is electrically connected to the conductive plug 104 and the bridge chip 105 respectively.
[0060] In this embodiment, the second redistribution layer 110 is electrically connected to the bridging chip 105 based on the chip lead 108, and the anti-warping layer 109 is located between the substrate and the second redistribution layer 110.
[0061] In this embodiment, the second redistribution layer 110 is formed on the second side of the substrate through thin film deposition, photolithography patterning, and electroplating processes.
[0062] Please refer to Figure 8 After the second redistribution layer 110 is formed, a plurality of solder balls 111 are formed on the second redistribution layer 110, and the solder balls 111 are electrically connected to the second redistribution layer 110.
[0063] The solder balls 111 provide a standardized packaging interface, facilitating surface mount soldering to the PCB board, improving the manufacturability and system-level integration capabilities of the package. At the same time, the solder ball array design supports higher I / O density, enabling reliable electrical connection between the package and external circuits, and enhancing the application compatibility and assembly efficiency of the product.
[0064] Please refer to Figure 9 After forming the solder balls 111, a second temporary carrier 112 is provided and the second temporary carrier 112 is bonded to the second redistribution layer 110; after bonding the second temporary carrier 112, the first temporary carrier 100 is debonded and removed, and the electroplating seed layer 101 is removed.
[0065] It should be noted that, in this embodiment, after the solder balls 111 are prepared, the second redistribution layer 110 is bonded to the second temporary carrier board 112 (typically made of glass, silicon, or ceramic). The core function of the second temporary carrier board 112 is to provide a rigid load-bearing platform, maintaining the flatness and dimensional stability of the overall structure during the subsequent fabrication and high-temperature curing of the first redistribution layer, and preventing warping and pattern distortion caused by material stress.
[0066] In this embodiment, the first temporary carrier plate 100 is debonded using thermal, optical, or mechanical methods.
[0067] Please refer to Figure 10 A first rewiring layer 113 is formed, which is located on the first side of the substrate and is electrically connected to the conductive plug 104 and the bridge chip 105 respectively.
[0068] In this embodiment, the first redistribution layer 113 is formed on the first side of the substrate through thin film deposition, photolithography patterning, and electroplating processes.
[0069] In this embodiment, the wiring width and spacing of the second redistribution layer 110 are both greater than those of the first redistribution layer 113. This double-sided redistribution layer design, with the wiring width and spacing of the second redistribution layer 110 being greater than those of the first redistribution layer 113, enables the chip structure to achieve high-density I / O fan-out, meeting the fine interconnection requirements of advanced process chips and forming a smooth interconnection transition from chip to system level.
[0070] Please refer to Figure 11 A chip structure 114 is provided, the chip structure 114 is located on the first redistribution layer 113, and the chip structure 114 is electrically connected to the first redistribution layer 113.
[0071] In this embodiment, the chip structure 114 is a system-on-a-chip (SoC) or a high-bandwidth memory (HBM) chip. The SoC is a chip integrating a central processing unit, a graphics processing core, and dedicated hardware acceleration units, with a microbump array density exceeding two hundred contacts per square millimeter, imposing sub-micron level precision requirements on the linewidth, spacing, and signal integrity of the first rewiring layer 113. The HBM is a memory structure formed by vertically stacking multiple layers of Dynamic Random Access Memory (DRAM) wafers through through-silicon vias, possessing terabits per second data transfer capability and nanometer-level alignment precision requirements. The two are heterogeneously integrated using thermoforming or flip-chip bonding processes, melting and interconnecting the microbumps to the first rewiring layer 113 to form ultra-short electrical paths to reduce transmission latency and power consumption.
[0072] In this embodiment, the main function of embedding the bridge chip 105 within the substrate is to achieve high-density, high-bandwidth interconnection between multiple chips. The bridge chip 105 provides fine wiring channels within the substrate, connecting adjacent chip structures 114, breaking through the limitations of traditional package pin spacing, reducing signal delay and power consumption, and improving the integration and communication efficiency of multi-chip systems.
[0073] In this embodiment, after the chip structure 114 is electrically connected to the first redistribution layer 113, the second temporary carrier 112 is debonded and removed.
