Rubber compositions containing hydrocarbon waxes based on pyrolysis fractions
By using a combination of hydrocarbon waxes produced from the pyrolysis of polyethylene raw materials, diene elastomers, reinforcing fillers, and crosslinking systems in pneumatic tires, the problems of high fossil resource consumption and the impact of recycled material performance are solved, improving tire fatigue strength and reducing environmental burden.
Patent Information
- Application Number
- CN202580026921.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-11
- Filing Date
- 2025-04-03
- Publication Date
- 2026-11-10
AI Technical Summary
The current manufacturing process of pneumatic tires uses a large amount of fossil resources, and the recycled rubber materials have a negative impact on tire performance, resulting in an environmental burden. Furthermore, existing technologies have failed to effectively utilize pyrolysis oil and intermediate products.
A rubber composition was prepared by combining a hydrocarbon wax produced from the pyrolysis of a main polyethylene-containing raw material with a diene elastomer, reinforcing filler, and crosslinking system to optimize fatigue strength properties.
This improves the fatigue strength of rubber compositions while reducing the use of fossil resources, achieving effective utilization of pyrolysis oil and reducing environmental impact.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of rubber compositions, particularly rubber compositions for pneumatic tires. Background Technology
[0002] Both pneumatic tires (more commonly rubber products, such as conveyor belts) and non-pneumatic tires are complex objects composed of numerous components. For example, a pneumatic tire is made up of more than 200 different raw materials.
[0003] While some raw materials, such as natural rubber, are derived from renewable resources, many components of pneumatic tires still come from fossil resources. Therefore, it is crucial to minimize the use of these resources through biological sources or by recycling used materials.
[0004] However, the recycling of materials, such as those derived from used plastics or rubber products, remains limited, particularly due to the primary impact of their composition on tire performance. In fact, recycling these materials can have an overall negative environmental impact due to the performance degradation of pneumatic tires made from them.
[0005] Extensive research has been conducted in the field of recycled products for their use in pneumatic tires, particularly regarding the recovery of oils from the pyrolysis of tire residues. For example, documents EP 0928817, WO 2013 / 170358, and JP2017 / 008214 teach the preparation of tire-grade carbon black using the pyrolysis of pneumatic tire scrap. Other studies have addressed the recovery of intermediate products. Document WO90 / 14409 relates to the separation of pyrolysis oil from tire residues by distillation in order to recover recyclable compounds, particularly limonene.
[0006] Reference CA 3 032 242 describes the catalytic depolymerization of plastics used to manufacture monomers and waxes. However, the utilization of the resulting effluents remains unresolved.
[0007] The applicant continued his research and found that rubber compositions containing hydrocarbon waxes produced by the pyrolysis of raw materials primarily containing polyethylene exhibited improved fatigue strength properties while retaining other properties.
[0008] definition The carbon-containing compounds mentioned in the specification can be fossil-derived compounds or bio-based compounds. In the case of bio-based compounds, they can be partially or completely derived from biomass or obtained from renewable starting materials derived from biomass.
[0009] C n A compound is a compound containing n carbon atoms. Similarly, "C n -C m A "compound" refers to a group of compounds containing n to m carbon atoms.
[0010] Heteroatoms are atoms other than carbon or hydrogen, such as nitrogen, sulfur, or oxygen.
[0011] As is known, the term "mainly" means accounting for at least 50% of the weight. Summary of the Invention
[0012] The present invention relates to a rubber composition based on at least one elastomer matrix, reinforcing filler, crosslinking system and hydrocarbon wax, wherein the hydrocarbon wax is based on a fraction produced by the pyrolysis of a raw material mainly comprising polyethylene, the fraction comprising up to 5% by weight of a compound containing up to 24 carbon atoms and up to 5% by weight of a compound containing at least 38 carbon atoms.
[0013] rubber composition elastomer The rubber composition according to the invention comprises at least one elastomer, preferably a diene elastomer. It should be recalled that "diene-type elastomer" should be understood as an elastomer that is at least partially (i.e., a homopolymer or copolymer) derived from a diene monomer (a monomer with two conjugated or non-conjugated carbon-carbon double bonds).
[0014] These diene elastomers can be classified into two categories: "substantially unsaturated" or "substantially saturated." The term "substantially unsaturated" generally refers to a diene elastomer that is at least partially derived from a conjugated diene monomer and has a diene source (conjugated diene) unit content greater than 15% (mol%). Therefore, diene elastomers such as butyl rubber or EPDM-type copolymers of dienes and α-olefins do not fall into the above definition but can be specifically referred to as "substantially saturated" diene elastomers (low or very low diene source unit content, always less than 15 mol%). The diene elastomers included in the rubber compositions according to the invention are preferably substantially unsaturated.
[0015] The phrase "dien elastomer capable of being used in rubber compositions according to the invention" specifically refers to: a) Any homopolymer of conjugated or non-conjugated diene monomers having 4 to 18 carbon atoms; b) Any copolymer of a conjugated or non-conjugated diene having 4 to 18 carbon atoms with at least one other monomer.
[0016] Other monomers can be ethylene, olefins, or conjugated or non-conjugated dienes.
[0017] Suitable conjugated dienes include those having 4 to 12 carbon atoms, particularly 1,3-dienes, especially, for example, 1,3-butadiene and isoprene.
