Method of manufacturing a metalized glass substrate

By performing multiple low-energy ion beam surface treatments and multilayer metal deposition on the glass substrate, the problem of poor adhesion between the glass substrate and the metal electrode layer was solved, achieving high adhesion and stability, which is suitable for the manufacture of 3D semiconductor substrates.

CN123076574APending Publication Date: 2026-11-10先技高科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202580028256.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-04-19
Filing Date
2025-04-18
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

The poor bonding between traditional glass substrates and metal electrode layers results in poor metallization and interconnectivity, making them unsuitable for highly integrated semiconductor substrates. Furthermore, traditional chemical processes are complex, polluting, and difficult to operate.

Method used

By performing multiple low-energy ion beam surface treatments on the glass material, dangling bonds and functional groups are formed. Combined with physical vapor deposition, a multi-layer metal layer is formed, ensuring the adhesion between the glass and the metal electrode layer and avoiding the use of catalytic/chemical plating processes.

Benefits of technology

It improves the adhesion and bonding stability between the glass substrate and the metal electrode layer, reduces the process defect rate, and provides an economical and environmentally friendly manufacturing method suitable for 3D semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076574A_ABST
    Figure CN123076574A_ABST
Patent Text Reader

Abstract

The present invention relates to a method of manufacturing a metalized glass substrate, and more particularly, to a method of manufacturing a metalized glass substrate that ensures adhesion and stability between a glass, which is an amorphous material, and a metal electrode layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing a metallized glass substrate, and more specifically, to a method for manufacturing a glass substrate for a glass-based printed circuit board (Glass PCB) that ensures adhesion and stability between the amorphous material and the metal electrode layer. Background Technology

[0002] In recent years, with the trends of miniaturization, multifunctionality and high performance, electronic devices are expected to become thinner and smaller. As the substrate mounting density (high integration) increases, the heat generation problem caused by the amount of current supplied is becoming increasingly prominent.

[0003] Traditional resin substrates are prone to deformation and warping due to the aforementioned heat generation. Furthermore, traditional resin substrates have poor flatness, making them unsuitable for use as substrates in displays such as Mini LEDs and Micro LEDs.

[0004] Currently, to realize three-dimensional (3D) semiconductors, extensive research is being conducted on silicon substrates using through-silicon-via (TSV) technology. However, since silicon itself is a semiconductor, an insulating film is indispensable, and at high frequencies, insertion loss occurs due to its low resistivity, leading to performance degradation.

[0005] Therefore, many companies and research institutions are conducting research to try to replace silicon with glass. As an insulator, glass has almost no electrical loss at high frequencies. In addition, it has small mechanical deformation, excellent surface flatness, and can realize large-area and thin substrates at low cost.

[0006] As mentioned above, glass has many advantages as a semiconductor substrate material, but one of its most fatal drawbacks is its poor metallization and interconnection, which makes it impossible to bond the glass material to the metal electrode layer.

[0007] Therefore, the ability to quickly master the bonding technologies between glass substrate materials and metal electrode layers, and to apply them as differentiated mass production technologies, is expected to become a crucial factor in the semiconductor substrate industry. Summary of the Invention

[0008] Technical issues The present invention aims to solve the above-mentioned problems and its purpose is to provide a method for processing glass material and forming a metal layer to ensure the adhesion between the glass substrate material and the metal electrode layer, thereby improving the reliability of the semiconductor substrate.

[0009] The purpose of this invention is to provide a method that does not use chemical processes such as catalytic / chemical plating. In traditional complex pretreatment and process steps, such chemical processes can cause electrical short circuits due to foreign matter flowing into the substrate surface and the inner wall of the holes. Furthermore, due to the use of strong alkaline, strong acid and toxic substances, wastewater treatment is difficult and the operation is poor.

[0010] The purpose of this invention is to provide a technique for forming thin films through surface treatment and sputtering processes to ensure adhesion. Compared with existing technologies, this technique is relatively simple, provides an economical method, and significantly reduces process defects, thereby avoiding a decrease in yield.

[0011] The objectives of the present invention are not limited to those described above, and the above and other objectives and advantages will become clear from the following description of preferred embodiments.

