Ether-based electrolyte compositions and lithium metal batteries containing them
By using an electrolyte composition containing lithium salt, non-aqueous ether organic solvent, organic antisolvent, SEI forming agent and dissociation inducing additive in lithium metal batteries, a high-concentration lithium salt region is formed, solving the problem of lithium dendrite growth and improving the output characteristics and lifespan of the battery.
Patent Information
- Application Number
- CN202580026863.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-27
- Filing Date
- 2025-06-18
- Publication Date
- 2026-11-10
AI Technical Summary
Dendrite growth in the lithium anode of lithium metal batteries poses safety risks and shortens battery life, while existing methods, such as the solubility limitations of LiNO3 additives and the limitations of low-concentration electrolytes, are also relevant.
An electrolyte composition comprising lithium salt, non-aqueous ether organic solvent, organic antisolvent, SEI forming agent and dissociation inducing additive is used to promote the dissolution of LiNO3 and form a stable SEI layer by forming a high-concentration lithium salt region in the lithium metal battery system, thereby inhibiting dendrite growth.
It improves the output characteristics and lifespan of lithium metal batteries by suppressing side reactions between the lithium metal layer and the electrolyte in high-concentration regions, stabilizing the electrode interface, and extending battery life.
Smart Images

Figure CN123076946A_ABST
Abstract
Description
Technical Field
[0001] Cross-reference to related applications
[0002] This application claims priority and benefit to Korean Patent Application No. 10-2024-0084471, filed on June 27, 2024, the disclosure of which is incorporated herein by reference in its entirety.
[0003] This disclosure relates to ether-based electrolyte compositions and lithium metal batteries containing the same. Background Technology
[0004] Recently, with the rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, and electric vehicles, the demand for small, lightweight, and relatively high-capacity rechargeable batteries has increased rapidly. In particular, lithium-ion batteries have attracted significant attention as power sources for portable devices due to their light weight and high energy density. Therefore, research and development efforts are actively underway to improve the performance of lithium-ion batteries. Specifically, lithium theoretically possesses the highest specific capacity (3860 mAh g / g). -1 With its low energy density and low reduction potential (-3.04 V vs. SHE), it has attracted much attention as a next-generation anode that can exceed the energy density limit of conventional lithium-ion batteries when used as an anode.
[0005] However, lithium anodes tend to deposit dendritic lithium during charge and discharge, which can lead to membrane permeation and the formation of dead lithium, thus acting as a factor threatening battery safety. The main cause of dendrite growth is the unstable organic film that naturally forms at the lithium-electrolyte interface, which is known to accelerate uneven lithium dissolution / deposition.
[0006] Therefore, various methods are being tried to solve the problems of lithium metal batteries, such as forming a protective layer on the surface of the lithium metal layer or developing new electrolytes that can suppress electrolyte decomposition reactions on the lithium metal surface.
[0007] As one of these various methods, the so-called Locally High Concentration Electrolyte (LHCE) has recently been proposed, in which the lithium salt concentration in the electrolyte is increased while an antisolvent with relatively low solubility for lithium salt is added (Chem, Vol. 4, No. 8, August 9, 2018, pp. 1877-1892). This LHCE forms a high-concentration region of lithium salt, thereby improving the output characteristics of lithium metal batteries, while simultaneously allowing the antisolvent to surround the high-concentration region of lithium salt. This is expected to suppress side reactions between the lithium metal layer and the electrolyte and enhance the lifespan of lithium metal batteries.
[0008] Furthermore, previous studies have explored methods to address this issue by forming a solid electrolyte interface (SEI) on the lithium electrode. This SEI, composed of materials such as LiF and Li3N, has been evaluated for its superior physical properties while enhancing lithium-ion mobility. Numerous studies have reported that this method can significantly improve battery life by suppressing dendrite formation.
[0009] On the other hand, LiNO3 (which is known to form a Li3N-based SEI on lithium surfaces) can stabilize the electrode interface and improve battery life when dissolved as an electrolyte additive. However, due to its limited solubility, LiNO3 is currently limited to use in low-concentration ether-based electrolytes. Summary of the Invention
[0010] Technical issues
[0011] Therefore, this disclosure aims to overcome the solubility limit of LiNO3 additives by applying ionic dissociation-inducing additives in lithium metal battery systems. This disclosure also aims to suppress dendrite formation and significantly improve battery life.