[0018] Suitable olefins include vinyl aromatic compounds having 8 to 20 carbon atoms and aliphatic α-monoolefins having 3 to 12 carbon atoms.
[0019] Suitable vinyl aromatic compounds include, for example, styrene, (o-, m-, or p-)methylstyrene, commercial mixtures of "vinyltoluene", or p-(tert-butyl)styrene.
[0020] Suitable aliphatic α-monoolefins particularly include noncyclic aliphatic α-monoolefins having 3 to 18 carbon atoms.
[0021] The diene elastomer is preferably a highly unsaturated diene elastomer, particularly selected from natural rubber (NR), synthetic polyisoprene (IR), polybutadiene (BR), butadiene copolymers, isoprene copolymers, and mixtures thereof. More preferably, such copolymers are selected from butadiene-styrene copolymers (SBR), isoprene-butadiene copolymers (BIR), isoprene-styrene copolymers (SIR), isoprene-butadiene-styrene copolymers (SBIR), ethylene-butadiene copolymers (EBR), and mixtures thereof.
[0022] The aforementioned diene elastomers can be, for example, block elastomers, random elastomers, sequential elastomers, or microsequential elastomers, and can be prepared in dispersions or solutions; they can be coupled and / or star-branched or functionalized (e.g., epoxidated) by coupling agents and / or star-branching agents or functionalizing agents.
[0023] The term "isoprene elastomer" refers to isoprene homopolymers or copolymers, in other words, diene elastomers selected from: natural rubber (NR) (which may be plasticized or sol-gelled), synthetic polyisoprene (IR), various isoprene copolymers (especially isoprene-styrene (SIR) copolymers, isoprene-butadiene (BIR) copolymers or isoprene-butadiene-styrene (SBIR) copolymers), and mixtures of these elastomers.
[0024] Preferably, the composition according to the invention comprises at least 50 phr of at least one butadiene elastomer, preferably selected from polybutadiene, butadiene copolymers and mixtures thereof, and preferably selected from polybutadiene, butadiene-styrene copolymers and mixtures thereof.
[0025] According to a preferred embodiment of the invention, the butadiene elastomer is a butadiene copolymer with a glass transition temperature (Tg) less than -20°C, preferably between -20°C and -110°C, more preferably between -60°C and -110°C, and even more preferably between -60°C and -90°C. These elastomers are well known to those skilled in the art and are described, for example, in documents WO 2015 / 185394 and WO 2017 / 168099.
[0026] Preferably, and according to this embodiment, the composition according to the invention comprises at least 70 phr, preferably at least 90 phr, of at least one butadiene copolymer, preferably a butadiene-styrene copolymer.
[0027] Preferably, according to any embodiment of the invention, the composition according to the invention further comprises at least 20 phr of an isoprene elastomer selected from natural rubber, synthetic polyisoprene and mixtures thereof.
[0028] Reinforced packing The rubber composition according to the invention comprises reinforcing fillers. Any type of reinforcing filler known to be capable of reinforcing elastomer compositions that can be used to manufacture pneumatic tires can be used, such as organic fillers like carbon black, reinforcing inorganic fillers like silica, or blends of both types of fillers, particularly blends of carbon black and silica.
[0029] All carbon blacks, especially HAF, ISAF, or SAF type carbon blacks commonly used in tires (“tire-grade” carbon black), are suitable for use as carbon black. Within “tire-grade” carbon black, more specific references will be made to reinforced carbon blacks of the 100, 200, or 300 series (ASTM grades) (e.g., N115, N134, N234, N326, N330, N339, N347, or N375 carbon black), or higher series carbon blacks depending on the target application (e.g., N660, N683, or N772). Carbon black can, for example, be incorporated into isoprene elastomers in masterbatch form (see, for example, applications WO 97 / 36724 and WO 99 / 16600). The BET specific surface area of the carbon black is measured according to standard D6556-10 [multi-point (minimum 5-point) method - gas: nitrogen - relative pressure p / p0 range: 0.1 to 0.3].
[0030] By definition, in this patent application, the term "reinforced inorganic filler" should be understood to mean any inorganic or mineral filler, regardless of its color and origin (natural or synthetic), also referred to as "white filler," "transparent filler," or even "non-black filler" in contrast to carbon black, which is capable of reinforcing rubber compositions intended for use in the manufacture of pneumatic tires without the need for any means other than intermediate coupling agents; in other words, it is capable of replacing conventional tire-grade carbon black in terms of reinforcement. Such fillers are generally characterized by the presence of hydroxyl groups (-OH) on their surface in a known manner.
[0031] Silica-type mineral fillers (preferably silicon dioxide (SiO2)) or alumina-type mineral fillers (especially alumina (Al2O3)) are particularly suitable as reinforcing inorganic fillers.
[0032] The silica used can be any reinforced silica known to those skilled in the art, in particular any precipitated silica or pyrolytic silica.
[0033] Precipitated silica can be prepared from raw materials derived from inorganic sand (silica from inorganic sand), recycled materials such as foundry sand, scrap tires (especially the tread of scrap tires that mainly contain silica as reinforcing filler), or from bio-based raw materials such as plant-derived organic waste (preferably non-edible plant-derived organic waste).
[0034] Among plants containing silica in their tissues, mustard, especially mustard husks, grass, especially bamboo leaves in grass, corn cobs, sugarcane bagasse, rice, wheat, especially rice husks and wheat husks, can be mentioned.
