solid-state batteries

By using carbon-based conductive materials in the positive electrode layer and terminal electrodes of solid-state batteries, and especially by controlling their content between 30-95% by volume, the short-circuit problem caused by metal migration is solved, ensuring the stability and discharge capacity of the battery.

CN123076941APending Publication Date: 2026-11-10MURATA MFG CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202580025790.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-07-26
Filing Date
2025-07-15
Publication Date
2026-11-10

AI Technical Summary

Technical Problem

In existing solid-state batteries, during repeated charging and discharging, the migration of metal materials can lead to short circuits between the positive and negative electrodes, affecting the proper functioning of the battery.

Method used

Carbon-based conductive materials are used as the main components of the positive electrode layer, negative electrode layer and terminal electrode. In particular, the content of carbon-based conductive materials in the positive terminal electrode is controlled between 30-95% by volume to suppress the migration of metal materials.

Benefits of technology

It effectively suppresses metal migration, ensures the structural stability and discharge capacity of the battery, avoids short-circuit faults, and realizes the normal function of solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123076941A_ABST
    Figure CN123076941A_ABST
Patent Text Reader

Abstract

A solid-state battery is provided, comprising a positive electrode layer, a negative electrode layer, a solid electrolyte layer, a positive terminal electrode electrically connected to the positive electrode layer, and a negative terminal electrode electrically connected to the negative electrode layer. At least the positive electrode layer and the positive terminal electrode each comprise a carbon-based conductive material. The content of the carbon-based conductive material in the positive terminal electrode is greater than 30% by volume and less than 95% by volume.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to a solid-state battery. Background Technology

[0002] Previously, rechargeable batteries were used for various purposes. For example, they were used as power sources for electronic devices such as smartphones and laptops.

[0003] In secondary batteries, liquid electrolytes are typically used as the medium for the movement of ions participating in charging and discharging. That is, the so-called electrolyte is used in secondary batteries. However, in such secondary batteries, safety requirements are generally placed on preventing electrolyte leakage. Furthermore, organic solvents and other flammable substances used in the electrolyte also require safety considerations.

[0004] Therefore, solid-state batteries that use solid electrolytes instead of liquid electrolytes were studied.

[0005] Existing technical documents

[0006] Patent documents

[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-220107 Summary of the Invention

[0008] The technical problem that the invention aims to solve

[0009] The inventors of this application have noticed that existing solid-state batteries have technical problems that need to be overcome, and have discovered the necessity of taking countermeasures. Specifically, the following technical problems have been discovered.

[0010] Solid-state batteries include electrode layers comprising a positive electrode layer and a negative electrode layer, and terminal electrodes electrically connected to the electrode layers. Conventionally, highly conductive metal materials such as silver have been used in the electrode layers and terminal electrodes (Patent Document 1). However, in such solid-state batteries, repeated charging and discharging can cause the metal material contained in the electrode layers or terminal electrodes to ionize and migrate towards the counter electrode, where it may be reduced and deposited as metal, potentially resulting in migration. Depending on the situation, such migration can cause a short circuit between the positive and negative electrodes, potentially preventing the solid-state battery from functioning properly.

[0011] This disclosure was made in view of the following technical problem: the main objective of this disclosure is to provide a solid-state battery that can suppress migration and function properly as a solid-state battery.

[0012] Technical solutions for solving technical problems

[0013] To achieve the above objectives, one embodiment of the solid-state battery disclosed herein includes a positive electrode layer, a negative electrode layer, a solid electrolyte layer, a positive terminal electrode electrically connected to the positive electrode layer, and a negative terminal electrode electrically connected to the negative electrode layer. At least the positive electrode layer and the positive terminal electrode each comprise a carbon-based conductive material. The content of the carbon-based conductive material in the positive terminal electrode is greater than 30% by volume and less than 95% by volume.

[0014] The effects of the invention

[0015] One embodiment of this disclosure relates to a solid-state battery that can suppress migration and function appropriately as a solid-state battery. Attached Figure Description

[0016] Figure 1 This is a schematic perspective view of a solid-state battery according to one embodiment of the present disclosure.

[0017] Figure 2 Observe in the direction of the arrow Figure 1 A schematic cross-sectional view of the solid-state battery at section AA.

[0018] Figure 3 This is a schematic cross-sectional view showing the AA section of a solid-state battery according to another embodiment of this disclosure. Detailed Implementation

[0019] The solid-state battery of this disclosure will now be described in detail. While the description is based on the accompanying drawings as needed, the illustrations are merely schematic and exemplary for the purpose of understanding this disclosure, and the appearance and size ratios may differ from the actual product. It should be noted that the applicant provides the following description and embodiments to enable those skilled in the art to fully understand this disclosure, and it is not intended to limit the subject matter described in the patent claims. That is, this disclosure is not particularly limited to the embodiments described below, and can be appropriately modified and implemented within its scope. Furthermore, for ease of explanation or understanding of key points, embodiments are sometimes shown for convenience, but partial substitutions and / or combinations of the structures shown in different embodiments are possible. In the description of such embodiments, sometimes repeated descriptions of substantially the same matters are omitted, and only the differences are described. In particular, the same effects produced by the same structure are sometimes not mentioned sequentially in each embodiment.

[0020] The term "sectional view" as used in this specification refers to a shape viewed from a direction substantially perpendicular to the stacking direction of the solid-state battery's layered structure (in short, a shape taken from a plane parallel to the thickness direction of the layers). Furthermore, the terms "top view" or "top view shape" as used in this specification refer to a schematic diagram of the object viewed from above or below along the thickness direction of the layer (i.e., the aforementioned stacking direction).

[0021] In this specification, the terms "up and down" and "left and right" as used directly or indirectly correspond to the up and down and left and right directions in the figures, respectively. Unless otherwise stated, the same reference numerals or symbols indicate the same parts / areas or have the same meaning. In a preferred embodiment, it can be understood that the vertical direction downward (i.e., the direction of gravity) corresponds to the "down direction," and its opposite direction corresponds to the "up direction."

[0022] In this disclosure, "solid-state battery" broadly refers to a battery whose constituent elements are made of solids, and narrowly refers to an all-solid-state battery whose constituent elements (particularly preferably all constituent elements) are made of solids. In a preferred embodiment, the solid-state battery of this disclosure is a stacked solid-state battery in which the layers constituting the battery structural unit are stacked on top of each other, preferably such layers are made of sintered material. "Solid-state battery" is a so-called "secondary battery" that can be repeatedly charged and discharged. "Secondary battery" is not overly limited to its name, and may also include, for example, energy storage devices.