[0012] Technical solution
[0013] According to one aspect of this disclosure, an electrolyte composition for lithium metal batteries is provided, the electrolyte composition comprising: an electrolyte containing a lithium salt, a non-aqueous ether-based organic solvent, and an organic antisolvent; an SEI forming agent containing LiNO3; and a dissociation-inducing additive, wherein the dissociation-inducing additive is an ionic additive having a fluorine group represented by Formula 1, and wherein the cation (A) of the dissociation-inducing additive is... n+ NO3 - The binding strength is greater than that of lithium ions (Li). + NO3 - The bonding strength.
[0014] [Formula 1]
[0015] AF n
[0016] Where A includes any one of Cu, Au, Ag, Pt, and Zn.
[0017] In one embodiment, the lithium salt can be dissolved in an electrolyte to have a concentration in the range of 2 to 5 M.
[0018] In one embodiment, the non-aqueous ether-based organic solvent may include one or more solvents selected from dimethoxyethane (DME), 1,2-diethoxyethane (EGDEE), dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, and diethylene glycol dimethyl ether.
[0019] In one embodiment, the organic antisolvent may exhibit at least 10 times lower solubility for the lithium salt than the non-aqueous ether-based organic solvent.
[0020] In one embodiment, the organic antisolvent may comprise one or more of the following groups: 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), ethylene glycol bis(1,1,2,2-tetrafluoroethyl) ether (TFEE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), methoxynonfluorobutane (MOFB), 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE), and ethoxynonfluorobutane (EOFB).
[0021] In one embodiment, the content of the SEI forming agent may be in the range of 0.5 to 1.5% by weight, based on the total weight of the electrolyte composition for lithium metal batteries.
[0022] In one embodiment, the content of the dissociation-inducing additive may be in the range of 0.3 to 1.0% by weight, based on the total weight of the electrolyte composition for lithium metal batteries.
[0023] In one embodiment, the content of the dissociation-inducing additive may be in the range of greater than 0.4% to less than or equal to 0.6% by weight, based on the total weight of the electrolyte composition for lithium metal batteries.
[0024] In one embodiment, based on the total weight of the electrolyte composition for lithium metal batteries, the content of the SEI forming agent can be in the range of 0.5 to 1.5% by weight, and the content of the dissociation inducing additive can be in the range of greater than 0.5% to less than or equal to 1.0% by weight.
[0025] According to another aspect of this disclosure, a lithium metal battery is provided, comprising: the above-described electrolyte composition for a lithium metal battery; a lithium metal electrode; and an SEI layer formed on the lithium metal electrode, wherein the SEI layer comprises LiF and Li3N.
[0026] Beneficial effects
[0027] As described above, the electrolyte composition for lithium metal batteries according to embodiments of this disclosure overcomes the solubility limit of LiNO3 additives by applying ionic dissociation-inducing additives in the lithium metal battery system. Specifically, the addition of specific amounts of SEI forming agent and dissociation-inducing additives promotes the dissolution of dissimilar SEI forming additives in high-concentration salt-ether electrolytes, and the SEI forming agent itself also participates in SEI formation and stabilizes the lithium interface, thereby improving battery life.
[0028] The effects obtainable from this disclosure are not limited to the effects described above, and those skilled in the art will clearly understand from the description of the appended claims other additional effects not mentioned herein. Attached Figure Description
[0029] Figure 1 The comparison shows the cycle life performance (discharge capacity) of lithium metal batteries with or without additives in high-concentration salt ether electrolytes according to Example 1 and Comparative Example 1 of this disclosure.
[0030] Figure 2 The comparison of the cycle life performance (capacity retention vs. initial cycle) of lithium metal batteries in terms of the additive effect of the electrolyte in Examples 1 and Comparative Examples 2-3 of this disclosure is shown. Detailed Implementation
[0031] In the following, specific embodiments of electrolyte compositions for lithium metal batteries, etc., according to this disclosure will be described.
[0032] The terms or words used in this specification and claims should not be construed as limited to their common or dictionary meanings, and this disclosure should be interpreted based on the principle that inventors can appropriately define the concepts of terms to best describe their own inventions, in a meaning and concept consistent with the technical idea of this disclosure.
[0033] The terminology used herein is provided for the description of exemplary embodiments and is not intended to limit the inventive concept. Unless the context clearly indicates otherwise, the singular form includes the plural form.