[0035] Silica derived from non-renewable raw materials (such as natural inorganic sand) is typically obtained by heating the sand in a glass-making furnace in the presence of sodium carbonate. The resulting sodium silicate is then dissolved in water, possibly in the presence of an alkali (such as sodium hydroxide). Silica is synthesized from this aqueous solution by controlled treatment of the silicate with an acid (e.g., an inorganic acid and / or an acidifying gas, such as carbon dioxide) to form a precipitate. Sometimes an electrolyte (e.g., sodium sulfate) may be present to promote the formation of precipitated silica particles. The recovered precipitated silica is amorphous precipitated silica.
[0036] Silica derived from bio-based raw materials such as those described above can be obtained, for example, by burning the bio-based raw materials to recover the ash of the bio-based materials, which mainly contain silica. For example, with rice husks, and in methods comparable to those for mineral-based or recycled raw material-based silica described above, rice husk ash is typically treated with a strong alkali, such as sodium hydroxide, to form an aqueous silicate solution (e.g., sodium silicate), followed by controlled addition of an acid (e.g., an inorganic acid and / or an acidifying gas, such as carbon dioxide) to form precipitated synthetic silica, wherein an electrolyte (e.g., sodium sulfate) may be present to promote the formation of precipitated silica particles derived from rice husks. The recovered precipitated silica is amorphous precipitated silica. Silica obtained from rice husk ash is known as RHA silica (rice husk ash silica). Bio-based silica can be obtained from suppliers such as Solvay, Evonik, Quechen, Wilmar International, and Wuxi.
[0037] In summary, the synthesis of precipitated silica, which can be used in the context of this invention, can be carried out using sodium silicate obtained entirely from bio-based raw materials, recycled raw materials, or non-renewable raw materials, or using a mixture of bio-based raw materials and / or recycled raw materials and / or non-renewable raw materials (e.g., commonly used sand).
[0038] Preferably, the precipitated silica, whether obtained from mineral raw materials, recycled raw materials, or bio-based raw materials, has a BET specific surface area and a CTAB specific surface area of less than 450 m². 2 / g, preferably 30 to 400m 2 Within the range of / g, especially 60 to 300m 2 / g.
[0039] Any type of precipitated silica can be used, especially highly dispersed precipitated silica (HDS). These precipitated silicas (which may or may not be highly dispersed precipitated silica) are well known to those skilled in the art.
[0040] For example, the silica described in applications WO 03 / 016215-A1 and WO 03 / 016387-A1 may be mentioned. In commercial HDS, Ultrasil® 5000GR and Ultrasil® 7000GR silica from Evonik may be used in particular, or Zeosil® 1085GR, Zeosil® 1115 MP, Zeosil® 1165MP, Zeosil® Premium 200MP, and Zeosil® HRS 1200 MP silica from Solvay. As non-HDS, the following commercially available silicas can be used: Ultrasil® VN2GR and Ultrasil® VN3GR silicas from Evonik, Zeosil® 175GR silicas from Solvay, Hi-Sil EZ120G(-D), Hi-Sil EZ160G(-D), Hi-Sil EZ200G(-D), Hi-Sil 243LD, Hi-Sil 210 and Hi-Sil HDP 320G silicas from PPG, or K160, K185 and K195 silicas from Wilmar International.
[0041] It is not important what physical state the reinforcing inorganic filler is provided in, whether it is in the form of powder, microspheres, granules, beads, or any other suitable densification form. Of course, the term "reinforcing inorganic filler" also refers to mixtures of different reinforcing inorganic fillers, especially mixtures of highly dispersible silica fillers and / or alumina fillers.
[0042] The reinforcing inorganic filler used (especially if it is silica) preferably has a pH of 45 and 400 μm. 2 Between / g, more preferably between 60 and 300 m 2 BET surface area between / g.
[0043] Preferably, the reinforcing filler of the rubber composition according to the invention comprises 10 to 150 phr, preferably 50 to 130 phr, of silica. In a preferred arrangement, the reinforcing filler comprises primarily silica, and is preferably composed of silica.
[0044] To couple an enhanced inorganic filler to an elastomer, a coupling agent (or binder) that is at least bifunctional, particularly a bifunctional organosilane or polyorganosiloxane, may be optionally used in a known manner to provide a satisfactory chemical and / or physical connection between the inorganic filler (its particle surface) and the elastomer.
[0045] In particular, silane polysulfides referred to as “symmetric” or “asymmetric” based on their specific structure may be used, such as those described in applications WO 03 / 002648 (or US 2005 / 016651) and WO 03 / 002649 (or US 2005 / 016650).
[0046] As examples of silane polysulfides, bis((C1-C4)alkoxy(C1-C4)alkylsilyl(C1-C4)alkyl) polysulfides (especially disulfides, trisulfides, or tetrasulfides), such as bis(3-trimethoxysilylpropyl) or bis(3-triethoxysilylpropyl) polysulfides, will be mentioned more specifically. Among these compounds, the bis(3-triethoxysilylpropyl) tetrasulfide of the formula [(C2H5O)3Si(CH2)3S2]2, abbreviated as TESPT, or the bis(triethoxysilylpropyl) disulfide of the formula [(C2H5O)3Si(CH2)3S]2, abbreviated as TESPD, is used in particular. As a preferred example, reference will also be made to bis(mono(C1-C4)alkoxybis(C1-C4)alkylsilylpropyl) polysulfides (especially disulfides, trisulfides or tetrasulfides), and more particularly bis(monoethoxydimethylsilylpropyl) tetrasulfides, as described in patent application US 2004 / 132880.
