Secondary battery with reduced gas generation
By using lithium oxide in lithium secondary batteries and controlling the composition and orientation of the negative electrode active material, the problem of high gas generation caused by manganese-rich oxides was solved, resulting in a reduction in gas generation and an improvement in fast charge and discharge efficiency.
Patent Information
- Application Number
- CN202580027723.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2025-01-08
- Filing Date
- 2025-12-22
- Publication Date
- 2026-11-10
AI Technical Summary
Existing manganese-rich oxide cathode active materials cause excessive gas generation in lithium secondary batteries.
Lithium oxide is used as the positive electrode active material, wherein the Mn content is based on the total metal excluding lithium being more than 50 mol%, and the proportion of natural graphite in the negative electrode active material is controlled to exceed 50 wt%. The orientation of the carbon-based active material is controlled by applying a magnetic field to reduce the release of oxygen and manganese ions.
It effectively reduces the amount of gas generated during the cycling and storage of lithium secondary batteries, and improves the mobility of lithium ions and the efficiency of fast charging and discharging.
Smart Images

Figure CN123076933A_ABST
Abstract
Description
Technical Field
[0001] This application claims priority to Korean Patent Application No. 10-2025-0002631, filed on January 8, 2025, the disclosure of which is incorporated herein by reference.
[0002] This invention relates to a secondary battery containing manganese-rich (Mn-rich) oxide as the positive electrode active material, while exhibiting reduced gas production. Background Technology
[0003] Lithium-ion batteries have been used as a variety of energy storage media through reversible electrochemical reactions. Among the various areas actively researching lithium-ion batteries, in-depth studies are being conducted aimed at improving energy density. One of the most promising approaches is the use of positive electrode active materials known as manganese-rich (Mn-rich), lithium-rich (Li-rich), and / or lithium-excess manganese-rich (Li-rich, Mn-rich) oxides.
[0004] This manganese-rich cathode active material exhibits a high theoretical reversible capacity of over 250 mAh / g by participating not only in the redox reactions of transition metals but also in the redox reactions of oxygen anions. Furthermore, these manganese-rich cathode active materials possess characteristics such as being cobalt-free (Co-free) and / or having low nickel content, thus they are being investigated as alternatives to conventional NCM-type cathode active materials in terms of energy density, development sustainability, and cost competitiveness.
[0005] For example, the problem with manganese-rich (Mn-rich) cathode active materials is that the manganese redox reaction (Mn redox reaction) electrochemically induces an interfacial reaction between the electrolyte and the cathode material, resulting in a higher amount of gas generation compared to other cathode materials.
[0006] Therefore, a technology is needed that can reduce gas generation while utilizing this manganese-rich cathode active material. Summary of the Invention
[0007] Technical issues
[0008] Therefore, the present invention aims to provide a secondary battery comprising a manganese-rich (Mn-rich) oxide as the positive electrode active material, while simultaneously achieving a reduction in gas generation.
[0009] Technical solution
[0010] To address the above problems, in one embodiment, the secondary battery according to the present invention comprises: A positive electrode, comprising lithium oxide as a positive electrode active material, wherein the Mn content in the lithium oxide is based on a total metal content excluding lithium of 50 mol% or more, or wherein the molar ratio of lithium to transition metals exceeds 1; and The negative electrode comprises a carbon-based active material, wherein The carbon-based active material comprises at least one selected from natural graphite and artificial graphite, and the proportion of natural graphite exceeds 50% by weight based on the total weight of the carbon-based active material.
[0011] In one embodiment, lithium oxide is represented by chemical formula 1.
[0012] [Chemical Formula 1]
[0013] Li x M (1-y-z) Mn y M 1 z O2
[0014] In chemical formula 1, M is selected from at least one of Ni, Co and Fe; M 1 It is at least one element selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo; x, y, and z satisfy 0.8≤x≤2, 0.5≤y<1, 0≤z≤0.1, and y+z=1, respectively.
[0015] Specifically, in chemical formula 1, x is in the range of 1.2 to 1.5.
[0016] In a specific instance, lithium oxide can be represented by chemical formula 2.
[0017] [Chemical Formula 2]
[0018] Li x M (1-y) Mn y O2
[0019] In chemical formula 2, M is selected from at least one of Ni and Co; x and y satisfy 1.01≤x≤2 and 0.5≤y<0.9 respectively.
[0020] In one embodiment, the proportion of natural graphite in the carbon-based active material ranges from 75% to 100% by weight. In a specific example, the proportion of natural graphite in the carbon-based active material ranges from 70% to 90% by weight.
[0021] In another embodiment, the average orientation index (OI) of the carbon-based active material, as defined by the following mathematical formula 1, is less than 15, specifically in the range of 0.1 to 15.
[0022] [Mathematical Expression 1]
[0023] OI=I 004 / I 110
[0024] In mathematical formula 1, I 110 This represents the intensity of the peak corresponding to the (110) crystal plane of the carbon-based active material, as measured by X-ray diffraction (XRD) spectroscopy; and I 004 This represents the intensity of the peak corresponding to the (004) crystal plane of the carbon-based active material, as measured by X-ray diffraction (XRD) spectroscopy.