[0023] The features of this disclosure relate to the electrode layer and terminal electrodes included in a solid-state battery. Hereinafter, in order to understand the overall structure of the solid-state battery, the basic structure of the solid-state battery of this disclosure will be described. However, the structure of the solid-state battery described herein is merely an example for understanding the invention and does not limit the invention.

[0024] [Basic Structure of Solid-State Batteries]

[0025] Figure 1 This is a schematic perspective view of a solid-state battery according to one embodiment of the present disclosure. Figure 2 Observe in the direction of the arrow Figure 1 A schematic cross-sectional view of a solid-state battery at section AA. A solid-state battery has at least positive and negative electrode layers, and a solid electrolyte. Specifically, as... Figure 1 as well as Figure 2 As shown, the solid-state battery 200 includes a solid-state battery stack 100, which includes a battery structure unit consisting of a positive electrode layer 10A, a negative electrode layer 10B and at least a solid electrolyte layer 20 between them.

[0026] The solid-state battery 200 disclosed herein typically includes: The solid-state battery stack 100, along the stacking direction L, has at least one battery structural unit consisting of a positive electrode layer 10A, a negative electrode layer 10B, and a solid electrolyte layer 20 interposed therebetween; and The positive terminal electrode 40A and the negative terminal electrode 40B are respectively disposed on opposite sides of the solid battery stack 100.

[0027] In the solid battery stack 100, the positive electrode layer 10A and the negative electrode layer 10B are alternately stacked with a solid electrolyte layer 20 in between.

[0028] In the solid-state battery 200, the various layers that make up the battery can be formed by firing, and the positive electrode layer, negative electrode layer, and solid electrolyte layer can also be formed as fired layers. For example, the positive electrode layer, negative electrode layer, and solid electrolyte layer can be fired together integrally, so that the solid-state battery stack can also form an integral fired body.

[0029] The positive electrode layer 10A is an electrode layer that at least contains a positive electrode active material. The positive electrode layer may further contain a solid electrolyte. In one embodiment, the positive electrode layer 10A is composed of a sintered body containing at least positive electrode active material particles and solid electrolyte particles. On the other hand, the negative electrode layer 10B is an electrode layer that at least contains a negative electrode active material. The negative electrode layer 10B may further contain a solid electrolyte. In one embodiment, the negative electrode layer 10B is composed of a sintered body containing at least negative electrode active material particles and solid electrolyte particles. The positive electrode layer 10A and the negative electrode layer 10B having such structures can also be referred to as a "composite positive electrode" and a "composite negative electrode," respectively.

[0030] The positive and negative electrode active materials are substances that participate in electron transfer in a solid-state battery. Ions move (conduct) between the positive and negative electrode layers via the solid electrolyte, thus transferring electrons and enabling charging and discharging. Each electrode layer of the positive and negative electrode layers is particularly preferably a layer capable of intercalating or deintercalating lithium ions or sodium ions. That is, the solid-state battery is preferably an all-solid-state secondary battery, in which lithium ions or sodium ions move between the positive electrode layer 10A and the negative electrode layer 10B via the solid electrolyte, thereby enabling charging and discharging of the battery.

[0031] As a positive electrode active material included in the positive electrode layer 10A, examples include at least one selected from the group consisting of lithium phosphate compounds having a NASICON-type structure, lithium phosphate compounds having an olivine-type structure, lithium-containing layered oxides, and lithium-containing oxides having a spinel-type structure.

[0032] Examples of lithium-containing phosphate compounds with a NASICON-type structure include Li3V2(PO4)3. Examples of lithium-containing phosphate compounds with an olivine-type structure include Li3Fe2(PO4)3, LiFePO4, and / or LiMnPO4. Examples of lithium-containing layered oxides include LiCoO2 and / or LiCo. 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, etc. Examples of lithium-containing oxides with a spinel-type structure include LiMn2O4 and / or LiNi. 0.5 Mn 1.5 O4, etc. The types of lithium compounds are not particularly limited; examples include lithium transition metal complex oxides and lithium transition metal phosphates. Lithium transition metal complex oxides are a general term for oxides containing lithium and one or more transition metal elements as constituent elements. Lithium transition metal phosphates are a general term for phosphate compounds containing lithium and one or more transition metal elements as constituent elements. The types of transition metal elements are not particularly limited; examples include cobalt (Co), nickel (Ni), manganese (Mn), and iron (Fe).

[0033] Furthermore, as positive electrode active materials capable of intercalating and deintercalating sodium ions, examples include at least one selected from the group consisting of sodium-containing phosphate compounds having a NASICON-type structure, sodium-containing phosphate compounds having an olivine-type structure, sodium-containing layered oxides, and sodium-containing oxides having a spinel-type structure. For example, in the case of sodium-containing phosphate compounds, examples include at least one selected from the group consisting of Na3V2(PO4)3, NaCoFe2(PO4)3, Na2Ni2Fe(PO4)3, Na3Fe2(PO4)3, Na2FeP2O7, Na4Fe3(PO4)2(P2O7), and NaFeO2 as a sodium-containing layered oxide.

[0034] Furthermore, the positive electrode active material can be, for example, an oxide, a disulfide, a chalcogenide, or a conductive polymer. Oxides can be, for example, titanium oxide, vanadium oxide, or manganese dioxide. Disulfides can be, for example, titanium disulfide or molybdenum sulfide. Chalcogenides can be, for example, niobium selenide. Conductive polymers can be, for example, disulfides, polypyrrole, polyaniline, polythiophene, poly(p-phenylene), polyacetylene, or poly(phenylene oxide).

[0035] (Negative electrode active material)

[0036] Examples of negative electrode active materials included in the negative electrode layer 10B include at least one selected from the group consisting of oxides, carbon materials such as lead oxide, lead-lithium compounds, lithium alloys, lithium phosphate compounds with a NASICON-type structure, lithium phosphate compounds with an olivine-type structure, and lithium oxides with a spinel-type structure. The oxides contain at least one element selected from the group consisting of titanium (Ti), silicon (Si), tin (Sn), chromium (Cr), iron (Fe), niobium (Nb), and molybdenum (Mo). Examples of lithium alloys include Li-Al. Examples of lithium phosphate compounds with a NASICON-type structure include Li3V2(PO4)3 and / or LiTi2(PO4)3. Examples of lithium phosphate compounds with an olivine-type structure include Li3Fe2(PO4)3 and / or LiCuPO4. Examples of lithium oxides with a spinel-type structure include Li4Ti5O. 12 wait.