[0047] Examples of coupling agents other than alkoxysilane polysulfides will be specifically mentioned as bifunctional POS (polyorganosiloxane) or hydroxysilane polysulfides, as described in patent applications WO 02 / 30939 and WO 02 / 31041, or silanes or POS with an azodicarbonyl functional group, as described, for example, in patent applications WO 2006 / 125532, WO 2006 / 125533 and WO2006 / 125534.
[0048] In the rubber composition according to the invention, the content of the coupling agent is preferably in the range of 5% to 18% by weight relative to the amount of silica, and more preferably in the range of 8% to 12% by weight relative to the amount of silica.
[0049] Those skilled in the art will understand that reinforcing fillers of another property (particularly organic properties) can be used as fillers equivalent to the reinforcing inorganic fillers described in this section, provided that the reinforcing filler is covered with an inorganic layer such as silica, or its surface contains functional sites (particularly hydroxyl sites) such that a bond can be established between the filler and the elastomer in the presence or absence of a covering agent or coupling agent.
[0050] In a preferred arrangement (where the rubber composition according to the invention comprises an isoprene elastomer), the rubber composition preferably comprises at least 25 phr of carbon black.
[0051] Crosslinking system The rubber composition according to the invention preferably comprises a sulfur-based crosslinking system, which includes a metal oxide, a stearic acid derivative, and a vulcanization accelerator. This is thus referred to as a vulcanization system. Sulfur can be provided in any form (particularly molecular sulfur or as a sulfur donor).
[0052] Sulfur is preferably used in a concentration of 1 to 20 phr, more preferably 1 to 10 phr.
[0053] As accelerators, any compound capable of acting as an accelerator for sulfurized diene elastomers in the presence of sulfur can be used, particularly thiazole-type accelerators and their derivatives, or accelerators of the sulfenamide, thiuram, dithiocarbamate, dithiophosphate, thiourea, and xanthate types. Examples of such accelerators include, in particular, 2-mercaptobenzothiazole disulfide (abbreviated MBTS), N-cyclohexyl-2-benzothiazole sulfenamide (CBS), N,N-dicyclohexyl-2-benzothiazole sulfenamide (DCBS), N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS), N-(tert-butyl)-2-benzothiazole sulfenimide (TBSI), tetrabenzylthiuram disulfide (TBZTD), zinc dibenzyl dithiuram (ZBEC), and mixtures of these compounds.
[0054] The crosslinking system may also optionally contain a vulcanization delay agent.
[0055] Hydrocarbon wax The rubber composition according to the invention comprises a hydrocarbon wax based on a fraction produced by the pyrolysis of a raw material mainly comprising polyethylene, said fraction comprising up to 5% by weight of a compound containing up to 24 carbon atoms and up to 5% by weight of a compound containing at least 38 carbon atoms.
[0056] Hydrocarbon waxes are waxes composed only of carbon and hydrogen atoms.
[0057] These properties enable the rubber compositions according to the present invention to achieve the desired performance levels.
[0058] The hydrocarbon wax is based on a fraction produced by the pyrolysis of a raw material primarily containing polyethylene. The method used to obtain the wax imparts different properties to rubber compositions compared to waxes with similar structures.
[0059] Preferably, the pyrolysis-substantiated raw material, which mainly comprises polyethylene, contains at least 60% by weight of polyethylene, more preferably at least 70% by weight of polyethylene, more preferably at least 80% by weight of polyethylene, more preferably at least 90% by weight of polyethylene, and very preferably consists of polyethylene.
[0060] Preferably, the hydrocarbon wax has olefin functional groups at the chain ends.
[0061] The hydrocarbon wax used in this invention can be obtained by a method comprising at least the following steps: a) A pyrolysis step mainly involving polyethylene raw materials, such that at least one pyrolysis effluent can be obtained; b) The step of separating the pyrolysis effluent into an intermediate effluent, an effluent of at least one light compound and an effluent of at least one heavy compound, wherein the intermediate effluent comprises at most 5% by weight of a compound containing at most 24 carbon atoms and at most 5% by weight of a compound containing at least 38 carbon atoms.
[0062] For example, this method may correspond to the method described in document CA 3 032 242.
[0063] The steps of pyrolysis a) Feeding raw materials, which mainly consist of polyethylene, into a pyrolysis step preferably operated at a temperature between 300°C and 600°C allows pyrolysis oil to be obtained.
[0064] The term "pyrolysis" refers to the thermal decomposition of a compound in an inert or low-oxygen atmosphere, i.e., an atmosphere containing less than 5% by volume, preferably less than 3% by volume, and more preferably less than 2% by volume of oxygen, preferably in an inert atmosphere.
[0065] The pyrolysis step is preferably carried out under an inert atmosphere, such as a nitrogen atmosphere, at a pressure of less than 1 bar.
[0066] The pyrolysis step can be carried out in a pyrolysis reactor, and can be continuous, semi-continuous, or intermittent. Such reactors are well known to those skilled in the art.
[0067] Preferably, the pyrolysis step of the method for obtaining hydrocarbon wax includes microwave-assisted pyrolysis. In this case, the heat energy required for pyrolysis is provided by microwave radiation.