[0025] In one embodiment, the negative electrode further comprises a silicon-based active material as an active material, and the content of the silicon-based active material ranges from 0.1% to 30% by weight, based on the total weight of the negative electrode active material. For example, the silicon-based active material comprises materials selected from silicon (Si), silicon carbide (SiC), silicon carbide / carbon composites (Si / C), and silicon oxide (SiO2). q At least one of the following: (where 0.8 ≤ q ≤ 2.5).
[0026] In addition, the secondary battery is a pouch-type secondary battery. As another example, the secondary battery is a cylindrical or prismatic secondary battery.
[0027] Furthermore, the secondary battery according to the present invention is, for example, a battery used in automobiles or energy storage systems (ESS).
[0028] Beneficial effects
[0029] The secondary battery according to the present invention can reduce gas generation while containing manganese-rich (Mn-rich) oxides as positive electrode active materials. Attached Figure Description
[0030] Figure 1 This is a graph showing the results of analyzing the gases generated in the secondary batteries of the examples and comparative examples under conditions of 45°C and 300 cycles.
[0031] Figure 2 This is a voltage-based capacity variation graph showing the secondary batteries of the examples and comparative examples under conditions of 45°C and 300 cycles.
[0032] Figure 3 This is a graph showing the results of analysis of the gases generated in the secondary batteries of the examples and comparative examples during storage at 60°C for 8 weeks.
[0033] Figure 4 This is a voltage-based capacity variation graph showing the secondary batteries of the examples and comparative examples under conditions of 60°C and 300 cycles. Detailed Implementation
[0034] Since various modifications can be made to the present invention, and the present invention can have various implementation schemes, the specific implementation schemes will be described in detail in the specific embodiments.
[0035] However, this is not intended to limit the invention to specific embodiments, and it should be understood that the invention covers all modifications, equivalents and substitutions that fall within the spirit and scope of the invention.
[0036] In this invention, terms such as “comprising” or “having” are intended to specify the presence of features, numbers, steps, operations, constituent elements, parts or combinations thereof described in the specification, and should be understood to not exclude the possibility of the presence or addition of one or more other features, numbers, steps, operations, constituent elements, parts or combinations thereof.
[0037] The invention will now be described in more detail.
[0038] In one embodiment, the secondary battery according to the present invention comprises: A positive electrode, comprising lithium oxide as a positive electrode active material, wherein the Mn content in the lithium oxide is based on a total metal content excluding lithium of 50 mol% or more, or wherein the molar ratio of lithium to transition metals exceeds 1; and The negative electrode contains a carbon-based active material.
[0039] In addition, the carbon-based active material includes at least one selected from natural graphite and artificial graphite, wherein the proportion of natural graphite exceeds 50% by weight based on the total weight of the carbon-based active material.
[0040] As the positive electrode active material, the present invention employs: (i) oxides in which the content of Mn is based on 50 mol% or more of all metals excluding lithium (hereinafter referred to as "manganese-rich oxides"); (ii) oxides in which the molar ratio of lithium to transition metals exceeds 1 (hereinafter referred to as "lithium-excess oxides"); and / or (iii) oxides in which the content of Mn is based on 50 mol% or more of all metals excluding lithium and has a molar ratio of lithium to transition metals exceeding 1 (hereinafter referred to as "lithium-excess manganese-rich oxides"). In the present invention, the above-mentioned oxides (i) to (iii) used for the positive electrode active material are collectively referred to as "manganese-rich oxides". Specifically, the positive electrode active material used in the present invention is a manganese-rich oxide or a lithium-excess manganese-rich oxide. For example, the positive electrode active material is a lithium-excess manganese-rich oxide.
[0041] In one embodiment, the lithium oxide used as the positive electrode active material can be represented by chemical formula 1.
[0042] [Chemical Formula 1]
[0043] Li x M (1-y-z) Mn y M 1 z O2
[0044] In chemical formula 1, M is selected from at least one of Ni, Co and Fe; M 1 It is at least one element selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo; x, y, and z satisfy 0.8≤x≤2, 0.5≤y<1, 0≤z≤0.1, and y+z=1, respectively.
[0045] For example, in chemical formula 1, x ranges from 1.2 to 1.5.
[0046] In a more specific implementation, lithium oxide can be represented by chemical formula 2.
[0047] [Chemical Formula 2]
[0048] Li x M (1-y) Mn y O2
[0049] In chemical formula 2, M is selected from at least one of Ni and Co; x and y satisfy 1.01≤x≤2 and 0.5≤y<0.9 respectively.
[0050] The lithium secondary battery containing the above-mentioned positive electrode active material shows a peak in the dQ / dV graph below 3.5 V during discharge. This peak is understood to be generated by the reduction of manganese ions (Mn ions) during the activation process. This invention, for example, controls the composition ratio of natural graphite to artificial graphite in the negative electrode active material and suppresses the utilization rate of the Li2MnO3 phase.
[0051] Furthermore, this invention reduces oxygen release from the crystal structure of the positive electrode active material and reduces cation mixing of manganese ions (Mn ions). Typically, as cation mixing increases, the resistance of the battery or positive electrode increases. By controlling the ratio of natural graphite to artificial graphite in the negative electrode, this invention reduces cation mixing, thereby reducing the amount of gas generated in manganese-rich batteries (Mn-rich batteries) during cycling and / or storage.