[0012] Technical solution The objective can be achieved by a method for manufacturing a metallized glass substrate for semiconductors or displays, characterized by comprising: a step of preparing a glass material; a step of performing a first surface treatment on the surface of the glass material; a step of performing a second surface treatment on the glass material after the first surface treatment; a step of performing surface treatments sequentially on the glass material after the second surface treatment up to the nth time; a step of forming a first metal layer on the surface of the glass material after the nth surface treatment; a step of forming a second metal layer on the first metal layer; a step of forming a metal electrode layer on the second metal layer; and a step of performing a heat treatment after forming the electrode layer, wherein the nth time is the 3rd to the 8th time.

[0013] The glass material is characterized in that it may include oxide glasses selected from silicate glass, borosilicate glass, phosphate glass, germanate glass, aluminate glass, vanadate glass, tungstate glass, molybdate glass, etc., and is not limited to the limitations caused by differences in the composition of metal oxides such as Al, Ca, Mg, Na, K, Pb, B, Ba, Ce, Fe, Zn.

[0014] The first surface treatment is characterized by using an active gas or an inert gas as the reactive gas in a vacuum chamber and performing ionization using a linear ion beam. The first surface treatment is also characterized by the inclusion of O2, N2, H2, or Ar gas as the reactive gas, or a mixture of two or more.

[0015] The surface treatment can be performed to bring the vacuum chamber to a vacuum level of 5×10⁻⁶.-5 ~5×10 -6 After the torr is in a vacuum state, a reactive gas is injected to achieve a vacuum degree of 1×10. -2 ~1×10 -4 torr is used for this.

[0016] The second to nth surface treatments are characterized by using an active gas or an inert gas as the reactive gas and performing ionization using a linear ion beam. The second to nth surface treatments are further characterized by using one or more gases selected from the group consisting of O2, N2, H2, and Ar as the reactive gas.

[0017] The characteristic of the ion dose density (ion quantity) in the linear ion beam is that, at 1×10⁻⁶, it is within the range of 1×10⁻⁶. 14 Up to 5×10 19 ions / cm 2 Within this range, the input voltage of the ion beam is characterized as being in the range of 0.5 kV to 3.0 kV.

[0018] The step of forming the first metal layer is characterized by using one or more metals or alloys selected from the group consisting of copper (Cu), nickel (Ni), chromium (Cr), titanium (Ti), zinc (Zn), aluminum (Al), zirconium (Zr), molybdenum (Mo), niobium (Nb), and ruthenium (Ru).

[0019] The step of forming the first metal layer is characterized by performing a physical vapor deposition (PVD) or thermal evaporation process.

[0020] The step of forming the second metal layer is characterized by using one or more metals selected from the group consisting of copper (Cu), silver (Ag), gold (Au), platinum (Pt), and alloys thereof. The step of forming the second metal layer is also characterized by performing a physical vapor deposition (PVD) or thermal evaporation process.

[0021] The metal electrode layer is characterized in that it is formed by chemical plating / electrolytic plating using gold (Au), silver (Ag), cobalt (Co), aluminum (Al), iron (Fe), nickel (Ni), chromium (Cr), or copper (Cu).

[0022] The effects of the invention The present invention has the following effect: it can ensure the adhesion between the glass substrate and the metal electrode layer, thereby providing a substrate that will be competitive as a 3D semiconductor substrate in the future.

[0023] Currently, the peel strength of thin copper (12-20μm) required by the glass circuit board (GCB) industry is 2-3 N / cm, while the present invention has a peel strength that is far superior to the peel strength value required by the industry.

[0024] This invention improves the surface energy of glass materials by performing first, second, and nth surface treatments using ion beam surface treatment, thereby enhancing adhesion. Specifically, depending on the type, flow rate, and mixing of the gases used in the surface treatment, glass materials with high adhesion can be provided. Furthermore, depending on the type, thickness, and alloy composition of the first metal layer, the adhesion between the glass material (as an insulator) and the metal electrode (as a conductor) can be increased, and the bonding stability can be improved.

[0025] The effects of the present invention are not limited to those described above, but should be understood to include all effects that can be inferred from the inventive concept described in the detailed description or claims of the present invention. Attached Figure Description

[0026] Figure 1 The following is a flowchart illustrating a method for manufacturing a metallized glass substrate according to an embodiment of the present invention.