[0068] Preferably, in this configuration, the power delivered by the microwave device for microwave-assisted pyrolysis is between 0.1 and 10 kW / kg of raw material, more preferably between 0.1 and 5 kW / kg of raw material, more preferably between 0.5 and 4 kW / kg of raw material, and even more preferably between 1 and 4 kW / kg of raw material.
[0069] When the pyrolysis step is carried out continuously or semi-continuously, it can be carried out in multiple regions.
[0070] Step b) of separating pyrolysis oil The pyrolysis oil is then processed in a separation step to obtain a wax containing up to 5% by weight of a compound containing up to 24 carbon atoms and up to 5% by weight of a compound containing at least 38 carbon atoms.
[0071] Any separation method known to those skilled in the art can be used. Since pyrolysis oil is a hydrocarbon effluent, such separation is well known to those skilled in the art and presents no difficulty.
[0072] For example, the pyrolysis oil is processed in a first separation step known as “topping” to separate the lightest fraction containing compounds having up to 16 carbon atoms. Such a separation step can be carried out by any means known to those skilled in the art, such as by evaporation in a distillation column, in an evaporator such as a scraped film evaporator, or by any other means.
[0073] In the second separation step, the effluent containing heavier compounds is processed to separate fractions containing compounds having 16 to 28 carbon atoms.
[0074] Finally, the residual fraction is processed in a final separation step called “bottoming out” to separate the fraction containing compounds with more than 36 carbon atoms.
[0075] Other additives The rubber composition according to the invention may preferably contain additives commonly used in elastomer compositions specifically intended for the manufacture of vehicle tires, such as pigments, protective agents such as anti-ozone waxes, chemical anti-ozone agents or antioxidants, plasticizers other than those mentioned above, anti-fatigue agents, reinforcing resins or methylene acceptors (e.g., phenolic varnish resins) or methylene donors (e.g., HMT or H3M).
[0076] In a preferred arrangement, the rubber composition according to the invention may contain 20 to 100 phr of plasticized hydrocarbon resin.
[0077] In particular, unlike liquid plasticizers (such as oils), the term "resin" is reserved by definition in this patent application to mean a compound that is solid at ambient temperature (20°C).
[0078] Hydrocarbon resins are polymers known to those skilled in the art, which are essentially based on carbon and hydrogen but can contain other types of atoms, and can be used, in particular, as plasticizers or tackifiers in polymer matrices. They are miscible (i.e., compatible) with the polymer composition to which they are intended at the levels used, thus acting as true diluents. They have been described, for example, in the work entitled “Hydrocarbon Resins” by R. Mildenberg, M. Zander, and G. Collin (New York, VCH, 1997, ISBN 3-527-28617-9), Chapter 5 of which relates to their applications, particularly in the field of rubber tires (5.5. “Rubber Tires and Mechanical Goods”). They can be aliphatic, alicyclic, aromatic, hydrogenated aromatic, or aliphatic / aromatic types (i.e., based on aliphatic and / or aromatic monomers). They can be natural or synthetic, petroleum-based or non-petroleum-based (in the case of petroleum-based resins, they are also referred to as petroleum resins). Their Tg is preferably greater than 30°C, especially between 30°C and 95°C.
[0079] Examples of such hydrocarbon resins include those selected from: cyclopentadiene (CPD) homopolymer or copolymer resins, dicyclopentadiene (DCPD) homopolymer or copolymer resins, terpene homopolymer or copolymer resins, C5 fraction homopolymer or copolymer resins, C9 fraction homopolymer or copolymer resins, α-methylstyrene homopolymer or copolymer resins, and mixtures of these resins. More particularly, among the aforementioned copolymer resins, those selected from: (D)CPD / vinyl aromatic copolymer resins, (D)CPD / terpene copolymer resins, terpene / phenol copolymer resins, (D)CPD / C5 fraction copolymer resins, (D)CPD / C9 fraction copolymer resins, terpene / vinyl aromatic copolymer resins, terpene / phenol copolymer resins, C5 fraction / vinyl aromatic copolymer resins, and blends of these resins.
[0080] The term "terpene" in this text refers to α-pinene, β-pinene, and limonene monomers in a known manner; preferably, limonene monomers are used, and the compound is known to exist in three possible isomers: L-limonene (levorotatory enantiomer), D-limonene (dextrorotatory enantiomer), or dipentene (a racemic mixture of dextrorotatory and levorotatory enantiomers). Suitable vinyl aromatic monomers include, for example, styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, vinyltoluene, p-(tert-butyl)styrene, methoxystyrene, chlorostyrene, hydroxystyrene, vinyltrimethylbenzene, divinylbenzene, vinylnaphthalene, or derived from C9 fractions (or more generally from C8 to C9 fractions).10 Any vinyl aromatic monomer (fraction).
[0081] More specifically, the resins mentioned are selected from (D)CPD homopolymer resins, (D)CPD / styrene copolymer resins, polylimonene resins, limonene / styrene copolymer resins, limonene / D(CPD) copolymer resins, C5 fraction / styrene copolymer resins, C5 fraction / C9 fraction copolymer resins, and mixtures of these resins.