[0052] This invention controls the composition and content of the negative electrode active material contained in the negative electrode. Specifically, this invention includes a carbon-based active material as the negative electrode active material. The carbon-based active material includes at least one selected from natural graphite and artificial graphite, wherein the proportion of natural graphite is greater than 50% by weight based on the total weight of the carbon-based active material. Specifically, in the carbon-based active material, the proportion of natural graphite is in the range of greater than 50% by weight and less than 100% by weight, or in the range of 75% by weight and 100% by weight. Alternatively, the proportion of natural graphite can be 100% by weight, which means that the carbon-based active material consists only of natural graphite. More specifically, in the carbon-based active material, the proportion of natural graphite is in the range of 70% by weight and 90% by weight, or in the range of 75% by weight and 85% by weight.
[0053] In one embodiment, the negative electrode active material layer comprises a carbon-based active material as the active material. Specifically, the carbon-based active material comprises at least one selected from natural graphite, artificial graphite, condensed graphite, pyrolytic carbon, carbon microspheres, mesophase calcined carbon derived from tar or pitch as raw materials, and graphitized coke. For example, graphite can be used as the carbon-based active material. Graphite may comprise at least one selected from natural graphite and artificial graphite. For example, the carbon-based active material may comprise only natural graphite, or in some cases, a mixture of natural and artificial graphite.
[0054] If the proportion of artificial graphite in the negative electrode active material is excessively increased, the amount of gas generated during charge / discharge or storage and the capacity expression rate below 3.5 V will increase. This invention takes into account these characteristics, the reduction in manufacturing costs associated with using natural graphite, and the increase in electrode capacity associated with using artificial graphite, resulting in the above composition ratio.
[0055] In another embodiment, the average orientation index (OI) of the carbon-based active material, as defined by the following mathematical formula 1, is less than 15.
[0056] [Mathematical Expression 1]
[0057] OI=I 004 / I 110
[0058] In mathematical formula 1, I 110This represents the intensity of the peak corresponding to the (110) crystal plane of the carbon-based active material, as measured by X-ray diffraction (XRD) spectroscopy; and I 004 This represents the intensity of the peak corresponding to the (004) crystal plane of the carbon-based active material, as measured by X-ray diffraction (XRD) spectroscopy.
[0059] Specifically, the orientation index of the carbon-based active material, as defined by Formula 1, is in the range of 0.1 to 15, 1 to 15, 1 to 10, 3 to 8, or 6 to 7. In this invention, during the fabrication of the negative electrode, a magnetic field is applied to the negative electrode active material layer before drying, causing the carbon-based active material to be oriented in a direction perpendicular to the current collector. By orienting the active material contained in the negative electrode active material layer, this invention improves the lithium-ion mobility, thereby improving fast charge / discharge efficiency.
[0060] In this invention, the term "carbon-based active material orientation" or "carbon-based active material arrangement" refers to the arrangement of specific crystal planes (e.g., the ab-axis crystal plane of graphite) representing the two-dimensional planar structure of the carbon-based active material constituting the active material particles, at a predetermined tilt angle relative to the surface of the current collector. This may differ from the arrangement of the carbon-based active material particles themselves having a specific orientation within the negative electrode active material layer.
[0061] In this invention, a small value for the "orientation index (OI)" can refer to the arrangement of the crystal planes of the carbon-based active material contained in the negative electrode active material layer at a high angle (e.g., a near-vertical angle, 45° or more; specifically, 60° or more) relative to the surface of the current collector. Conversely, a large value for the "orientation index (OI)" can refer to the arrangement of specific crystal planes (e.g., the ab-axis crystal plane of graphite) representing the two-dimensional planar structure of the carbon-based active material contained in the negative electrode active material layer at a low angle (e.g., less than 45°) relative to the surface of the current collector, or to random orientation.
[0062] Furthermore, in this invention, "crystal plane of carbon-based active material" refers to the plane in which the atoms of carbon-based active material form the external shape of the crystal, and can refer to the crystal plane containing the carbon-based active material, or the crystal plane containing the a-axis / b-axis / ab-axis of the carbon-based active material crystal.
[0063] Furthermore, the method for controlling the orientation index of the aforementioned carbon-based active materials according to the mathematical formula 1 is as follows. During the manufacturing process of the negative electrode, a negative electrode slurry is coated onto a current collector, a magnetic field is applied to the surface of the coated negative electrode slurry, and then the negative electrode slurry is dried, thereby manufacturing a negative electrode in which the crystallization characteristics of the active material are controlled.
[0064] Here, the step of coating the negative electrode slurry involves discharging the negative electrode slurry and coating it onto the surface of the moving current collector. There are no particular limitations on this step, as long as it is a method commonly used in the art; however, die coating is preferred. Die coating can be performed using a slit die equipped with a shim for controlling the discharge conditions of the negative electrode slurry. In this case, by controlling the shape of the shim, the load and coating thickness of the negative electrode slurry coated onto the negative electrode current collector can be easily controlled.