[0037] Furthermore, as a negative electrode active material capable of intercalating and deintercalating sodium ions, examples include at least one selected from the group consisting of sodium phosphate compounds having a NASICON-type structure, sodium phosphate compounds having an olivine-type structure, and sodium oxides having a spinel-type structure.

[0038] In addition, in the solid-state battery 200, the positive electrode layer 10A and the negative electrode layer 10B can be made of the same material or they can be made of different materials.

[0039] Furthermore, the positive electrode layer 10A and / or the negative electrode layer 10B may contain a sintering aid. Examples of sintering aids include at least one selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, boron oxide, silicon oxide, bismuth oxide, and phosphorus oxide.

[0040] The thickness of the positive electrode layer 10A and the negative electrode layer 10B is not particularly limited. For example, they can be 2 μm or more and 50 μm or less, especially 5 μm or more and 30 μm or less.

[0041] (Positive current collector layer / Negative current collector layer)

[0042] Although not a necessary element of the electrode layers, the positive electrode layer 10A and the negative electrode layer 10B can each include a positive current collector layer 11A and a negative current collector layer 11B, respectively. The positive current collector layer 11A and the negative current collector layer 11B can also each have a foil-like form. On the other hand, if the focus is on improving electronic conductivity, reducing the manufacturing cost of solid-state batteries, and / or reducing the internal resistance of solid-state batteries through integral firing, then the positive current collector layer 11A and the negative current collector layer 11B can also each have a fired body form. The positive current collector layer 11A and the negative current collector layer 11B can also each have an electrical connection portion for external electrical connection, and can be configured to be electrically connected to the terminal electrode.

[0043] Furthermore, when the positive current collector layer 11A and the negative current collector layer 11B have the form of sintered bodies, they can be composed of sintered bodies containing conductive materials and sintering aids. The sintering aids contained in the positive current collector layer 11A and the negative current collector layer 11B can be selected, for example, from the same materials that can be contained in the positive and / or negative electrode layers.

[0044] As described above, in a solid-state battery, the positive electrode current collector layer 11A and the negative electrode current collector layer 11B are not essential, and it is also possible to consider a solid-state battery without such a positive electrode current collector layer 11A and negative electrode current collector layer 11B. That is, the solid-state battery of this disclosure can also be a solid-state battery without current collector layers.

[0045] (Solid electrolyte layer)

[0046] A solid electrolyte layer 20 may be disposed at least between the positive electrode layer 10A and the negative electrode layer 10B. That is, the solid electrolyte layer 20 may exist around the positive electrode layer 10A and / or the negative electrode layer 10B in a manner that extends from between the positive electrode layer 10A and the negative electrode layer 10B. The solid electrolyte contained in the solid electrolyte layer is a material capable of conducting lithium ions or sodium ions. In particular, the solid electrolyte constituting the battery structural unit in a solid-state battery may form a lithium ion conducting layer 20 between the positive electrode layer and the negative electrode layer. As a specific solid electrolyte, it may be any one or more of crystalline solid electrolytes, glass-based solid electrolytes, and glass-ceramic solid electrolytes.

[0047] Crystalline solid electrolytes include, for example, oxide-based crystalline materials and sulfide-based crystalline materials. Examples of oxide-based crystalline materials include lithium phosphate compounds with a NASICON structure, oxides with a perovskite structure, oxides with a garnet-type or garnet-like structure, and oxide glass-ceramic lithium-ion conductors.

[0048] Examples of lithium phosphate compounds with a NASICON structure include Li xM y (PO4)3 (1≤x≤2, 1≤y≤2, M is at least one selected from the group consisting of titanium (Ti), germanium (Ge), aluminum (Al), gallium (Ga), and zirconium (Zr). As an example of a lithium phosphate compound having a NASICON structure, Li can be cited as an example. 1.2 Al 0.2 Ti 1.8 (PO4)3, etc. As an example of an oxide with a perovskite structure, La can be cited. 0.55 Li 0.35 TiO3, etc. As an example of oxides with garnet-type or garnet-like structures, Li7La3Zr2O can be cited. 12 Furthermore, thio-LISICON, for example, Li, is a sulfide-based crystalline material. 3.25 Ge 0.25 P 0.75 S4 and Li 10 GeP2S 12 Crystalline solid electrolytes may also contain polymeric materials (e.g., polyethylene oxide (PEO)).

[0049] Glass-based solid electrolytes include, for example, oxide-based glass materials and sulfide-based glass materials. An example of an oxide-based glass material is 50Li₄SiO₄. 50Li3BO3, etc. In addition, 30Li2S is used as a sulfide-based glass material. 26B2S3 44LiI, 63Li2S 36SiS2 1Li3PO4, 57Li2S 38SiS2 5Li4SiO4, 70Li2S 30P2S5 and 50Li2S 50GeS2, etc.

[0050] Glass-ceramic solid electrolytes include, for example, oxide-based and sulfide-based glass-ceramic materials. As oxide-based glass-ceramic materials, examples include lithium-aluminum-titanium phosphate compounds (LATP) and lithium-aluminum-germanium phosphate compounds (LAGP). For example, Li... 1.07 Al 0.69 Ti 1.46 (PO4)3, etc. Furthermore, LAGP is, for example, Li. 1.5 Al 0.5 Ge 1.5(PO4), etc. In addition, as a sulfide-based glass-ceramic material, there is, for example, Li7P3S. 11 And Li 3.25 P 0.95 S4, etc.

[0051] Furthermore, examples of solid electrolytes capable of conducting sodium ions include sodium-containing phosphate compounds with a NASICON structure, oxides with a perovskite structure, and oxides with garnet-type or garnet-like structures. For example, Na... x M y (PO4)3 (1≤x≤2, 1≤y≤2, M is at least one selected from the group consisting of Ti, Ge, Al, Ga and Zr).

[0052] The solid electrolyte layer 20 may also contain sintering aids. The sintering aids contained in the solid electrolyte layer 20 may be selected from the same materials as those that may be contained in the positive electrode layer 10A and / or the negative electrode layer 10B.

[0053] The thickness of the solid electrolyte layer 20 is not particularly limited. The thickness of the solid electrolyte layer 20 located between the positive electrode layer 10A and the negative electrode layer 10B can be, for example, more than 1 μm and less than 15 μm, and in particular, more than 1 μm and less than 5 μm.