[0027] Figure 2 This is a schematic diagram illustrating the layered structure of a metallized glass substrate manufactured according to an embodiment of the present invention.

[0028] Figure 3 This is a schematic diagram illustrating the layered structure of a metallized glass substrate manufactured according to another embodiment of the present invention.

[0029] Figure 4 A graph showing the contact angle measurement results of Experimental Example 1 of the present invention.

[0030] Figure 5 A graph showing the peel strength measurement results of Experimental Example 2 of the present invention.

[0031] Figure 6 A graph showing the peel strength test results of Experimental Example 3 of the present invention.

[0032] Figure 7 A graph showing the peel strength test results of Experimental Example 4 of the present invention. Detailed Implementation

[0033] In this specification, the embodiments are merely illustrative examples provided to illustrate the invention in more detail, and are not limited to the embodiments described herein, but may be embodied in other forms.

[0034] The embodiments described herein are provided merely to make the disclosure thorough and complete, and to fully convey the ideas of this disclosure to those skilled in the art.

[0035] Furthermore, unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains, and in the event of conflict, the description contained in this specification shall take precedence.

[0036] To clearly illustrate the invention in the accompanying drawings, parts unrelated to the description have been omitted, and similar reference numerals have been used for similar parts throughout the specification.

[0037] Furthermore, when a part is described as "including" a structural element, unless otherwise stated, this does not mean that other structural elements are excluded, but rather that other structural elements may also be included.

[0038] Hereinafter, embodiments of the present invention will be described in more detail with reference to the accompanying drawings.

[0039] Figure 1 The flowchart shows a method for manufacturing a metallized glass substrate according to an embodiment of the present invention. Figure 2 This is a schematic diagram illustrating the layered structure of a metallized glass substrate.

[0040] Refer to together Figure 1 and Figure 2 This will help in understanding the manufacturing method of the aforementioned metallized glass substrate. The present invention includes: a step of preparing a glass material; a step of performing a first surface treatment on the surface of the glass material (S10); a step of performing a second surface treatment on the glass material after the first surface treatment (S20); a step of sequentially performing surface treatments on the glass material after the second surface treatment up to the nth time (S30); a step of forming a first metal layer on the surface of the glass material after the nth surface treatment (S40); a step of forming a second metal layer on the first metal layer (S50); a step of forming a metal electrode layer on the second metal layer (S60); and a step of heat-treating the glass material on which the metal electrode layer is formed (S70).

[0041] First, prepare 100g of glass material.

[0042] The glass material 100 of the present invention may include, for example, oxide glasses such as silicate glass, borosilicate glass, phosphate glass, germanate glass, aluminate glass, vanadate glass, tungstenate glass, and molybdate glass, and is not limited to metal oxides (SiO2, Al2O3, CaO, MgO, Na2O, K2O, PbO, B2O3, BaO, V2O5, P2O5, Bi2O3, ZnO, CaF2, CdO, Ag2O, Li2O) added to impart functions such as improved chemical durability, inhibition of glass crystallization, high insulation, and facilitate X-ray and ultraviolet / infrared transmission, as well as materials resulting from differences in composition. As glass materials in the embodiments described, Corning and Schott glass were used.

[0043] The thickness of the glass material 100 is preferably formed to be, for example, 200 μm to 700 μm.

[0044] Next, the surface of the glass material 100 can be subjected to a first surface treatment 201 (step S10).

[0045] The first surface treatment is performed using an ion beam, which minimizes shape changes on the glass surface, imparts hydrophilic functional groups, and forms dangling bonds.

[0046] The first surface treatment 201 can use an active gas or an inert gas as the reactive gas and is performed using an ion beam, specifically a linear ion beam ionization. Surface treatment using an ion beam can involve irradiating the surface of the glass material with an ion beam containing a reactive gas accelerated at a specific energy range. For example, the reactive gas in the first surface treatment can contain O2, N2, H2, or Ar gas, or a mixture of two or more.