[0065] On the other hand, the step of applying a magnetic field can be a step of controlling the crystallization characteristics of the active material contained in the negative electrode slurry. Specifically, this step involves applying a magnetic field to the surface of the negative electrode slurry coated onto the current collector, causing the ab-axis crystal planes of the carbon-based active material contained in each negative electrode slurry to align at a high angle relative to the current collector.
[0066] At this point, the magnetic field can be applied by magnetic components located at the upper and lower parts of the current collector, which is coated with a negative electrode paste on its surface and is in motion. Furthermore, the polarities of the magnetic components located at the upper and lower parts can be different from each other.
[0067] Furthermore, the orientation degree (OI) of the carbon-based active material contained in the negative electrode slurry can be adjusted by the strength of the applied magnetic field. Therefore, the step of applying the magnetic field can be carried out under predetermined magnetic field strength conditions.
[0068] Specifically, in the step of applying the magnetic field, a magnetic field in the range of 1,000 to 20,000 G (Gauss) can be applied. Specifically, a magnetic field with an intensity of 1,500 G to 9,000 G; 2,000 G to 6,500 G; 5,500 G to 8,500 G; or 2,500 G to 3,500 G can be applied.
[0069] In addition, the application of the magnetic field can be carried out for 1 to 20 seconds, specifically 1 to 15 seconds; 1 to 10 seconds; 5 to 20 seconds; 10 to 20 seconds; 11 to 18 seconds; 1 to 5 seconds; 4 to 9 seconds; or 6 to 11 seconds.
[0070] As an example, in the step of applying the magnetic field, a magnetic field of 3,000 ± 50 G can be applied to the negative electrode slurry for 1 to 30 seconds.
[0071] Furthermore, as described above, the step of applying a magnetic field is performed by introducing magnetic components to the upper and lower parts of the coated negative electrode paste. The size of the magnetic components can be adjusted to be larger than the size of the coated negative electrode paste, so that the magnetic field applied to the negative electrode paste can be uniformly applied to the entire surface of the negative electrode paste. For example, the length ratio of the magnetic component to the width direction length of the negative electrode paste can be 105% to 200%. Specifically, the length ratio of the magnetic component to the width direction length of the negative electrode paste can be 110% to 180%; 110% to 160%; 110% to 140%; 110% to 130%; 130% to 150%; or 105% to 120%.
[0072] Following the step of applying a magnetic field, the present invention includes steps of drying the negative electrode and calendering the negative electrode. In the step of drying the negative electrode, the negative electrode slurry after the magnetic field is applied is dried at a high temperature to form a negative electrode active material layer on the current collector. The step of drying the negative electrode can be performed, for example, by applying hot air at a temperature of 160°C to 250°C. The calendering step can be performed by pressing the dried negative electrode on one or both sides. The pressing method can be a roller press or a flat press. For example, the calendering step is performed using a roller press such that the porosity of the negative electrode active material layer after rolling is 25 ± 5%.
[0073] In one embodiment, the negative electrode further comprises a silicon-based active material as the active material. Specifically, based on the total weight of the active material in the negative electrode active material layer, the content of the silicon-based active material ranges from 0.1 wt% to 30 wt%. More specifically, based on the total weight of the active material contained in the negative electrode active material layer, the content of the silicon-based active material ranges from 0.1 wt% to 30 wt%, 1 wt% to 30 wt%, 1 wt% to 10 wt%, 0.1 wt% to 5 wt%, 5 wt% to 30 wt%, or 6 wt% to 20 wt%. Compared to carbon-based active materials, silicon-based active materials have the advantage of being able to improve the negative electrode capacity. On the other hand, a problem with silicon-based active materials is that they cause volume changes during the charge and discharge process. Therefore, it is desirable to control the content of silicon-based active materials when considering the application area or shape of the secondary battery.
[0074] Specifically, silicon-based active materials include those selected from silicon (Si), silicon carbide (SiC), silicon carbide / carbon composites (Si / C), and silicon oxide (SiO). qAt least one of the following (where 0.8 ≤ q ≤ 2.5). As an example, the active material may simultaneously contain graphite and silicon (Si) particles. The graphite may contain at least one selected from natural graphite having a layered crystal structure and artificial graphite having an isotropic structure. The silicon (Si) particles may be particles containing silicon (Si) as the main (semi-)metallic component, and may contain silicon (Si) particles, silicon oxide (SiO, SiO2) particles, or a mixture of silicon (Si) particles and silicon oxide (SiO, SiO2) particles.
[0075] Furthermore, silicon-based active materials can be doped with Li, Mg, Al, Ca, or Ti, or can form alloys with them. Additionally, silicon-based active materials can be surface-treated with a carbon coating to suppress volume expansion during charging or improve conductivity.
[0076] Specifically, the secondary battery is a pouch-shaped secondary battery. As another example, the secondary battery is a cylindrical or prismatic secondary battery.
[0077] Secondary batteries
[0078] In one embodiment of the invention, the secondary battery can be a cylindrical, prismatic, or pouch-shaped secondary battery. For example, the secondary battery is a pouch-shaped secondary battery. The pouch-shaped secondary battery includes an electrode assembly in which various unit structures consisting of stacked positive electrodes, separators, and negative electrodes repeat.
[0079] A secondary battery includes an electrode assembly comprising a positive electrode, a negative electrode, and a separator located between the positive and negative electrodes, as well as a casing surrounding the electrode assembly.