[0034] It should be understood that the terms “comprising,” “including,” “having,” etc., are used herein to specify the presence of the stated feature, number, step, component, or combination thereof, but do not exclude the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0035] Furthermore, since the dimensions and thicknesses of the elements shown in the accompanying drawings are arbitrarily given for better understanding and ease of description, the inventive concept is not limited to the dimensions and thicknesses shown. In the drawings, the thicknesses of layers, regions, etc., have been enlarged for clarity. In the drawings, the thicknesses of some layers and regions have been enlarged for better understanding and ease of description.
[0036] Furthermore, it should be understood that when a portion such as a layer, membrane, region, or plate is referred to as being "on" or "above" another portion, it can be directly on the other portion, or there may be an intermediate portion. Conversely, when a portion is referred to as being "directly" "on" another portion, it means that there is no other intermediate portion. Additionally, the statement that a particular portion is "above" or "on" a reference portion means that the particular portion is located above or below the reference portion, and does not specifically indicate that the particular portion is "above" or "on" in the opposite direction of gravity.
[0037] Furthermore, throughout the specification, when a section is referred to as "containing" or "containing a certain component," it means that the section may also contain other components, without excluding other components, unless otherwise stated.
[0038] Furthermore, throughout the instruction manual, the term "plane" refers to the view of the target portion from above, while the term "section" refers to the view of the target portion from the side of a vertically cut section.
[0039] Electrolyte composition for lithium metal batteries
[0040] One embodiment of this disclosure provides an electrolyte composition for lithium metal batteries, the electrolyte composition comprising: an electrolyte containing a lithium salt, a non-aqueous ether-based organic solvent, and an organic antisolvent; an SEI forming agent containing LiNO3; and a dissociation-inducing additive, wherein the dissociation-inducing additive is an ionic additive having a fluorine group represented by Formula 1, and wherein the cation (A) of the dissociation-inducing additive is... n+ NO3 - The binding strength is greater than that of lithium ions (Li). + NO3 - The bonding strength.
[0041] [Formula 1]
[0042] AF n
[0043] Where A includes any one of Cu, Au, Ag, Pt, and Zn.
[0044] The electrolyte in this embodiment can belong to the category of locally high concentration electrolytes (LHCE) and can exhibit a high concentration region in which lithium salt dissolves in the organic antisolvent during battery charging and discharging, and a form in which the organic antisolvent is distributed around the high concentration region. Therefore, when using this electrolyte, the output characteristics of the battery can be improved due to the high concentration distribution of lithium salt. Furthermore, depending on the distribution region of the organic antisolvent, side reactions between the lithium metal layer and the electrolyte can be suppressed and the lifespan characteristics of the lithium metal secondary battery can be improved.
[0045] Specifically, the cation (A) of ionic additives with fluorine groups n+ NO3 - The binding strength is greater than that of lithium ions (Li). + NO3 - The binding strength, therefore, when two ionic substances are added together, the cation passes through NO3. - Ion coordination promotes the dissolution of LiNO3.
[0046] Therefore, the significance of the electrolyte composition according to the embodiments of this disclosure is that it can function in a manner independent of electrolyte concentration, thereby breaking away from the existing limitation that it is only applicable to low-concentration ether-based electrolytes.
[0047] The lithium salt contained in the electrolyte serves as a medium for transferring ions within a lithium metal battery. Lithium salts commonly used in electrolytes can be used. For example, the lithium salt may contain Li. + As a cation, and can be selected from F - Cl - ,Br - I - NO3 - N(CN)2 - BF4 - ClO4 - B 10 Cl 10 - AlCl4 - AlO2 - PF6 - CF3SO3 - CH3CO2 - CF3CO2 - AsF6 - SbF6 - CH3SO3 - (CF3CF2SO2)2N - (CF3SO2)2N - (FSO2)2N - BF2C2O4 - BC4O8 - PF4C2O4 - PF2C4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - C4F9SO3 -CF3CF2SO3 - CF3CF2(CF3)2CO - (CF3SO2)2CH - CF3(CF2)7SO3 - and SCN - The anions of the group are included together. For example, lithium salts may contain one or more of the following groups: LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 Lithium salts, including but not limited to LiPF6, LiCF3SO3, LiCF3CO2, LiC4BO8, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, CF3SO3Li, (C2F5SO2)2NLi, (SO2F)2NLi (i.e., LiFSI), (CF3SO2)2NLi (i.e., LiTFSI), (CF3SO2)3CLi, lithium chloroborane, lower aliphatic carboxylic acids having four or fewer carbon atoms, lithium 4-phenylborate, and lithium iminoate, are dissolved in non-aqueous ether solvents and act as lithium-ion sources to enable the basic operation of lithium metal batteries and facilitate the movement of lithium ions between the positive and negative electrodes.