[0054] (Terminal electrode)

[0055] In a solid-state battery 200, terminal electrodes 40A and 40B are generally provided. Specifically, terminal electrodes 40A and 40B are provided on the side of the solid-state battery. More specifically, a positive electrode side terminal electrode 40A connected to the positive electrode layer 10A and a negative electrode side terminal electrode 40B connected to the negative electrode layer 10B are provided (see reference). Figure 2 The terminal electrodes 40A and 40B contain conductive material.

[0056] [Features of the solid-state battery disclosed herein]

[0057] The inventors have conducted in-depth research on solutions for providing solid-state batteries capable of suppressing migration. As a result, it was found that using carbon-based conductive materials as both the electrode layer and the terminal electrode is effective. In particular, considering that migration in solid-state batteries is largely caused by the ionization of metal materials contained in the positive electrode under high voltage conditions and their movement towards the negative electrode, it was discovered that by using carbon-based conductive materials at least in the positive electrode layer and the positive terminal electrode, migration can be suppressed. Furthermore, it was newly discovered that when the content of carbon-based conductive material in the terminal electrode is within a specified range, a solid-state battery that suppresses migration and functions appropriately as a solid-state battery can be provided.

[0058] In the solid-state battery 200 of this disclosure, at least the positive electrode layer 10A and the positive terminal electrode 40A electrically connected to the positive electrode layer 10A each contain a carbon-based conductive material. Specifically, based on the volume of the positive terminal electrode 40A, the content of the carbon-based conductive material contained in the positive terminal electrode 40A is greater than 30% by volume and less than 95% by volume. In both the positive electrode layer 10A and the negative electrode layer 10B, at least the positive electrode layer 10A contains a carbon-based conductive material, and in both the positive terminal electrode 40A and the negative terminal electrode 40B, at least the positive terminal electrode 40A contains a carbon-based conductive material, thereby suppressing the ionization of the metal material in the positive electrode layer 10A and the positive terminal electrode 40A due to the applied voltage. As a result, migration is suppressed, and short circuits caused by migration are suppressed. Furthermore, by ensuring that the content of the carbon-based conductive material in the positive terminal electrode 40A is within the aforementioned range, a solid-state battery capable of suppressing migration and functioning appropriately as a solid-state battery can be obtained.

[0059] In this specification, "functioning appropriately as a solid-state battery" refers to excellent mechanical strength that sufficiently ensures the discharge capacity of the solid-state battery and prevents damage during use. For example, if the content of carbon-based conductive material in the positive terminal electrode 40A is less than 30% by volume, the electronic conductivity in the positive terminal electrode 40A cannot be sufficiently ensured, the discharge capacity becomes too low, and it may not function appropriately as a solid-state battery. Furthermore, if the content of carbon-based conductive material in the positive terminal electrode 40A is 95% by volume or more, the adhesion strength between the solid-state battery stack 100, which includes the electrode layer and the solid electrolyte layer, and the terminal electrode may decrease. As a result, during use of the solid-state battery (e.g., during charging or discharging), the terminal electrode may peel off from the solid-state battery stack 100, affecting structural stability. In the solid-state battery disclosed herein, the content of carbon-based conductive material in the positive terminal electrode 40A is greater than 30% by volume and less than 95% by volume. By keeping the content of the carbon-based conductive material within the aforementioned range, sufficient discharge capacity can be achieved, and the solid-state battery stack 100 can be appropriately bonded to the terminal electrode 40A. Therefore, the solid-state battery of this disclosure, by containing the carbon-based conductive material, can suppress migration and function appropriately as a solid-state battery.

[0060] Preferably, the content of carbon-based conductive material in the positive terminal electrode 40A can be 35% by volume or more, more preferably 40% by volume or more. If the content of carbon-based conductive material in the positive terminal electrode 40A is within the above range, a solid-state battery with better discharge capacity can be provided. Furthermore, the content of carbon-based conductive material in the positive terminal electrode 40A is more preferably 90% by volume or less. If the content of carbon-based conductive material in the positive terminal electrode 40A is within the above range, a solid-state battery with better adhesion strength between the solid-state battery stack 100 and the terminal electrode 40A can be obtained.

[0061] Furthermore, similar to the positive terminal electrode 40A, the negative terminal electrode 40B, which is electrically connected to the negative electrode layer 10B, may also contain a carbon-based conductive material. The negative terminal electrode 40B may contain the carbon-based conductive material within the same content range as described above for the positive terminal electrode 40A. That is, both the positive terminal electrode 40A and the negative terminal electrode 40B may each contain a carbon-based conductive material. This further suppresses migration.

[0062] As the carbon-based conductive material included in the terminal electrode, at least one of graphite (black lead), carbon fiber, carbon black, and carbon nanotubes can be used. For example, vapor-grown carbon fiber (VGCF) can be used. For the carbon black, at least one of thermal cracking carbon black, furnace black, channel black, acetylene black, and Ketjen black can be used. For the carbon nanotubes, multi-walled carbon nanotubes (MWCNTs) such as single-walled carbon nanotubes (SWCNTs) and double-walled carbon nanotubes (DWCNTs) can be used. More preferably, the carbon-based conductive material included in the terminal electrode can be at least one of graphite and VGCF. Thus, a solid-state battery that can suppress migration and function appropriately as a solid-state battery can be obtained.

[0063] When both the positive terminal electrode 40A and the negative terminal electrode 40B contain carbon-based conductive materials, the carbon-based conductive materials contained in the positive terminal electrode 40A and the negative terminal electrode 40B can be the same material or different materials. Furthermore, the content of the carbon-based conductive material in the positive terminal electrode 40A and the negative terminal electrode 40B can be the same content or different content.

[0064] [First Implementation Method]

[0065] like Figure 2 As shown, in a solid-state battery, at least one of the positive electrode layer 10A and the negative electrode layer 10B may have a current collector layer. That is, the electrode layer may have an electrode active material layer and a current collector layer. When the electrode layer has a current collector layer, at least the current collector layer 11A of the positive electrode layer 10A may contain a carbon-based conductive material. In other words, in a solid-state battery, at least the positive electrode layer 10A may have a current collector layer 11A containing a carbon-based conductive material.

[0066] Furthermore, similar to the positive electrode layer 10A, the negative electrode layer 10B may also have a current collector layer 11B comprising a carbon-based conductive material. That is, both the positive electrode layer 10A and the negative electrode layer 10B may each have a current collector layer comprising a carbon-based conductive material. This allows for more appropriate suppression of migration.