[0080] The secondary battery according to the present invention includes an electrode assembly having a structure in which a plurality of positive electrodes and a plurality of negative electrodes are arranged alternately, with a separator located between them. The lithium secondary battery is equipped with the negative electrode of the present invention described above, thereby improving lithium-ion diffusion rate, providing excellent fast-charging performance, and also having the advantage of high energy density.
[0081] Here, since the negative electrode active material contained in the negative electrode has the same structure as described above, a detailed description thereof will be omitted. The negative electrode may comprise a negative electrode current collector and a layer of negative electrode active material located on the negative electrode current collector and containing the negative electrode active material. Specifically, the negative electrode is manufactured by coating, drying, and calendering the negative electrode active material on the negative electrode current collector, and may optionally further comprise conductive materials, organic binder polymers, fillers, etc., as needed.
[0082] In this case, the negative electrode active material may contain at least one selected from natural graphite and artificial graphite. Furthermore, it may further contain a silicon-based active material as the negative electrode active material.
[0083] Conductive materials may include at least one of the following substances: carbon black such as acetylene black, danca black, kejjung black, Super-P, furnace black, lamp black and thermal cracking carbon black; graphene; carbon nanotubes; and carbon fibers, but not limited thereto.
[0084] As an example, the negative electrode active material layer can contain carbon black, carbon nanotubes, carbon fibers, etc., as conductive materials, either alone or in combination.
[0085] At this point, based on the total weight of 100 parts by weight of the negative electrode active material layer, the content of conductive material can be from 0.1 to 10 parts by weight. Specifically, based on the total weight of 100 parts by weight of the negative electrode active material layer, the conductive material can be 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, 2 to 6 parts by weight, or 0.5 to 2 parts by weight. By controlling the content of conductive material within the above range, the present invention can prevent a decrease in charging capacity caused by an increase in negative electrode resistance due to a low content of conductive material. Furthermore, the present invention can prevent problems such as a decrease in charging capacity caused by a reduction in the content of negative electrode active material due to excessive conductive material exceeding the above range, or an increase in resistance caused by an increase in the loading of the negative electrode active material layer.
[0086] Furthermore, the adhesive is a component that assists in the bonding of the negative electrode active material and the conductive material, as well as their bonding with the current collector, and can be appropriately applied within a range that does not degrade the electrical performance of the negative electrode. For example, the adhesive may contain at least one selected from the following substances: polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene propylene diene monomer (EPDM), sulfonated ethylene propylene diene monomer (EPDM), styrene-butadiene rubber (SBR), and fluororubber.
[0087] Based on the total weight of 100 parts by weight of the negative electrode active material layer, the binder content can be from 0.1 to 10 parts by weight. Specifically, based on the total weight of 100 parts by weight of the negative electrode active material layer, the binder can be from 0.1 to 8 parts by weight, 0.1 to 5 parts by weight, 0.1 to 3 parts by weight, or 2 to 6 parts by weight. By controlling the binder content contained in the negative electrode active material layer within the above range, the present invention can prevent a decrease in the adhesion of the active material layer due to a low binder content, or a decrease in the electrical performance of the negative electrode due to an excessive binder content.
[0088] In addition, the average thickness of the negative electrode active material layer can be from 100 μm to 800 μm, specifically from 100 μm to 780 μm; from 100 μm to 550 μm; from 120 μm to 500 μm; from 140 μm to 200 μm; or from 140 μm to 160 μm.
[0089] Furthermore, there are no particular restrictions on the negative electrode current collector, as long as it has high conductivity and does not cause chemical changes in the battery. For example, copper, stainless steel, nickel, titanium, calcined carbon, etc., can be used. In the case of copper or stainless steel, copper or stainless steel that has undergone surface treatment with carbon, nickel, titanium, silver, etc., can be used.
[0090] Furthermore, similar to positive electrode current collectors, negative electrode current collectors can enhance their adhesion to the negative electrode active material by forming fine irregularities on their surface, and can take various forms such as films, sheets, foils, meshes, porous bodies, foams, and nonwoven fabrics. Moreover, considering the conductivity and total thickness of the manufactured negative electrode, the average thickness of the negative electrode current collector can be appropriately applied in the range of 3 to 500 μm.
[0091] In addition, the positive electrode includes a positive electrode active material layer containing positive electrode active material on the positive electrode current collector, and the positive electrode active material layer may optionally further include conductive materials, adhesives, other additives, etc. as needed.
[0092] Positive electrode active materials are materials that can undergo electrochemical reactions at the positive electrode current collector. The description of positive electrode active materials is as described above.
[0093] Furthermore, based on the total weight of 100 parts by weight of the positive electrode active material layer, the content of the positive electrode active material can be 85 parts by weight or more. Specifically, based on the total weight of 100 parts by weight of the positive electrode active material layer, the content of the positive electrode active material can be 90 parts by weight or more, 93 parts by weight or more, or 95 parts by weight or more.
[0094] In addition to containing positive electrode active materials, the positive electrode active material layer may further contain conductive materials, binders, other additives, etc.