[0047] The present invention preferably uses a low-energy ion beam as the ion beam, and the input voltage of the ion beam can be applied in the range of 0.5kV to 3.0kV. When the input voltage of the ion beam of the present invention is as described above, the surface can be modified without deforming the material, thereby obtaining effects such as cleaning effect, hydrophilicity, adhesion, and nanostructure formation.

[0048] The injection of the reactive gas can be, for example, from 1 sccm to 100 sccm (Standard Cubic Centimeter per Minute), preferably from 30 sccm to 100 sccm, and more preferably from 40 sccm to 70 sccm, within which the ion beam can be stably irradiated onto the glass material surface.

[0049] There is no particular limitation on the irradiation time of the ion beam, which can be adjusted appropriately according to the purpose.

[0050] The ion dose density irradiated onto the glass surface by the low-energy ion beam can be adjusted to 1×10⁻⁶. 14 ions / cm 2 Up to 5×10 19 ions / cm 2 Preferably 1×10 16 ions / cm 2 Up to 5×10 19 ions / cm 2 More preferably 1×10 16 ions / cm 2 Up to 5×10 18 ions / cm 2 Within the range.

[0051] When irradiated with an ion beam under the above conditions, the high adhesion to metal and excellent surface properties can be maximized, which can subsequently improve the bonding stability between the glass material and the metal electrode layer.

[0052] Next, a second surface treatment can be performed on the glass material after the first surface treatment 201 (step S20).

[0053] The second surface treatment can be performed using an ionized reactive gas or an inert gas as the reactive gas, and an ion beam, specifically a linear ion beam. Similar to the first surface treatment, it can contain O2, N2, H2, or Ar gas, or a mixture of two or more.

[0054] Next, the glass material after the second surface treatment can be subjected to surface treatments sequentially up to the nth time (step S30). In other words, this means that the surface of the glass material after the second surface treatment is continuously surface treated. In this case, the nth surface treatment 200 may include at least the third time, specifically, it includes surface treatments up to the third to the eighth time, but is not limited thereto.

[0055] In this invention, by performing a first surface treatment and a second to nth surface treatment on the glass material as described above, functional groups such as carboxyl and hydroxyl groups are promoted to form on the glass surface, inducing chemical interactions between them and the glass oxide chains, thereby significantly improving adhesion to dissimilar materials or substances. Furthermore, the effectiveness varies greatly depending on the amount, type, and mixture of reactive gases injected, as well as the voltage of the ion beam.

[0056] Therefore, when various types of conductive metal layers are subsequently formed on the surface formed by the above surface treatment, excellent reliability (thermal shock, high temperature, moisture, etc.) between dissimilar materials such as glass and metal electrode layers can be ensured.

[0057] Next, a first metal layer 300 can be formed on the surface of the glass material after the nth surface treatment 200 (step S40).

[0058] The first metal layer 300 may be one or more metals selected from the group consisting of copper (Cu), nickel (Ni), chromium (Cr), titanium (Ti), zinc (Zn), aluminum (Al), zirconium (Zr), molybdenum (Mo), niobium (Nb), and ruthenium (Ru).

[0059] The step of forming the first metal layer can be performed using physical vapor deposition (PVD) or thermal evaporation processes.

[0060] The deposition thickness of the first metal layer 300 can be, for example, 10 nm to 100 nm, preferably 10 nm to 80 nm, more preferably 10 nm to 60 nm, but is not limited thereto. The first metal layer of the present invention is used to improve the bonding force between the glass material and the second metal layer. When the deposition thickness of the surface of the surface-treated glass material is as described above, the function of the adhesive layer can be fully utilized without making the substrate too thick, which is beneficial to subsequent processes.

[0061] Next, a second metal layer 400 can be formed on the first metal layer 300 (step S50).

[0062] The step of forming the second metal layer 400 may use one or more metals selected from the group consisting of copper (Cu), silver (Ag), gold (Au), platinum (Pt) and their alloys.

[0063] The type of metal constituting the second metal layer 400 may be the same as or different from the type of metal constituting the first metal layer 300.

[0064] As a method for forming the second metal layer 400, physical vapor deposition (PVD) or thermal evaporation processes can be performed.

[0065] Preferably, the deposition thickness of the second metal layer 400 is, for example, formed to be 100 nm to 700 nm, more preferably 200 nm to 600 nm. When the thickness of the second metal layer is as described above, the role of the main metal layer for wiring and patterning can be fully utilized.