[0067] If greater discharge capacity and higher structural stability are desired, the content of carbon-based conductive material in the current collector layer can be greater than 30% by volume and less than 90% by volume, more preferably greater than 40% by volume and less than 90% by volume, based on the volume of the current collector layer. By keeping the content of carbon-based conductive material in the current collector layer within the above range, a solid-state battery that can suppress migration and function appropriately as a solid-state battery can be provided.

[0068] While not specifically limited, at least one of the following can be used as the carbon-based conductive material in the current collector layer: graphite (black lead), carbon fiber, carbon black, and carbon nanotubes. For example, VGCF can be used as the carbon fiber. For example, at least one of the following can be used as the carbon black: thermal cracking carbon black, furnace black, channel black, acetylene black, and Ketjen black. For example, multi-walled carbon nanotubes (MWCNTs) such as single-walled carbon nanotubes (SWCNTs) and double-walled carbon nanotubes (DWCNTs) can be used. If high conductivity, structural stability as the current collector layer, heat resistance, and ease of handling during manufacturing are important, then graphite is preferred as the carbon-based conductive material in the current collector layer. This allows for the acquisition of a solid-state battery that can suppress migration and function more appropriately as a solid-state battery.

[0069] When both the positive electrode layer 10A and the negative electrode layer 10B have a current collector layer containing a carbon-based conductive material, the carbon-based conductive materials contained in the current collector layer 11A in the positive electrode layer 10A and the current collector layer 11B in the negative electrode layer 10B can be the same material or different materials. Furthermore, the content of the carbon-based conductive material can be the same or different in the current collector layers 11A and 11B of the positive electrode layer 10A and the negative electrode layer 10B.

[0070] The content of carbon-based conductive materials in the electrode layer and terminal electrodes can be determined by combining electron microscopy observation and energy-dispersive X-ray (EDX) image analysis. Specifically, a cross-section is cut using an ion milling device or similar equipment, and a cross-sectional image of the current collector layer or terminal electrode is obtained using a scanning electron microscope (SEM) (Hitachi High-Tech Co., Ltd., model SU-8040). Then, EDX mapping is performed on the obtained cross-sectional image. Next, image analysis software (e.g., ImageJ) is used to calculate the area ratio of carbon-based conductive materials in the current collector layer or terminal electrode. The area ratio of carbon-based conductive materials in the current collector layer or terminal electrode can be considered to be the same as the volume ratio of carbon-based conductive materials in the current collector layer or terminal electrode. Through these operations, the content of carbon-based conductive materials can be determined.

[0071] [Second Implementation]

[0072] Figure 3This is a schematic cross-sectional view showing a solid-state battery 201 according to a second embodiment of the present disclosure. As shown, in the solid-state battery 201 according to the second embodiment, at least one of the positive electrode layer 10A and the negative electrode layer 10B is a "current collector-free" battery (which can also be simply referred to as a "current collector-free solid-state battery," "current collector-free battery," or "current collector-free solid-state battery," etc.). In the solid-state battery 201 according to the second embodiment of the present disclosure, since there is "no current collector," there is no current collector or current collector layer provided in the solid-state battery stack 100 in a manner that is in direct contact with the electrode layer, nor is there a current collector or current collector layer provided extending inside the electrode layer. Thus, the battery of the present disclosure, in particular the solid-state battery stack 100, can have a current collector-free structure or a current collector-free structure.

[0073] Furthermore, the current collector / current collector layer that is not present in the structure referred to as "without a current collector" refers to a "conductive layer that does not contain active material (e.g., a sintered body layer formed by a conductive agent and a sintering aid)" that is provided from the viewpoint of reducing internal resistance, etc., and is distinct from a "layer containing active material". Therefore, the solid-state battery of this embodiment does not have such a "conductive layer that does not contain active material" specifically provided for reducing internal resistance (in particular, a "conductive layer that does not contain active material" that is provided in contact with a "layer containing active material" or is provided inside such a layer containing active material).

[0074] In the solid-state battery 201 of the second embodiment, at least the positive electrode layer 10A and the negative electrode layer 10B are current collector-free electrode layers (hereinafter also referred to as "current collector-free electrode layers"). This current collector-free electrode layer may contain a carbon-based conductive material. This means that the current collector-free electrode layer contains at least an electrode active material and a carbon-based conductive material as a conductive aid. That is, within the electrode layer, the electrode active material and the carbon-based conductive material as a conductive aid may coexist. The current collector-free electrode layer may further contain auxiliary components such as a solid electrolyte and / or sintering aids.

[0075] Furthermore, similar to the positive electrode layer 10A, the negative electrode layer 10B can also be a current-free electrode layer containing a carbon-based conductive material. That is, both the positive electrode layer 10A and the negative electrode layer 10B can be current-free electrode layers containing a carbon-based conductive material as a conductive aid. This further suppresses migration.

[0076] If a greater discharge capacity and higher structural stability are desired, the content of carbon-based conductive material in the current collector-less electrode layer can be greater than 1% by volume and less than 20% by volume, more preferably 3% by volume and less than 15% by volume, based on the volume of the current collector-less electrode layer. By keeping the content of carbon-based conductive material in the current collector layer within the above range, a solid-state battery that can suppress migration and function more appropriately as a solid-state battery can be provided.

[0077] As the carbon-based conductive material included in the current collector-free electrode layer, at least one of graphite (black lead), carbon fiber, carbon black, and carbon nanotubes can be used. For example, VGCF can be used as the carbon fiber. For example, at least one of thermal cracking carbon black, furnace black, channel black, acetylene black, and Ketjen black can be used as the carbon black. For example, multi-walled carbon nanotubes (MWCNTs) such as single-walled carbon nanotubes (SWCNTs) and double-walled carbon nanotubes (DWCNTs) can be used. If the discharge capacity of the solid-state battery, the structural stability of the current collector-free electrode layer, and the ease of handling during manufacturing are important considerations, then VGCF is preferred as the carbon-based conductive material included in the current collector-free electrode layer. Therefore, a solid-state battery that can suppress migration and function more appropriately as a solid-state battery can be obtained.

[0078] When both the positive electrode layer 10A and the negative electrode layer 10B are current collector-less electrode layers containing carbon-based conductive materials, the carbon-based conductive materials contained in each of the positive electrode layer 10A and the negative electrode layer 10B can be the same material or different materials. Furthermore, the content of the carbon-based conductive material in the positive electrode layer 10A and the negative electrode layer 10B can be the same or different.