[0095] At this point, the conductive material is used to improve the electrical properties of the positive electrode, and can be any conductive material commonly used in the art. Specifically, the conductive material may comprise at least one of the following substances: natural graphite; artificial graphite; carbon black such as acetylene black, tantalizer black, Ketjen black, Super-P, furnace black, lamp black, and thermally cracked carbon black; graphene; and carbon nanotubes.
[0096] Furthermore, based on 100 parts by weight of each positive electrode active material layer, the content of conductive material can be from 0.1 to 5 parts by weight. Specifically, based on 100 parts by weight of each positive electrode active material layer, the content of conductive material can be from 0.1 to 4 parts by weight; 2 to 4 parts by weight; 1.5 to 5 parts by weight; 1 to 3 parts by weight; 0.1 to 2 parts by weight; or 0.1 to 1 part by weight.
[0097] Furthermore, the adhesive is used to bond the positive electrode active material, positive electrode additive, and conductive material together, and can be used without particular restriction, as long as it has this function. Specifically, the adhesive may contain at least one resin selected from the following substances: polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-co-HFP), polyvinylidene fluoride (PVdF), polyacrylonitrile, polymethyl methacrylate, and copolymers thereof. As an example, the adhesive may contain polyvinylidene fluoride.
[0098] Furthermore, based on 100 parts by weight of each positive electrode active material layer, the binder content can be 1 to 10 parts by weight. Specifically, based on 100 parts by weight of the positive electrode active material layer, the binder content can be 2 to 8 parts by weight or 1 to 5 parts by weight.
[0099] There is no particular limitation on the total thickness of the positive electrode active material layer, but it can be in the range of 50 μm to 800 μm, more specifically 100 μm to 800 μm; 80 μm to 150 μm; 120 μm to 170 μm; 150 μm to 300 μm; 200 μm to 600 μm; or 150 μm to 390 μm.
[0100] Furthermore, as the positive electrode current collector, a positive electrode current collector with high conductivity that does not cause chemical changes in the battery can be used. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc., can be used. In the case of aluminum or stainless steel, aluminum or stainless steel that has undergone surface treatment with carbon, nickel, titanium, silver, etc., can also be used. Moreover, considering the conductivity and overall thickness of the manufactured positive electrode, the average thickness of the current collector can be appropriately applied in the range of 3 μm to 500 μm.
[0101] Furthermore, the separator between the positive and negative electrodes of the lithium secondary battery is an insulating film with high ion permeability and mechanical strength, and there are no particular limitations, as long as it is commonly used in the art. Specifically, the separator may comprise at least one polymer selected from chemically resistant and hydrophobic polypropylene; polyethylene; and polyethylene-propylene copolymers. The separator may be in the form of a porous polymer substrate comprising the above-mentioned polymers, such as a sheet or nonwoven fabric. In some cases, it may be in the form of a composite separator, wherein organic or inorganic particles are coated onto the porous polymer substrate by an organic binder. Furthermore, the average pore size of the separator may be from 0.01 μm to 10 μm, and the average thickness may be from 5 μm to 300 μm.
[0102] On the other hand, there are no particular limitations on the secondary battery according to the present invention, but it can be a secondary battery that can include stacked, Z-shaped or Z-shaped stacked electrode assemblies.
[0103] Furthermore, the secondary battery according to the present invention may contain a lithium salt-containing electrolyte. The lithium salt-containing electrolyte may consist of an electrolyte and a lithium salt. As the electrolyte, non-aqueous organic solvents, organic solid electrolytes, inorganic solid electrolytes, etc., may be used.
[0104] As non-aqueous organic solvents, aprotic organic solvents such as N-methyl-2-pyrrolidone, ethylene carbonate, propylene carbonate, butyl carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triphosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, or ethyl propionate can be used.
[0105] As an organic solid electrolyte, for example, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polylysine, polysulfides, polyvinyl alcohol, polyvinylidene fluoride, or polymers containing ion-dissociating groups can be used.
[0106] As an inorganic solid electrolyte, for example, nitrides, halides or sulfates of Li can be used, such as Li3N, LiI, Li5Ni2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH or Li3PO4-Li2S-SiS2.
[0107] Lithium salts are substances that dissolve well in non-aqueous electrolytes, such as LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB. 10 Cl 10 LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylic acids, lithium tetraphenylborate or lithium imide.
[0108] In addition, to improve charge / discharge characteristics and flame retardancy, the electrolyte can be supplemented with substances such as pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, (condensed) glycol dimethyl ethers, hexamethylphosphoryltriamine, nitrobenzene derivatives, sulfur, quinone imine dyes, and N-substituted compounds. Alzolidinediones, N,N-substituted imidazolines, ethylene glycol dialkyl ethers, ammonium salts, pyrroles, 2-methoxyethanol, aluminum trichloride, etc. In some cases, to impart non-flammability, halogenated solvents such as carbon tetrachloride or trifluoroethylene may be further included. To improve high-temperature storage properties, carbon dioxide gas may be further included, and fluoroethylene carbonate (FEC), propylene sulpholactone (PRS), etc., may also be included.
[0109] On the other hand, in one embodiment, the present invention provides a battery module comprising the aforementioned secondary battery, or a battery pack comprising the battery module.