[0066] Next, the step of forming a metal electrode layer 500 on the second metal layer 400 is included (S60).

[0067] The metal electrode layer 500 can be formed, for example, by electrolytic plating or chemical plating, and can be done by methods commonly used in the field of plating technology.

[0068] The metal electrode layer 500 can be gold (Au), silver (Ag), cobalt (Co), aluminum (Al), iron (Fe), nickel (Ni), chromium (Cr), or copper (Cu). Preferably, copper can be used, but it is not limited to this.

[0069] The thickness of the metal electrode layer 500 can be formed to be from 2 μm to 20 μm.

[0070] Next, the metal electrode layer 500 can be heat-treated (step S70). The heat treatment can be performed after the metal electrode layer is plated to remove stress, reduce diffusion between materials / metals or metals / metals, and improve peel strength.

[0071] The heat treatment can be carried out using an electric furnace, but is not limited to this; heaters and other furnaces can also be used.

[0072] The heat treatment can vary depending on the type and composition of the glass material, but for example, it is preferably carried out at a temperature between 100°C and 600°C. When the heat treatment temperature is below 100°C, it is difficult to form an intermetallic compound between the first metal layer and the second metal layer. When the temperature exceeds 600°C, overheating may occur, which may cause warpage or cracking problems due to the difference in thermal expansion coefficients between the glass and the metal.

[0073] The structure of a metallized glass substrate manufactured according to an embodiment of the present invention may include: a glass material 100; a first surface treatment layer 201 formed on the surface of the glass material 100; an nth surface treatment layer 200 formed on the first surface treatment layer 201; a first metal layer 300 formed on the nth surface treatment layer 200; a second metal layer 400 formed on the first metal layer 300; and a metal electrode layer 500 formed on the second metal layer 400.

[0074] In this context, the term "surface treatment layer" is used for the purpose of illustration and explanation of the layer structure, and the meaning of "surface treatment layer" is preferably interpreted as indicating the state of a surface-treated coating.

[0075] Figure 3 This is a schematic diagram illustrating the layered structure of a metallized glass substrate manufactured according to another embodiment of the present invention.

[0076] Reference Figure 2 This is intended to demonstrate that by performing the same process on the lower surface of the glass material 100, the substrate can also be formed into a composite structure.

[0077] Furthermore, in addition to the above-mentioned structure, those skilled in the art can make any design changes to the multilayer, structure, manufacturing process, etc., to develop 3D semiconductor substrates.

[0078] According to an embodiment of the present invention, a method for manufacturing a metallized glass substrate is provided to ensure adhesion between a glass substrate and a metal electrode layer.

[0079] Specifically, according to the present invention, by using a low-energy ion beam for the first, second, and nth surface treatments, the surface of the glass material is cleaned, nanostructures are formed, and chemical modifications are achieved. Dangling bonds can also be formed, thereby improving the reactivity between dissimilar materials. Furthermore, by performing a multilayer metal thin film deposition and coating process, the adhesion between the glass material (as an insulator) and the metal electrode (as a conductor) can be increased, and bonding stability is imparted.

[0080] Embodiments of the present invention The structure and effects of the present invention will be described in more detail through specific embodiments and comparative examples. However, these embodiments are intended to illustrate the present invention more specifically, and the scope of the present invention is not limited to these embodiments.

[0081] [Example 1] For 500 μm thick borosilicate glass (Eagle XG), a linear ion beam was used with Ar gas as the reactive gas on the glass surface at an ion dose density of 5 × 10⁻⁶. 14 ions / cm 2 The first surface treatment was performed at a speed of 0.5 m / min. The input voltage was set to 1.0 kV.

[0082] [Example 2] For the glass material after the first surface treatment in Example 1, Ar gas was used as the reactive gas on the surface of the glass, with an ion dose density of 5 × 10⁻⁶. 14 ions / cm2 The second and third surface treatments were performed at a speed of 0.5 m / min. The input voltage was set to 1.0 kV.