[0082] C5 resin is commercially available, for example, sold by Eastman under the names Piccotac 1105 or Impera R1507, by Exxon under the name Escorez 1102, by Kolon under the name Hikorez A1100, or by Cray Valley Total under the name Wingtack 98. C5-C9 resin is commercially available, for example, sold by Exxon under the name Oppa 373, by Eastman under the name Piccotac 8090, or by Cray Valley Total under the name Wingtack STS.
[0083] Preparation of rubber composition The rubber composition according to the invention is prepared in a suitable mixer using preparation stages known to those skilled in the art: - The thermomechanical processing or kneading stage, which can be carried out in a single thermomechanical step, involves introducing all necessary components, particularly the elastomer matrix, hydrocarbon resin, filler, and various other optional additives, into a suitable mixer such as a standard closed mixer (e.g., a "Banbury" type). During thermomechanical kneading, fillers can be introduced into the elastomer in one or multiple batches. Where fillers (particularly carbon black or silica) have already been fully or partially introduced into the elastomer in masterbatch form (as described, for example, in patent applications WO 97 / 36724 or WO 99 / 16600), the masterbatch is kneaded directly, and where appropriate, other elastomers or fillers present in the composition (not in masterbatch form) and various other optional additives are introduced.
[0084] Thermomechanical kneading is carried out at high temperatures, up to between 110°C and 200°C, preferably at a maximum temperature between 130°C and 185°C, typically for a period of time between 2 and 10 minutes.
[0085] - The mixture obtained in the first stage is then cooled to a lower temperature, typically below 120°C, such as between 40°C and 100°C, and then subjected to a second stage of machining in an open mixer such as a two-roll mill.
[0086] The cross-linking system will be added during the second stage of the process.
[0087] The resulting final composition is then calendered, for example, into sheets or plates for laboratory characterization, or extruded into rubber semi-finished products (or molded elements).
[0088] The composition can be in an uncured state (before crosslinking or vulcanization) or in a cured state (after crosslinking or vulcanization), or it can be a semi-finished product that can be used in tires.
[0089] Curing can be carried out in a manner known to those skilled in the art at a temperature typically between 130°C and 200°C and under pressure for a sufficient time, the time range being, for example, between 5 and 90 minutes, which varies, in particular, with the curing temperature, the crosslinking system employed, the crosslinking kinetics of the composition under consideration, or the size of the tire.
[0090] vehicle tires The present invention also relates to vehicle tires comprising a rubber composition based on at least one elastomer and a hydrocarbon wax according to the present invention.
[0091] Vehicle tires can be pneumatic or non-pneumatic. Non-pneumatic tires are those that can support the vehicle's load through means other than pressurizing with gas, such as by using struts.
[0092] The vehicle tires according to the invention will be selected, without limitation, from tires intended for mounting two-wheeled vehicles, passenger vehicles, “heavy-duty” vehicles (i.e., subways, buses, all-terrain vehicles, heavy-duty transport vehicles such as trucks, tractors or trailers), aircraft, construction equipment, heavy agricultural vehicles or material handling vehicles.
[0093] Vehicle tires typically consist of a crown, two sidewalls, and two beads, with each sidewall connecting each bead to the crown. Each bead includes at least one circumferential reinforcing element, typically in the form of a bead line.
[0094] The vehicle tire also includes a carcass reinforcement anchored in each bead and extending in each sidewall and crown. The carcass reinforcement includes carcass layers comprising portions wound around each circumferential reinforcing element.
[0095] The tread includes a tread portion intended to contact the ground when the vehicle tire is in operation, and a tread reinforcement arranged radially between the tread and the carcass reinforcement. The tread reinforcement includes a working reinforcement comprising at least one working layer. The tread reinforcement also includes a hoop reinforcement arranged radially outside the working reinforcement, the hoop reinforcement being axially defined by two axial edges and including at least one hoop filamentary reinforcement element, which is circumferentially helically wound such that it extends axially from one axial edge of the hoop reinforcement to the other axial edge in the main direction of the hoop filamentary reinforcement element or each hoop filamentary reinforcement element.
[0096] Therefore, the present invention also relates to a vehicle tire having a sidewall as described above, the sidewall comprising at least one rubber composition according to the present invention.
[0097] The present invention also relates to vehicle tires whose treads comprise a rubber composition according to the present invention. Detailed Implementation
[0098] Measurement methods Mooney Plasticity Mooney plasticity is measured according to the following principles and in accordance with ASTM D-1646. The green composition is molded in a cylindrical chamber heated to a given temperature (typically 100°C). After 1 minute of preheating, an L-shaped rotor rotates within the test specimen at 2 revolutions per minute. After 4 minutes of rotation, the working torque used to maintain this motion is measured. Mooney plasticity (ML 1+4) is expressed in Mooney units (MU, 1 MU = 0.83 N·m).
[0099] Tensile test Tests were conducted according to French standard NF T 46-002 of September 1988. All tensile measurements were performed according to French standard NF T 40-101 (December 1979) under standard conditions of temperature (23±2℃) and humidity (50%±5% relative humidity).
[0100] In the second elongation (i.e., after adjustment), elongations of 100% and 300% (denoted as MA, respectively) are recorded. 100 and MA 300 The nominal secant modulus (or apparent stress, in MPa) of a sample cured at 150°C for 25 minutes is measured (which is calculated by reducing to the initial cross-section of the test sample).
[0101] Results are expressed as a base of 100, with a value of 100 assigned to the control. A result greater than 100 indicates that the stiffness of the composition of the considered embodiment is greater than that of the control.