[0079] The aforementioned terminal electrodes, current collector layers, and current collector-free electrode layers containing carbon-based conductive materials may substantially not contain metallic materials from the group consisting of Ag, Ni, Cu, Sn, Zn, and Al. These metallic materials may migrate due to ionization caused by electrolytic corrosion, etc. The solid-state battery of this disclosure substantially does not contain these metallic materials, but instead contains carbon-based conductive materials, thereby appropriately suppressing the occurrence of migration. In addition, "substantially does not contain" in this specification means that the presence of trace amounts of components that are unavoidably or accidentally mixed in during the formation of the electrode layers is permissible. For example, such unavoidable or accidental components may be allowed to contain less than 5% by weight, preferably less than 2% by weight, and more preferably less than 1% by weight, based on the respective volume total of the terminal electrodes, current collector layers, and / or current collector-free electrode layers.

[0080] [Solid-state battery manufacturing method]

[0081] The solid-state battery disclosed herein can be manufactured by printing methods such as screen printing, green sheet methods using green sheets, or a combination thereof. Hereinafter, for the purpose of understanding this disclosure, the use of printing methods and green sheet methods will be described in detail, but this disclosure is not limited to these methods.

[0082] (Formation process of solid-state battery stacked precursor)

[0083] In this process, various pastes, including positive electrode paste, negative electrode paste, solid electrolyte layer paste, current collector paste, and insulating layer paste, are used as inks. That is, the pastes are applied using a printing method to form a paste with a specified structure on the support substrate.

[0084] During printing, by sequentially stacking printing layers with a specified thickness and pattern shape, a solid-state battery preform corresponding to the specified solid-state battery structure can be formed on the substrate. The type of pattern forming method is not particularly limited as long as it can form the specified pattern; for example, screen printing and gravure printing can be selected.

[0085] The paste can be prepared by wet mixing a specified constituent material of each layer appropriately selected from the group consisting of a positive electrode active material, a negative electrode active material, a conductive material, a solid electrolyte, an insulating material, a binder, and a sintering aid with an organic carrier obtained by dissolving an organic material in a solvent. The positive electrode paste may, for example, include a positive electrode active material, a conductive material, a solid electrolyte, a binder, a sintering aid, an organic material, and a solvent. The negative electrode paste may, for example, include a negative electrode active material, a conductive material, a solid electrolyte, a binder, a sintering aid, an organic material, and a solvent. The paste for the solid electrolyte layer may, for example, include a solid electrolyte, a binder, a sintering aid, an organic material, and a solvent. The positive and negative electrode current collector pastes may include conductive materials, active materials, solid electrolytes, binders, sintering aids, organic materials, and a solvent. At least the conductive material included in the positive electrode current collector paste is a carbon-based conductive material. Alternatively, the conductive materials included in the positive and negative electrode current collector pastes may each be carbon-based conductive materials. Furthermore, for example, when the positive electrode layer and / or negative electrode layer are used as current collector-free electrode layers, the conductive material contained in the positive electrode paste and / or negative electrode paste that are current collector-free electrode layers can be a carbon-based conductive material.

[0086] The paste for the insulating layer may, for example, contain insulating materials including heat-resistant resins (imide resins and / or imidazole resins), binders, sintering aids, organic materials, and solvents.

[0087] The organic materials contained in the paste are not particularly limited, and at least one polymeric material selected from the group consisting of polyvinyl alcohol acetal resin, cellulose resin, polyacrylic acid resin, polyurethane resin, polyvinyl acetate resin, and polyvinyl alcohol resin can be used. The type of solvent is not particularly limited, and for example, it can be any one or more organic solvents selected from butyl acetate, N-methylpyrrolidone, toluene, terpineol, and N-methylpyrrolidone.

[0088] In wet mixing, media can be used, specifically ball milling or Visco milling. On the other hand, wet mixing methods without media can also be used, such as sand milling, high-pressure homogenizers, or kneading dispersion.

[0089] The supporting substrate is not particularly limited as long as it can support each paste layer; for example, it can be a release film that has undergone a release treatment on one side. Specifically, a substrate made of polymer materials such as polyethylene terephthalate can be used. When the paste layers are supplied to the firing process while held on the substrate, a substrate that exhibits heat resistance to the firing temperature can be used.

[0090] By drying the applied paste on a heated plate, positive electrode green sheets, negative electrode green sheets, solid electrolyte green sheets, electrode separation green sheets, and / or protective layer green sheets with specified shapes and thicknesses are formed on a substrate (e.g., PET film).

[0091] Next, each green sheet is peeled off from the substrate. After peeling, green sheets of each component of a battery structural unit are sequentially stacked along the stacking direction, thereby forming a solid-state battery stack precursor. After stacking, a solid electrolyte layer, electrode separation section, and / or protective layer can also be provided on the side regions of the electrode green sheets by screen printing.

[0092] (Firing process)

[0093] In the firing process, the solid-state battery stack precursor is fired. Although this is just an example, firing is carried out by heating in a nitrogen atmosphere containing oxygen or in the atmosphere. Firing can be performed simultaneously with pressurization of the solid-state battery stack precursor in the stacking direction (in the case, the stacking direction and the direction perpendicular to that stacking direction).

[0094] By undergoing such a firing process, a solid-state battery stack is formed, and the desired solid-state battery can eventually be obtained.

[0095] (Terminal electrode formation process)

[0096] Terminal electrodes can be formed by coating the exposed positive and negative electrode sides of the battery element with a terminal electrode paste containing a conductive material. If the terminal electrodes on the positive and negative electrode sides are arranged to extend to the lower surface of the battery element, they can be connected to the mounting pads with a small area during surface mounting of the solid-state battery, which is therefore preferable. After coating the terminal electrode paste with the conductive material, the terminal electrodes are fired. This allows the solid-state battery of the present disclosure to be manufactured.

[0097] Alternatively, the terminal electrodes can also be manufactured by resin curing without firing. Specifically, a resin-curing conductive paste is used in the terminal electrode paste, and this paste is applied to the exposed positive and negative electrode sides of the battery element. The resin material is then cured by thermosetting or photocuring (UV curing), thereby manufacturing a solid-state battery with terminal electrodes. In the terminal electrodes of the solid-state battery obtained in this way, the composition of the materials contained in the terminal electrodes remains substantially unchanged during the manufacturing process. That is, the volume ratio of the conductive material used in manufacturing in the terminal electrodes can be considered the same as the volume ratio of the conductive material in the terminal electrodes of the obtained solid-state battery.

[0098] In addition, one embodiment of the present disclosure as described above includes the following preferred embodiments.