[0083] [Example 3] For the glass material that underwent the third surface treatment in Example 2, Ar gas was used as the reactive gas on the glass surface, with an ion dose density of 5 × 10⁻⁶. 14 ions / cm 2 The fourth and fifth surface treatments were performed at a speed of 0.5 m / min. The input voltage was set to 1.0 kV.

[0084] [Example 4] For the glass material that underwent the fifth surface treatment in Example 3, Ar gas was used as the reactive gas on the glass surface at an ion dose density of 5 × 10⁻⁶. 14 ions / cm 2 The surface treatment was performed for the 6th to 8th times at a speed of 0.5 m / min. The input voltage was set to 1.0 kV.

[0085] <Experimental Example 1: Confirming the surface modification effect based on the number of surface treatments> To confirm the surface modification effect based on the Nth surface treatment, the untreated (control group), the first surface treatment (Example 1), the third (Example 2), the fifth (Example 3), and the eighth (Example 4) surface treatments were set as experimental groups.

[0086] The modification effect was confirmed by measuring the contact angle. The smaller the contact angle, the higher the hydrophilicity of the glass surface and the better the adhesion to the metal layer.

[0087] The surface treatment results showed that the contact angle of the control group was 38.8°, the contact angle after the first surface treatment was 17.2°, the contact angle after the third surface treatment was 9.3°, and the contact angle after the fifth surface treatment was 3–4°, indicating complete hydrophilicity. The results are shown in… Figure 4 .

[0088] <Experimental Example 2: Determination of Peel Strength Based on Ion Dosage Density> A peel strength determination experiment based on ion dose density was conducted.

[0089] For 500 μm thick borosilicate glass (Eagle XG), a linear ion beam was used to treat the surface of the glass with Ar gas as the reactive gas at an input voltage of 1.0 kV and a velocity of 0.5 m / min. The ion dose density was set to 5 × 10⁻⁶. 13 ions / cm2 (Control group), 5×10 14 ions / cm 2 5×10 15 ions / cm 2 5×10 16 ions / cm 2 5×10 17 ions / cm 2 5×10 18 ions / cm 2 Then perform the fifth surface treatment.

[0090] Then, a 30 nm Ti layer was deposited as the first metal layer, and a 500 nm Cu layer was deposited as the second metal layer, followed by electroplating to a thickness of 18 μm. The mixture was then heat-treated in an Ar atmosphere furnace at 250 °C for 1 hour, and the peel strength was confirmed by the 90° peel strength test method according to JIS C6481. The results are shown in... Figure 5 .

[0091] Reference Figure 5 , in 5×10 13 ions / cm 2 The peel strength value was confirmed to be approximately 2–3 N / cm under traditional conditions, when the ion dose density was 5 × 10⁻⁶. 14 ions / cm 2 ~5×10 18 ions / cm 2 When surface treatment was performed within the specified range, a value higher than that of conventional peel strength was confirmed.

[0092] <Experimental Example 3: Determination of Peel Strength Based on Gas Type> Peel strength tests were conducted based on the type of gas. To improve the adhesion between the glass and metal layers during the nth surface treatment, single or mixed gases of O2, N2, H2, and Ar were used as experimental groups. The input voltage was fixed at 1.0 kV, and the ion dose density was fixed at 5 × 10⁻⁶. 18 ions / cm 2 The surface treatment was performed up to the fifth time under all conditions. After the surface treatment, the process was the same as in Example 2, and the peel strength was measured. The results are shown in... Figure 6 It was confirmed that when surface treatment is performed using O2 gas, the bonding strength with the metal is further improved by forming and modifying the non-crosslinked dangling bonds in the oxide layer on the glass surface.

[0093] <Experimental Example 4: Peel Strength Measurement Based on the Type of the First Metal Layer> Peel strength tests were conducted based on the type of the first metal layer. A control group without a first metal layer, and Ni and Ti were used as experimental groups. The input voltage was fixed at 1.0 kV, and the ion dose density was fixed at 5 × 10⁻⁶. 18 ions / cm 2 The surface treatment was performed up to the fifth time using O2 gas under all conditions. A first metal layer of 30 nm thick Ni and Ti was deposited, followed by a second metal layer of 500 nm thick Cu, and then electroplating was performed to a thickness of 18 μm. A heat treatment was then performed in an Ar atmosphere furnace at 250 °C for 1 hour, and the peel strength was confirmed by the 90° peel strength test method according to JIS C 6481. The results are shown in... Figure 7 .