[0074] Accordingly, this invention also provides an anti-warping packaging structure, please refer to [link / reference needed]. Figure 11The system includes: a substrate having a bridging chip 105 and a plurality of conductive plugs 104 therein, the conductive plugs 104 penetrating the substrate, the substrate having opposing first and second sides; an anti-warping layer 109 located at least on one side of the substrate, the anti-warping layer 109 having through holes 115, the through holes 115 exposing the end surfaces of corresponding conductive plugs 104, the coefficient of thermal expansion of the anti-warping layer 109 being greater than the coefficient of thermal expansion of the bridging chip 105, and the coefficient of thermal expansion of the anti-warping layer 109 being less than the coefficient of thermal expansion of the conductive plugs 104; the first A first wiring layer 113 is located on a first side of the substrate and is electrically connected to the conductive plug 104 and the bridging chip 105, respectively; a second wiring layer 110 is located on a second side of the substrate and is electrically connected to the conductive plug 104 and the bridging chip 105, respectively; and a chip structure 114 is located on the first wiring layer 113 and is electrically connected to the first wiring layer 113.
[0075] By introducing the anti-warping layer 109 on at least one side of the substrate, and utilizing the characteristic that the coefficient of thermal expansion of the anti-warping layer 109 is between that of the bridging chip 105 and the conductive plug 104, the thermal stress distribution of the package structure can be optimized and controlled. Specifically, since the coefficient of thermal expansion of the anti-warping layer 109 is greater than that of the bridging chip 105 but less than that of the conductive plug 104, the anti-warping layer 109 can act as a stress buffer between the bridging chip 105 and the conductive plug 104 when the temperature changes. On the one hand, the expansion degree of the anti-warping layer 109 is higher than that of the bridging chip 105, which can moderately compensate for the low expansion trend of the bridging chip 105 and avoid local stress concentration in the area of the bridging chip 105 due to excessive contraction or expansion; on the other hand, the expansion degree of the anti-warping layer 109 is lower than that of the conductive plug 104, which can constrain the highly expanded conductive plug 104 and suppress its displacement caused by thermal expansion and contraction. Based on the added anti-warping layer 109, warping deformation caused by the significant difference in the coefficients of thermal expansion of the materials in each layer can be significantly reduced. In addition, the through-hole 115 design on the anti-warping layer 109 can ensure reliable exposure of the end surface of the conductive plug 104, providing a structural basis for the electrical connection of the first rewiring layer 113 and the second rewiring layer 110 to the conductive plug 104 and the bridging chip 105, respectively.
[0076] In this embodiment, the anti-warping layer 109 is located on the second side of the substrate, and the anti-warping layer 109 is located between the substrate and the second redistribution layer 110.
[0077] In this embodiment, the anti-warping layer 109 is made of silicon oxide.
[0078] In other embodiments, the anti-warping layer 109 may also be made of silicon nitride.
[0079] In this embodiment, the wiring width and spacing of the second redistribution layer 110 are both greater than those of the first redistribution layer 113. This double-sided redistribution layer design, with the wiring width and spacing of the second redistribution layer 110 being greater than those of the first redistribution layer 113, enables the chip structure 114 to achieve high-density I / O fan-out, meeting the fine interconnection requirements of advanced process chips and forming a smooth interconnection transition from chip to system level.
[0080] In this embodiment, the system further includes a plurality of solder balls 111 located on the second redistribution layer 110, the solder balls 111 being electrically connected to the second redistribution layer 110. The solder balls 111 provide a standardized packaging interface, facilitating surface mount soldering to the PCB board, improving the package's manufacturability and system-level integration capabilities. Simultaneously, the solder ball array design supports higher I / O density, achieving reliable electrical connection between the package and external circuits, enhancing product application compatibility and assembly efficiency.
[0081] Figure 12 This is a schematic diagram of the anti-warping packaging structure in another embodiment of the present invention.
[0082] This embodiment is based on the above embodiment ( Figure 11 Based on the previous embodiment, the description of the anti-warpage packaging structure will continue. The rest is the same as the previous embodiment, except that the anti-warpage layer 109 is formed at a different location. The following will provide a detailed description in conjunction with the accompanying drawings.
[0083] Please refer to Figure 12 The anti-warping layer 109 is located on the first side of the substrate, and the anti-warping layer 109 is located between the substrate and the first redistribution layer 113.
[0084] In this embodiment, the anti-warping layer 109 is located only on the first side of the substrate, and its manufacturing process is the same as that in the above embodiment where the anti-warping layer 109 is disposed on the second side of the substrate, and will not be described again here.
[0085] Figure 13 This is a schematic diagram of the anti-warping packaging structure in another embodiment of the present invention.
[0086] This embodiment is based on the above embodiment ( Figure 11Based on the previous embodiment, the description of the anti-warpage packaging structure will continue. The rest is the same as the previous embodiment, except that the anti-warpage layer 109 is formed at a different location. The following will provide a detailed description in conjunction with the accompanying drawings.