[0048] In another exemplary embodiment, the non-aqueous ether-based organic solvent has high solubility for lithium salts and may contain one or more of, for example, dimethoxyethane (DME), 1,2-diethoxyethane (EGDEE), dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, and diethylene glycol dimethyl ether. On the other hand, carbonate-based solvents, widely used as electrolyte solvents, have higher reduction potentials than non-aqueous ether-based solvents and are therefore more readily reduced at the lithium metal anode. Therefore, it may be advantageous to use non-aqueous ether-based solvents instead of carbonate-based solvents in electrolyte compositions for lithium metal batteries.
[0049] On the other hand, in addition to containing the aforementioned lithium salt and non-aqueous ether-based organic solvent, the electrolyte of the exemplary embodiments may further contain an organic antisolvent that exhibits a solubility for lithium salt that is at least 10 times lower or 10 to 30 times lower than that of the non-aqueous ether-based organic solvent, and therefore is substantially insoluble in lithium salt. Such an organic antisolvent can be defined as a solvent that exhibits substantially no solubility for lithium salt, for example, a solvent that can only dissolve lithium salt at concentrations below 0.1 M, or 0 to 0.1 M, or 0 to 0.05 M. The organic antisolvent may also be an organic solvent that exhibits low solubility for the lithium salt but is miscible with the non-aqueous ether-based organic solvent.
[0050] In an exemplary embodiment, the organic antisolvent may comprise one or more selected from the group consisting of: 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), ethylene glycol bis(1,1,2,2-tetrafluoroethyl) ether (TFEE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), methoxynonfluorobutane (MOFB), 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE), and ethoxynonfluorobutane (EOFB).
[0051] Such organic antisolvents can be selected considering their miscibility with non-aqueous ether organic solvents and their solubility depending on the type and concentration of the lithium salt. For example, if dimethoxyethane (DME) is used as the non-aqueous ether organic solvent, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) can be appropriately used.
[0052] As described above, exemplary embodiments of electrolytes that also include organic antisolvents may include regions in which high local concentrations of lithium salts are present within non-aqueous ether-based organic solvents, and regions in which organic antisolvents are substantially free of lithium salts.
[0053] As described above, the electrolyte according to the exemplary embodiment, which also includes an organic antisolvent, may comprise a region in which a high concentration of lithium salt is locally present in a non-aqueous ether-based organic solvent, and an organic antisolvent distribution region that is substantially free of lithium salt. In this way, since a high concentration of lithium salt is present in a solvated form within the electrolyte, the increase in viscosity and decrease in fluidity of the electrolyte due to the organic antisolvent distribution region can be reduced.
[0054] The amount of organic antisolvent used can be adjusted according to the type of non-aqueous ether organic antisolvent and lithium salt, or the total concentration of lithium salt. For example, the organic antisolvent can be included in the electrolyte in an amount such that the molar ratio of organic antisolvent to non-aqueous ether organic solvent is 1:0.4 to 1:1 or 1:0.4 to 1:0.67.
[0055] In an exemplary embodiment, the lithium salt can be dissolved in the electrolyte to have a concentration in the range of 2 to 5 M. For example, the concentration of the lithium salt can be in the range of 2.5 M or more, 3.0 M or more, 3.5 M or more, or 4.5 M or less, 4.0 M or less, or 3.5 M or less. Unlike conventional electrolyte compositions, the electrolyte composition according to embodiments of this disclosure is able to sufficiently dissolve the SEI forming agent even at high salt concentrations within the above range, thereby stabilizing the electrode interface and improving lifetime.
[0056] In an exemplary embodiment, the content of the SEI forming agent can range from 0.5% to 1.5% by weight, based on the total weight of the electrolyte composition for lithium metal batteries. Excellent battery life improvement can be achieved within this range.
[0057] In an exemplary embodiment, the content of the dissociation-inducing additive can range from 0.3 to 1.0% by weight, based on the total weight of the lithium metal battery electrolyte. Specifically, this content can be 0.4% or more, 0.5% or more, 0.4% or more, less than 0.9% by weight, less than 0.8% by weight, less than 0.7% by weight, or less than 0.6% by weight. For example, the content of the dissociation-inducing additive can range from greater than 0.4% by weight to less than or equal to 0.6% by weight, based on the total weight of the lithium metal battery electrolyte. When the content of the dissociation-inducing additive is within the above range, the solubility of the SEI forming agent can be improved. In particular, when the amount added is insufficient, the effect of improving lifetime characteristics is reduced, and when the amount added is excessive, solubility problems may occur.