[0094] The above embodiments should be understood in all respects as exemplary and not restrictive. For example, the structural elements described in a single form may also be implemented separately, and similarly, the structural elements described in a separate form may also be implemented in combination.

[0095] The scope of this invention is defined by the claims described below, and all modifications or variations derived from the meaning and scope of the claims and their equivalents shall be construed as being included within the scope of this invention.

[0096] Industrial availability This invention relates to a method for manufacturing a metallized glass substrate, which, by ensuring the adhesion and stability between the amorphous material and the metal electrode layer, can be used to manufacture glass substrates for glass-based printed circuit boards.

Claims

1. A method for manufacturing a metallized glass substrate, characterized in that, include: The steps for preparing glass material; the steps for performing a first surface treatment on the surface of the glass material; The steps include: performing a second surface treatment on the glass material after the first surface treatment; performing surface treatments sequentially on the glass material after the second surface treatment up to the nth time; forming a first metal layer on the surface of the glass material after the nth surface treatment; forming a second metal layer on the first metal layer; forming a metal electrode layer on the second metal layer; and performing a heat treatment on the glass material with the metal electrode layer formed thereon, wherein the nth time is the 3rd to the 8th time.

2. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The glass material is an oxide glass selected from silicate glass, borosilicate glass, phosphate glass, germanate glass, aluminate glass, vanadate glass, tungstate glass, or molybdate glass.

3. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The first surface treatment is performed by using an active or inert gas as the reactive gas and ionizing it with a linear ion beam.

4. The method for manufacturing a metallized glass substrate according to claim 3, characterized in that, The reactive gas used in the first surface treatment includes one or more gases selected from the group consisting of O2, N2, H2 and Ar.

5. The method for manufacturing a metallized glass substrate according to claim 4, characterized in that, The injection volume of reactive gas is in the range of 1 sccm to 100 sccm, or 30 to 100 sccm, or 40 to 70 sccm.

6. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The second to nth surface treatments are performed by using an active or inert gas as the reactive gas and ionizing it with a linear ion beam.

7. The method for manufacturing a metallized glass substrate according to claim 6, characterized in that, The reactive gases used in the second to nth surface treatments include one or more gases selected from the group consisting of O2, N2, H2, and Ar.

8. The method for manufacturing a metallized glass substrate according to claim 3, characterized in that, The ion dose density irradiated onto the glass surface by a linear ion beam is 1×10⁻⁶. 14 ions / cm 2 Up to 5×10 19 ions / cm 2 Within the range.

9. The method for manufacturing a metallized glass substrate according to claim 8, characterized in that, The input voltage of the linear ion beam is in the range of 0.5kV to 3.0kV.

10. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The step of forming the first metal layer uses one or more metals selected from the group consisting of copper, nickel, chromium, titanium, zinc, aluminum, zirconium, molybdenum, niobium and ruthenium.

11. The method for manufacturing a metallized glass substrate according to claim 10, characterized in that, The deposition thickness of the first metal layer is in the range of 10 nm to 100 nm, or 10 nm to 80 nm, or 10 nm to 60 nm.

12. The method for manufacturing a metallized glass substrate according to claim 11, characterized in that, In the step of forming the first metal layer, a physical vapor deposition or thermal evaporation process is performed.

13. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The step of forming the second metal layer 400 uses one or more metals selected from the group consisting of copper, silver, gold, platinum and their alloys.

14. The method for manufacturing a metallized glass substrate according to claim 13, characterized in that, The deposition thickness of the second metal layer is in the range of 100 nm to 700 nm.

15. The method for manufacturing a metallized glass substrate according to claim 14, characterized in that, In the step of forming the second metal layer, a physical vapor deposition or thermal evaporation process is performed.

16. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The metal electrode layer is formed by electrolytic plating or chemical plating using gold, silver, cobalt, aluminum, iron, nickel, chromium or copper metals.

17. The method for manufacturing a metallized glass substrate according to claim 1, characterized in that, The heat treatment is carried out in a furnace at a temperature of 100°C to 600°C.