[0102] The fracture stress (in MPa) and fracture strain (in %) at 23℃ ± 2℃ were also measured on green samples or samples cured at 150℃ for 25 minutes or 160℃ for 90 minutes, according to standard NF T 46-002. The fracture energy is equal to the product of the fracture elongation and the fracture stress.
[0103] Dynamic properties The dynamic properties G* and tan(δ) were measured on a viscosity analyzer (Metravib VA4000) according to standard ASTM D 5992-96. The response of cross-linked composition samples (cylindrical test samples with a thickness of 4 mm and a cross-sectional area of 400 mm²) subjected to simple alternating sinusoidal shear stress at a frequency of 10 Hz was recorded according to standard ASTM D 1349-99. Strain amplitude scans were performed from 0.1% to 100% (outward cycle) and then from 100% to 1% (backward cycle). The results used are the complex dynamic shear modulus G* and shear loss modulus G'', as well as the tan(δ) value. For the backward cycle, the G* and G'' values at 10% strain are shown, along with the maximum observed tan(δ). The G'' value measured at 23°C is an indicator of rolling resistance. A low value indicates a smaller contribution of the composition to rolling resistance.
[0104] Flood test: The blooming test measures the tendency of anti-ozone wax to migrate excessively after long-term storage. The test procedure consists of the following steps.
[0105] After cutting, the 2.5 mm thick test sample sheets were baked in air at 70°C for 12 hours. Subsequently, they were baked in air at 40°C for 4, 6, and 8 weeks. After being removed from the oven and returned to ambient temperature for 15 minutes, mechanical stimulation (consisting of the action of scraping the test sample with a metal blade) was applied to expose the wax bloom.
[0106] The degree of blooming (whitening of the surface) was then assessed using a subjective scale representing the final appearance of the samples. The scale ranged from 0 to 3, corresponding to the following appearances of the samples: 0 - no blooming / 1 - slight blooming / 2 - moderate blooming / 3 - complete blooming. Lower values indicated better blooming performance.
[0107] Fatigue measurement According to standards ASTM D4482-85 and ISO 6943, fatigue strength, expressed in cycles or relative units (ur), is measured in a known manner on 12 test specimens subjected to repeated low-frequency tensile deformation up to 75% elongation at 23°C, using a Monsanto (MFTR) machine until the test specimen breaks.
[0108] Results are expressed in relative units (ur). Values larger than the control value arbitrarily set to 100 indicate improved results, meaning the rubber sample has better fatigue strength.
[0109] Ozone resistance The ozone resistance of the material was measured as follows: After curing, it was baked in air at 77°C for 14 days. Ten test samples were placed on a trapezoidal frame, and measurements were taken at different elongations ranging from 10% to 100% along the main axis (length of the test sample). The “B15” test sample was produced from MFTR (called Monsanto) sheet material, with two beads at the ends used to hold the test sample. The “B15” test sample had the following dimensions: 78.5 mm × 15 mm × 1.5 mm. After exposure to 38°C and an ozone level of 50 pphm (parts per billion), the appearance of each sample was visually analyzed by photographs using a binocular magnifying glass after 3 and 8 days. Each appearance was scored according to its color, with a maximum score of 20 points: completely black = 20 points (test sample intact), cracked test sample = 0 points. Between these two extreme scores, the number and depth of cracks determined the grayscale level of the test sample (measured with computer processing assistance). This rating (out of 20 points) considers all test samples under various strains. The higher the score, the better the ozone performance.
[0110] Curing time The times t0 and t90 were determined according to DIN 53529 standard, from the curing rheology diagram at 150°C or 160°C. The α value was determined based on the following calculation: α(t) = (C(t) - C min ) / (C max -C min ), where C is the torque obtained from the rheological diagram, t is time, t0 is the time at which α(t0) = 0, and t90 is the time at which α = 0.90.
[0111] Example Example 1 – Synthesis of Hydrocarbon Wax The pyrolysis step, as described in document CA 3 032 242, is fed with a feedstock comprising 100% by weight of polyethylene (high-density polyethylene, referred to as HDPE) in particulate form, with a maximum size between 3 and 5 mm. The microwave pyrolysis step is carried out at a power of approximately 600 W under a nitrogen inert atmosphere. Pyrolysis is stopped when the gas temperature at the pyrolysis outlet drops below 50°C.
[0112] The pyrolysis effluent undergoes a first fractionation step in a wiped-film evaporator, primarily separating compounds containing fewer than 16 carbon atoms. The residue containing heavier compounds is separated in a second wiped-film evaporator, primarily separating compounds containing fewer than 28 carbon atoms. The residue from this second separation step is processed in a third separation step in a wiped-film evaporator, primarily separating compounds containing more than 36 carbon atoms. The extract constituting the hydrocarbon wax collected at the end of this final separation comprises up to 5% by weight of compounds containing up to 24 carbon atoms and up to 5% by weight of compounds containing at least 38 carbon atoms.
[0113] The properties of the obtained hydrocarbon wax are shown in Table 1.
[0114] Example 2 – Rubber Composition All components except the vulcanization system were introduced into a closed mixer to produce the rubber compositions detailed in Tables 2 and 3. The vulcanizing agent (sulfur and accelerator) was introduced into an open mixer at a low temperature (30°C for the mixer's component rollers). For compositions A-0, A-1, and A-2, the compositions were pressure-cured at 160°C; for compositions A-3 and A-4, the compositions were pressure-cured at 150°C.