[0099] First method: A solid-state battery, It comprises a positive electrode layer, a negative electrode layer, a solid electrolyte layer, a positive terminal electrode electrically connected to the positive electrode layer, and a negative terminal electrode electrically connected to the negative electrode layer. At least the positive electrode layer and the positive terminal electrode each comprise a carbon-based conductive material. The content of the carbon-based conductive material in the positive terminal electrode is greater than 30% by volume and less than 95% by volume.

[0100] Second method: A solid-state battery, in the first embodiment described above, wherein the content of the carbon-based conductive material in the positive terminal electrode is 40% by volume or more and 90% by volume or less.

[0101] Third method: A solid-state battery, in either the first or second embodiment described above, wherein the carbon-based conductive material contained in the positive terminal electrode is at least one of graphite and carbon black.

[0102] Fourth method: A solid-state battery, in any one of the first to third embodiments described above, wherein the positive electrode layer, the negative electrode layer, the positive terminal electrode, and the negative terminal electrode each comprise a carbon-based conductive material.

[0103] Fifth method: A solid-state battery, in any one of the first to fourth embodiments described above, wherein at least the positive electrode layer includes a current collector layer in both the positive electrode layer and the negative electrode layer. The current collector layer comprises the carbon-based conductive material. The content of the carbon-based conductive material in the current collector layer is greater than 30% by volume and less than 90% by volume.

[0104] Sixth method: In a solid-state battery, in the fifth embodiment described above, the content of the carbon-based conductive material in the current collector layer is 40% by volume or more and 90% by volume or less.

[0105] Seventh method: In a solid-state battery, in either the fifth or sixth embodiment described above, the carbon-based conductive material contained in the current collector layer is graphite.

[0106] Eighth method: A solid-state battery, in any one of the first to fourth embodiments described above, wherein, of the positive electrode layer and the negative electrode layer, at least the positive electrode layer is a current collector-less electrode layer without a current collector layer. The content of the carbon-based conductive material in the current collectorless electrode layer is greater than 1% by volume and less than 15% by volume.

[0107] Ninth method: In a solid-state battery, in the eighth embodiment described above, the content of the carbon-based conductive material in the current collector-free electrode layer is 3% by volume or more and 15% by volume or less.

[0108] Tenth method: In a solid-state battery, in either the eighth or ninth embodiment described above, the carbon-based conductive material contained in the current collectorless electrode layer is VGCF.

[0109] Eleventh method: A solid-state battery, in any one of the first to tenth embodiments described above, wherein at least the positive electrode layer and the positive terminal electrode do not contain Ag, Ni, Cu, Zn, Sn, or Al.

[0110] Example

[0111] Verification experiments were conducted based on this disclosure. The solid-state battery structure adopts... Figure 2 as well as Figure 3 The structure.

[0112] <Example 1>

[0113] According to the solid-state battery manufacturing method described above, the solid-state battery of Example 1 was manufactured. Furthermore, the terminal electrodes were fabricated by resin curing. Specifically, a solid-state battery was manufactured using a positive electrode paste containing lithium cobalt oxide, a negative electrode paste containing lithium titanate, a positive and negative current collector pastes containing a specified amount of graphite (Imerys Corporation, SFG15), and positive and negative terminal electrode pastes containing a thermosetting resin (phenolic resin), graphite (Japan Black Lead Co., Ltd., JB-10), and carbon black (Lion Special Chemicals, Ketjen Black EC300J).

[0114] <Comparative Example 1>

[0115] A solid-state battery was manufactured using the same method as in Example 1, except that silver (Mitsui Metal Mining, SF-KS) was used instead of graphite in the positive and negative current collector pastes.

[0116] <Comparative Example 2>

[0117] A solid-state battery was manufactured using the same method as in Example 1, except that silver (Mitsui Metal Mining, SF-KS) was used instead of graphite and carbon black in the positive and negative electrode pastes.

[0118] <Examples 2-4>

[0119] A solid-state battery was manufactured using the same method as in Example 1, except that the graphite content in the positive and negative current collector pastes was changed.

[0120] <Examples 5-6 and Comparative Examples 3-4>

[0121] A solid-state battery was manufactured using the same method as in Example 1, except that the total content of graphite and carbon black in the positive and negative electrode pastes was changed.

[0122] <Example 7>

[0123] A solid-state battery was manufactured using the same method as in Example 1, except that silver (Mitsui Metal Mining, SF-KS) was used instead of graphite in the negative electrode current collector paste.

[0124] <Example 8>

[0125] Manufactured using Figure 3The solid-state battery shown has a current collector-free structure. Specifically, a solid-state battery was manufactured using a positive electrode paste containing lithium cobalt oxide and VGCF (manufactured by RESONAC, VGCF-H), a negative electrode paste containing lithium titanate and VGCF (manufactured by RESONAC, VGCF-H), and positive and negative electrode pastes containing thermosetting resin (phenolic resin), graphite (manufactured by Japan Black Lead Co., Ltd., JB-10), and carbon black (manufactured by Lion Special Chemicals, Ketjen Black EC300J).

[0126] <Examples 9-10>

[0127] Aside from changing the VGCF content in the positive and negative electrode pastes, a solid-state battery was manufactured in the same manner as in Example 8.

[0128] <Example 11>

[0129] A solid-state battery was manufactured in the same manner as in Example 8, except that silver (Mitsui Metal Mining, SF-KS) was used instead of VGCF in the negative electrode paste.

[0130] (Evaluation of battery characteristics)

[0131] The battery cells manufactured as described above are charged and discharged under the conditions of charging voltage 2.5V, charging rate 0.1C, discharging voltage 0.5V, and discharging rate 0.1C. Battery cells that achieve a discharge capacity of more than 90% of the theoretical discharge capacity are judged as good (A), battery cells that achieve a discharge capacity of more than 50% but less than 90% of the theoretical discharge capacity are judged as acceptable (B), and battery cells that achieve a discharge capacity of less than 50% of the theoretical discharge capacity are judged as poor (C).

[0132] (Evaluation of reliability (resistance to migration and structural stability))

[0133] For the battery cell manufactured with the described structure, a charge-discharge cycle test was conducted in a constant temperature bath at 105°C under the conditions of a charging voltage of 2.5V, a charging rate of 0.3C, a discharging voltage of 0.5V, and a discharging rate of 1C. During the 3-month test, any cell that exhibited migration and / or failed to charge / discharge normally due to peeling of the terminal electrodes was deemed defective (C). Regarding migration, if the charging voltage did not reach 2.5V after 20 hours, migration was considered to have occurred.