[0110] Battery packs can be used as power sources for medium to large-sized devices that require high-temperature stability, long cycle life, and high rate capability. Specific examples of such devices include: power tools powered by electric motors; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheelers, including electric bicycles and electric scooters; electric golf carts; and energy storage systems. More specifically, hybrid electric vehicles (HEVs) may be mentioned, but are not limited to.
[0111] Furthermore, the positive and negative electrodes can be wound and housed in a cylindrical, prismatic, or pouch-shaped battery in a jelly-roll form, or they can be folded or stacked and housed in a pouch-shaped battery. For example, the secondary battery according to the present invention can be a pouch-shaped battery.
[0112] As described above, the secondary battery according to the present invention can be used in battery modules or battery packs that include multiple said secondary batteries as unit batteries. Specifically, it can be used in portable devices such as mobile phones, laptops, and digital cameras, as well as in electric vehicles such as hybrid electric vehicles (HEVs).
[0113] Preferred Implementation
[0114] The invention will be described in more detail below through examples and other means. However, the scope of the invention is not limited thereto.
[0115] Examples and Comparative Examples: Manufacturing of Secondary Batteries
[0116] By using positive electrode active material (Li 1.35 [Ni 0.360 Co 0.005 Mn 0.635 A positive electrode slurry (solids content: 65 wt%) was prepared by adding O2 (lithium-excess manganese oxide), conductive material (carbon nanotubes), and binder (polyvinylidene fluoride) to N-methyl-2-pyrrolidone (NMP) as a solvent in a weight ratio of 96.0:1.5:2.5. The positive electrode slurry was coated on one side of a positive electrode current collector (Al foil) with a thickness of 12 μm, and then dried and calendered to manufacture the positive electrode.
[0117] A negative electrode slurry (solids content: 50 wt%) was prepared by adding a negative electrode active material (a mixture of artificial and natural graphite), a conductive material (carbon black), and a binder (styrene-butadiene rubber) in a weight ratio of 96.7:1.0:2.3 to distilled water as a solvent. The negative electrode slurry was coated onto one side of a negative electrode current collector (Cu foil) with a thickness of 8 μm, then dried and calendered to manufacture the negative electrode. The mixture of artificial and natural graphite constituting the negative electrode active material is shown in Table 1 below.
[0118] In a drying chamber, a porous polyethylene membrane is inserted between the prepared positive and negative electrodes, and the prepared non-aqueous electrolyte is injected to manufacture a secondary battery.
[0119] [Table 1]
[0120] Experimental Example 1: Calculation of gas generation and voltage-based capacity change rate during charge and discharge.
[0121] For each secondary battery manufactured in the Examples and Comparative Examples, the amount of gas generated during charge and discharge was measured. Specifically, each secondary battery was subjected to charge and discharge cycles at 45°C, 300 cycles, and 1 C. At the completion of the charge and discharge cycles, the gas generated during this period and the capacity change rate based on voltage were analyzed. The amount of gas generated by each secondary battery is shown in Table 2 below. Furthermore, for the gases generated in the secondary batteries according to Examples 1 and 2 and Comparative Example 2, the type and amount of the generated gases were analyzed using gas chromatography, and the results are shown in... Figure 1 middle.
[0122] Furthermore, the capacities below 3.5 V and above 3.5 V for each secondary battery were determined separately. The rate of change of capacity below 3.5 V after 300 charge-discharge cycles is also shown in Table 2 below. Additionally, the rate of change of capacity based on voltage during charge-discharge cycles is shown in... Figure 2 middle.
[0123] [Table 2]
[0124] First, referring to Table 2, it can be seen that when lithium-excess manganese-rich oxide is used as the positive electrode active material, the gas generation tends to increase to a certain level as the content of artificial graphite in the negative electrode increases. Specifically, it can be seen that the gas generation of the secondary batteries according to Examples 1 to 5 is less than 160 mL. In particular, it is confirmed that the gas generation of the secondary battery according to Example 1 is the lowest, at 120.6 mL. The gas generation of the secondary batteries according to Comparative Examples 1 and 2 is calculated to be 172.7 mL and 185.2 mL, respectively. It is confirmed that when the content of artificial graphite in the negative electrode active material is 50% by weight or more, the gas generation increases sharply. Figure 1 This allows us to confirm the type and amount of gas generated in the secondary batteries according to Examples 1 and 2 and Comparative Example 1. From... Figure 1 It can be seen that as the content of artificial graphite increases, the amount of gas generated increases, especially the amount of CO2 gas generated increases sharply. By controlling the content of artificial graphite in the negative electrode active material to less than 50% by weight, the present invention can reduce the amount of gas generated, especially significantly reduce the generation of CO2 gas.
[0125] In addition, refer to Table 2 and Figure 2 It can be seen that in batteries containing lithium-excess manganese-rich oxide as the positive electrode active material, the capacity expression rate below 3.5 V increases with the increase of the artificial graphite content in the negative electrode. However, despite the increase in artificial graphite content, the secondary batteries according to Examples 1 to 5 effectively suppressed the capacity expression rate below 3.5 V. In contrast, it was confirmed that the capacity expression rate below 3.5 V of the secondary batteries according to Comparative Examples 1 and 2 exceeded 120%. In particular, in Figure 2 In comparing the secondary batteries according to Examples 1 and 2 and Comparative Example 1, it can be seen that the capacity above 3.5 V did not show a significant difference as charge-discharge cycles continued. In contrast, the secondary batteries according to Examples 1 and 2 showed that the capacity below 3.5 V was effectively suppressed.