[0115] Various waxes were used to prepare these compositions, and their properties are shown in the table below.
[0116] [Table 1] (1) C32 anti-ozone wax, Redezon 500, obtained from Repsol. (2) C36 anti-ozone wax, Redezon 7236, obtained from Repsol. Tables 2 and 3 show the various rubber compositions using the waxes shown in Table 1 and the measurement results obtained.
[0117] Results are expressed as a base of 100, with a value of 100 assigned to the control (A-0 in Table 2, A-3 in Table 3). A result greater than 100 indicates that the value is greater than that of the control.
[0118] [Table 2] Table 2 Reference Number (3) Natural rubber (4) Synteca 44 Nd:4 polybutadiene, obtained from Syntheos (5) Carbon black, ASTM N660, obtained from Cabot Corporation (6) Vivatec 500 TDAE oil, obtained from British Petroleum (BP). (7) Vulkanox 4020 antioxidant, obtained from Lanxess Company (8) Naugard Q antioxidant, obtained from Chemtura (9) DelacS (tert-butyl)benzothiazole sulfenamide (TBBS), obtained from Chemtura.
[0119] It has been observed that the compositions according to the present invention exhibit properties comparable to those of compositions containing commercially available waxes in terms of curing behavior and curing performance, while also exhibiting better fatigue strength.
[0120] [Table 3] Table 3 Reference Number (10) SBR copolymer of styrene and butadiene, Tg -65℃ (11) Carbon black, ASTM N234, obtained from Cabot Corporation (12) Zeosil 1165MP silica, obtained from Solvay. (13) Oppera PR 383 resin, obtained from ExxonMobil (14) Oleic sunflower oil, obtained from Cargill Company (15) SI69 silane, obtained from Evonik. (16) Diphenylguanidine, DPG, obtained from Akrochem (17) Santoflex 6PPD antioxidant, obtained from Flexsys It was observed that the compositions according to the invention exhibited properties comparable to those of compositions containing commercially available waxes in terms of their curing behavior and curing performance, and also exhibited good fracture properties.
Claims
1. A rubber composition based on at least one elastomer matrix, reinforcing filler, crosslinking system and hydrocarbon wax, said hydrocarbon wax being based on a fraction produced by the pyrolysis of a raw material mainly comprising polyethylene, said fraction comprising up to 5% by weight of a compound containing up to 24 carbon atoms and up to 5% by weight of a compound containing at least 38 carbon atoms.
2. The composition according to the preceding claim, wherein, The pyrolysis feedstock comprises at least 60% by weight polyethylene, preferably at least 70% by weight polyethylene, preferably at least 80% by weight polyethylene, preferably at least 90% by weight polyethylene, and most preferably composed of polyethylene.
3. The composition according to any one of the preceding claims, wherein, The hydrocarbon wax has olefin functional groups at the chain ends.
4. The composition according to any one of the preceding claims, wherein, The hydrocarbon wax is obtained by a method comprising at least the following steps: a) A pyrolysis step mainly involving polyethylene raw materials, which enables the production of at least one pyrolysis effluent; b) The step of separating the pyrolysis effluent into an intermediate effluent, an effluent of at least one light compound and an effluent of at least one heavy compound, wherein the intermediate effluent comprises at most 5% by weight of a compound containing at most 24 carbon atoms and at most 5% by weight of a compound containing at least 38 carbon atoms.
5. The composition according to any one of the preceding claims, wherein, The pyrolysis step of the method for obtaining the hydrocarbon wax includes microwave-assisted pyrolysis.
6. The composition according to any one of the preceding claims, wherein, The reinforcing filler comprises 10 phr to 150 phr, preferably 50 phr to 130 phr of silica.
7. The composition according to any one of the preceding claims, comprising 20 phr to 100 phr of a plasticized hydrocarbon resin.
8. The composition according to any one of the preceding claims, comprising at least 50 phr of butadiene elastomer.
9. The composition according to the preceding claim, wherein, The butadiene elastomer is a butadiene copolymer with a glass transition temperature (Tg) less than -20°C, preferably between -20°C and -110°C.
10. The composition according to the preceding claim, comprising at least 70 phr, preferably at least 90 phr, of at least one butadiene copolymer, preferably a butadiene-styrene copolymer.
11. The composition according to any one of the preceding claims further comprises at least 20 phr of isoprene elastomer, said isoprene elastomer being selected from natural rubber, synthetic polyisoprene, and mixtures thereof.
12. The composition according to the preceding claim, comprising at least 25 phr of carbon black.
13. A vehicle tire comprising a rubber composition according to any one of the preceding claims.
14. A vehicle tire having a tread comprising a rubber composition according to any one of claims 1 to 10.
15. A vehicle tire having an outer tire sidewall, said outer tire sidewall comprising at least one composition according to claim 11 or 12.
Citation Information
Patent Citations
Catalytic microwave depolymerisation of plastic for production of monomer and waxes
CA3032242A1
Method for manufacturing carbon black
EP0928817A1
Method of producing carbon black, carbon black, rubber composition, tire
JP2017008214A
Tire and tread comprising a bis-alkoxysilane testrasulfide as coupling agent
US20040132880A1
Tire tread reinforced with a silica of very low specific surface area
US20050016650A1