[0134] As a comprehensive evaluation, the case where both battery characteristics and reliability evaluation results are good (A) is evaluated as the best product (AA), the case where one is good (A) and the other is acceptable (B) is evaluated as the good product (AB), the case where both are acceptable (B) is evaluated as the acceptable product (BB), the case where either or both are bad (C) is evaluated as the bad product (CC). The best product (AA), good product (AB), and acceptable product (BB) are set as qualified, and the bad product (CC) is set as unqualified.

[0135] Table 1 shows the evaluation results of the solid-state batteries of Examples 1-11 and Comparative Examples 1-4. Furthermore, the "conductive material ratio" shown in the table corresponds to the volume ratio of carbon-based conductive materials in the electrode layers or terminal electrodes of the manufactured solid-state batteries.

[0136]

[0137] Based on the above results, in Comparative Examples 1 and 2, where either the positive electrode layer or the terminal electrode contains silver, migration from the silver-containing positive electrode layer or terminal electrode was confirmed. On the other hand, in Examples 1-11 and Comparative Example 4, where at least the positive electrode layer and the positive terminal electrode contain carbon-based conductive materials, no migration was confirmed. From the above results, it can be confirmed that using carbon-based conductive materials can improve migration resistance.

[0138] On the other hand, in Comparative Example 3, where the content of carbon-based conductive material in the terminal electrode was 95% by volume, the terminal electrode peeled off from the solid-state battery laminate during the test. Furthermore, in Comparative Example 4, where the content of carbon-based conductive material in the terminal electrode was 30% by volume, the discharge capacity was too small. On the other hand, Examples 1 to 11, where the content of carbon-based conductive material in the terminal electrode was greater than 30% by volume and less than 95% by volume, also showed good results in terms of discharge capacity. From the above, it can be seen that, according to this disclosure, a solid-state battery capable of suppressing migration and functioning appropriately as a solid-state battery is provided.

[0139] Furthermore, in Examples 1-3 and 5-6, where the content of carbon-based conductive material in the current collector layer is greater than 30% by volume, a higher discharge capacity was observed compared to Example 4, where the content is less than 30% by volume. Additionally, in Examples 8 and 9, where the content of carbon-based conductive material in the electrode layer without a current collector layer is greater than 1% by volume, a higher discharge capacity was observed compared to Example 10, where the content is less than 1% by volume.

[0140] The embodiments of this disclosure have been described above, but only typical examples have been illustrated. Therefore, this disclosure is not limited thereto, and those skilled in the art will readily understand that various methods can be conceived without altering the spirit of this disclosure.

[0141] Industrial availability

[0142] The solid-state battery disclosed herein can be applied to a wide range of fields assuming energy storage. While merely examples, the solid-state battery disclosed herein can be applied to electrical / information / communication fields using mobile devices (e.g., electrical / electronic equipment fields or mobile devices including mobile phones, smartphones, laptops, digital cameras, activity meters, wrist computers, electronic paper, RFID tags, card-type electronic money, smartwatches, etc.), home / small industrial applications (e.g., power tools, golf carts, home / care / industrial robots), large industrial applications (e.g., forklifts, elevators, port cranes), transportation systems (e.g., hybrid vehicles, electric vehicles, buses, trams, electric-assisted bicycles, electric motorcycles, etc.), power system applications (e.g., various power generation systems, load conditioners, smart grids, general household energy storage systems, etc.), medical applications (medical devices such as headphones and hearing aids), pharmaceutical applications (medical management systems, etc.), and IoT fields, space / deep-sea applications (e.g., space probes, underwater research vessels, etc.), etc.

[0143] Explanation of reference numerals in the attached figures

[0144] 10A: Positive electrode layer; 10B: Negative electrode layer; 11A: Positive current collector layer; 11B: Negative current collector layer; 12A: Positive active material layer; 12B: Negative active material layer; 20: Solid electrolyte layer; 40A: Positive terminal electrode; 40B: Negative terminal electrode; 60: Outer layer material; 100: Solid battery stack; 200: Solid battery.

Claims

1. A solid-state battery, It comprises a positive electrode layer, a negative electrode layer, a solid electrolyte layer, a positive terminal electrode electrically connected to the positive electrode layer, and a negative terminal electrode electrically connected to the negative electrode layer. At least the positive electrode layer and the positive terminal electrode each comprise a carbon-based conductive material. The content of the carbon-based conductive material in the positive terminal electrode is greater than 30% by volume and less than 95% by volume.

2. The solid-state battery according to claim 1, wherein, The content of the carbon-based conductive material in the positive terminal electrode is more than 40% by volume and less than 90% by volume.

3. The solid-state battery according to claim 1 or 2, wherein, The carbon-based conductive material contained in the positive terminal electrode is at least one of graphite and carbon black.

4. The solid-state battery according to any one of claims 1 to 3, wherein, The positive electrode layer, the negative electrode layer, the positive terminal electrode, and the negative terminal electrode each contain a carbon-based conductive material.

5. The solid-state battery according to any one of claims 1 to 4, wherein, In the positive electrode layer and the negative electrode layer, at least the positive electrode layer includes a current collector layer. The current collector layer comprises the carbon-based conductive material. The content of the carbon-based conductive material in the current collector layer is greater than 30% by volume and less than 90% by volume.

6. The solid-state battery according to claim 5, wherein, The content of the carbon-based conductive material in the current collector layer is more than 40% by volume and less than 90% by volume.

7. The solid-state battery according to claim 5 or 6, wherein, The carbon-based conductive material contained in the current collector layer is graphite.

8. The solid-state battery according to any one of claims 1 to 4, wherein, Of the positive electrode layer and the negative electrode layer, at least the positive electrode layer is a current collector-less electrode layer that does not have a current collector layer. The content of the carbon-based conductive material in the current collectorless electrode layer is greater than 1% by volume and less than 15% by volume.

9. The solid-state battery according to claim 8, wherein, The content of the carbon-based conductive material in the current collectorless electrode layer is more than 3% by volume and less than 15% by volume.

10. The solid-state battery according to claim 8 or 9, wherein, The carbon-based conductive material contained in the current collectorless electrode layer is VGCF.

11. The solid-state battery according to any one of claims 1 to 10, wherein, At least the positive electrode layer and the positive terminal electrode do not contain Ag, Ni, Cu, Zn, Sn and Al.

Citation Information

Patent Citations

  • All-solid lithium ion secondary battery

    JP2015220107A