[0126] Experimental Example 2: Calculation of Gas Generation and Voltage-Based Capacity Change Rate During High-Temperature Storage
[0127] For each secondary battery manufactured in Examples 1 and 2 and Comparative Example 1, the amount of gas generated during high-temperature storage was measured. Specifically, each secondary battery was stored at 60°C for 8 weeks, and the gas generated during this period and the voltage-based capacity change rate were analyzed. The amount of gas generated by each secondary battery is shown in Table 3 below. Furthermore, for the gas generated in each secondary battery, the type and amount of the generated gas were analyzed using gas chromatography, and the results are shown in... Figure 3 middle.
[0128] Furthermore, the capacities below 3.5 V and above 3.5 V for each secondary battery were determined separately. The capacity change rate over 8 storage cycles at 60°C is also shown in Table 3 below. Additionally, the voltage-based capacity change rate for each storage period during high-temperature storage is shown in... Figure 4 middle.
[0129] [Table 3]
[0130] First, refer to Table 3 and Figure 3 It was confirmed that, compared with the secondary batteries according to Examples 1 and 2, the secondary battery according to Comparative Example 1 showed a significant improvement in both gas production and capacity expression rate below 3.5 V. Furthermore, referring to… Figure 4 When comparing the secondary batteries according to Examples 1 and 2 with Comparative Example 1, it can be seen that no significant difference was observed in capacity above 3.5 V during high-temperature storage. In contrast, it can be seen that the capacity expression below 3.5 V of the secondary batteries according to Examples 1 and 2 was effectively suppressed.
[0131] Although the present invention has been described above with reference to preferred embodiments, those skilled in the art or of ordinary skill in the art should understand that the present invention can be modified and altered in various ways without departing from the spirit and scope of the invention, and such modifications and alterations will be described in the claims below.
[0132] Therefore, the technical scope of the present invention should not be limited to the contents described in the specific embodiments of the specification, but should be defined by the scope of the claims.
Claims
1. A secondary battery, the secondary battery comprising: A positive electrode, comprising lithium oxide as a positive electrode active material, wherein the Mn content in the lithium oxide is based on a total metal content excluding lithium of 50 mol% or more, or wherein the molar ratio of lithium to transition metals exceeds 1; and The negative electrode comprises a carbon-based active material, wherein The carbon-based active material comprises at least one selected from natural graphite and artificial graphite, and the proportion of natural graphite exceeds 50% by weight based on the total weight of the carbon-based active material.
2. The secondary battery according to claim 1, wherein... The lithium oxide is represented by chemical formula 1: [Chemical Formula 1] Li x M (1-y-z) Mn y M 1 z O2 In chemical formula 1, M is selected from at least one of Ni, Co and Fe; M 1 It is at least one element selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B and Mo; x, y, and z satisfy 0.8≤x≤2, 0.5≤y<1, 0≤z≤0.1, and y+z=1, respectively.
3. The secondary battery according to claim 1, wherein... In chemical formula 1, x is in the range of 1.2 to 1.
5.
4. The secondary battery according to claim 1, wherein... The lithium oxide is represented by chemical formula 2: [Chemical Formula 2] Li x M (1-y) Mn y O2 In chemical formula 2, M is selected from at least one of Ni and Co; x and y satisfy 1.01≤x≤2 and 0.5≤y<0.9 respectively.
5. The secondary battery according to claim 1, wherein... In the carbon-based active material, the proportion of natural graphite is in the range of 75% to 100% by weight.
6. The secondary battery according to claim 1, wherein... In the carbon-based active material, the proportion of natural graphite is in the range of 70% to 90% by weight.
7. The secondary battery according to claim 1, wherein... The average orientation index (OI) of the carbon-based active material, as defined by the following mathematical formula 1, is 15 or less: [Mathematical Expression 1] OI=I 004 / I 110 In mathematical formula 1, I 110 This represents the intensity of the peak corresponding to the (110) crystal plane of the carbon-based active material, as measured by X-ray diffraction (XRD) spectroscopy; and I 004 This indicates the intensity of the peak corresponding to the (004) crystal plane of the carbon-based active material as measured by X-ray diffraction (XRD) spectroscopy.
8. The secondary battery according to claim 1, wherein The negative electrode further comprises a silicon-based active material as the active material, and Based on the total weight of the negative electrode active material, the content of the silicon-based active material is in the range of 0.1% to 30% by weight.
9. The secondary battery according to claim 8, wherein The silicon-based active material comprises silicon (Si), silicon carbide (SiC), silicon carbide / C composites (Si / C), and silicon oxide (SiO). q At least one of the following: (where 0.8 ≤ q ≤ 2.5).
10. The secondary battery according to claim 1, wherein... The secondary battery is a pouch-type secondary battery.
11. The secondary battery according to claim 1, wherein... The secondary battery is a cylindrical or prismatic secondary battery.
Citation Information
Patent Citations
Communication methods and devices, storage media and program products
KR1020250002631A