[0087] Please refer to Figure 13 The anti-warping layer 109 is located on the first side and the second side of the substrate, respectively, and the anti-warping layer 109 is located between the substrate and the second redistribution layer 110, and between the substrate and the second redistribution layer 110.
[0088] In this embodiment, the fabrication process of forming the anti-warping layer 109 on the first side of the substrate is the same as the fabrication process of setting the anti-warping layer 109 on the second side of the substrate, and will not be described again here.
[0089] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. An anti-warpage packaging structure, characterized in that, include: A substrate having a bridging chip and a plurality of conductive plugs therein, the conductive plugs penetrating the substrate, the substrate having a first side and a second side opposite to each other; An anti-warping layer is located at least on one side of the substrate, the anti-warping layer has through holes that expose the corresponding end surface of the conductive plug, the coefficient of thermal expansion of the anti-warping layer is greater than the coefficient of thermal expansion of the bridging chip, and the coefficient of thermal expansion of the anti-warping layer is less than the coefficient of thermal expansion of the conductive plug. The first wiring layer is located on the first side of the substrate and is electrically connected to the conductive plug and the bridge chip respectively. The second wiring layer is located on the second side of the substrate and is electrically connected to the conductive plug and the bridge chip respectively. A chip structure is located on the first wiring layer and is electrically connected to the first wiring layer.
2. The anti-warpage packaging structure as described in claim 1, characterized in that, The anti-warping layer is located on the first side of the substrate, and the anti-warping layer is located between the substrate and the first redistribution layer.
3. The anti-warpage packaging structure as described in claim 1, characterized in that, The anti-warping layer is located on the second side of the substrate, and the anti-warping layer is located between the substrate and the second redistribution layer.
4. The anti-warping packaging structure as described in claim 1, characterized in that, The anti-warping layers are located on the first and second sides of the substrate, respectively, and are located between the substrate and the second redistribution layer, and between the substrate and the second redistribution layer, respectively.
5. The anti-warping packaging structure as described in claim 1, characterized in that, The anti-warping layer is made of silicon oxide or silicon nitride.
6. The anti-warping packaging structure as described in claim 1, characterized in that, The wiring width and spacing of the second wiring layer are both greater than those of the first wiring layer.
7. The anti-warpage packaging structure as described in claim 1, characterized in that, Also includes: A plurality of solder balls are located on the second overlay layer, and the solder balls are electrically connected to the second overlay layer.
8. A method for forming an anti-warpage packaging structure, characterized in that, include: A substrate is formed, wherein a bridging chip and a plurality of conductive plugs are present in the substrate, the conductive plugs penetrate the substrate, and the substrate has a first side and a second side opposite to each other. An anti-warping layer is formed on at least one side of the substrate. The anti-warping layer has through holes that expose the corresponding end surface of the conductive plug. The coefficient of thermal expansion of the anti-warping layer is greater than that of the bridging chip and less than that of the conductive plug. A first wiring layer is formed, the first wiring layer is located on a first side of the substrate, and the first wiring layer is electrically connected to the conductive plug and the bridge chip respectively. A second wiring layer is formed, which is located on the second side of the substrate and is electrically connected to the conductive plug and the bridging chip, respectively. A chip structure is provided, the chip structure is located on the first overlay layer, and the chip structure is electrically connected to the first overlay layer.
9. The method for forming the anti-warpage packaging structure as described in claim 8, characterized in that, The anti-warping layer is formed on a first side of the substrate and is located between the substrate and the first redistribution layer.
10. The method for forming the anti-warpage packaging structure as described in claim 8, characterized in that, The anti-warping layer is formed on the second side of the substrate and is located between the substrate and the second redistribution layer.
11. The method for forming the anti-warpage packaging structure as described in claim 8, characterized in that, The anti-warping layers are formed on the first and second sides of the substrate, respectively, and are located between the substrate and the second redistribution layer, and between the substrate and the second redistribution layer.
12. The method for forming the anti-warpage packaging structure as described in claim 8, characterized in that, Before forming the anti-warping layer, the process further includes: performing stress simulation on the packaging structure to obtain the stress distribution; and determining the formation location and thickness of the anti-warping layer based on the simulation results.
13. The method for forming the anti-warpage packaging structure as described in claim 12, characterized in that, Thermal stress simulation of the packaging structure is performed using finite element analysis.
14. The method for forming the anti-warpage packaging structure as described in claim 8, characterized in that, The method for forming the anti-warping layer includes: forming an anti-warping material layer on one side of the substrate using a chemical vapor deposition process; and performing patterned etching on the anti-warping material layer until the end surface of the corresponding conductive plug is exposed, thereby forming the anti-warping layer.