[0058] On the other hand, in an exemplary embodiment, the content of the SEI forming agent can be 0.5 to 1.5% by weight, and the content of the dissociation inducing additive can be 0.5 to 1.0% by weight, based on the total weight of the electrolyte composition for lithium metal batteries. In this case, improving the solubility of the SEI forming agent can have an excellent effect on improving battery life, but if the SEI forming agent is contained in excess, it will not dissolve but precipitate.
[0059] Lithium metal batteries
[0060] In another embodiment of this disclosure, a lithium metal battery is provided, comprising: the above-described electrolyte composition for lithium metal batteries; a lithium metal electrode; and an SEI layer formed on the lithium metal electrode, wherein the SEI layer comprises LiF and Li3N.
[0061] In an exemplary embodiment, the lithium metal electrode may be a negative electrode comprising a lithium metal thin film or a lithium metal thin film formed on a negative electrode current collector, and may be structurally no different from conventionally known lithium metal negative electrodes.
[0062] Specifically, the lithium metal anode may consist solely of a copper current collector with a thickness of 1 μm to 20 μm, or may include a lithium metal layer with a thickness of 1 μm to 100 μm (e.g., 1 μm to 50 μm) coated on both sides or one side of the copper current collector.
[0063] In addition, the lithium metal battery according to the exemplary embodiment may further include a positive electrode. In this case, the positive electrode may not be structurally different from positive electrodes of lithium metal batteries generally known in the art. Specifically, the positive electrode may be formed on a positive electrode current collector and include a positive electrode active material layer containing a lithium metal oxide.
[0064] Here, the lithium metal oxide may be those generally known as positive electrode active materials, for example, composite metal oxides such as LiFePO4, LiCoO2, LiMn2O4, LiNiO2, LiNi 1-x Co x O2 (0<x<1), LiMnO2 and the like.
[0065] Alternatively, a lithium metal oxide represented by the following Formula 1 may be used: [Formula 1] Li x MeM1 d O2 wherein, in Formula 1, M1 is Zr, Mg, Al, Ni, Mn, Zn, Fe, Cr, Mo or W, and Me is represented by the following Formula 2: [Formula 2] Ni a Co b Mn c wherein, in Formula 2, 0.97≤x≤1.03, 0.50≤a≤0.90, 0<b≤0.3, 0<c≤0.3, 0≤d<0.01, and a+b+c+d=1.
[0066] The lithium metal oxide represented by Formula 1 is a positive electrode active material known as so-called NCM, and has a layered crystal structure, which may have a higher energy density than the composite metal oxides listed above such as LiCoO2, LiMn2O4, LiNiO2, LiNi 1- x Co x O2 (0<x<1) and LiMnO2.
[0067] More specifically, as "a" in Formula 2 has a higher value within the above range, it may contribute to improving the output of the battery, but the exemplary embodiments are not limited thereto.
[0068] Regardless of the composition of the lithium metal oxide, lithium metal oxides with a coating on their surface can be used, or mixtures of lithium metal oxides and coating compounds can be used. The coating may contain coating element compounds, such as coating element oxides, coating element hydroxides, coating element hydroxy oxides, coating element oxycarbonates, or coating element hydroxycarbonates. The compounds constituting the coating can be amorphous or crystalline. The coating elements included in the coating may include Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or mixtures thereof. The coating formation process can be carried out by any coating method (e.g., spraying, dipping, etc.) as long as the coating method does not adversely affect the physical properties of the positive electrode active material by using these elements in the compound. This is something that those skilled in the art will readily understand, and therefore, a detailed description will be omitted.
[0069] The positive electrode active material layer of the exemplary embodiment may further include an irreversible compensation additive. This irreversible compensation additive desorbs lithium ions during the initial charging of the lithium metal battery to supply lithium ions to the monolayer of the negative electrode current collector, and the irreversible compensation additive in which lithium ions have been desorbed can be converted to an irreversible state, thus preventing the resorption of lithium ions. Here, the irreversible compensation additive may be one or more selected from the group consisting of Li2NiO2, Li2CuO2, Li6CoO4, Li5FeO4, Li6MnO4, Li2MoO3, Li3N, Li2O, LiOH, and Li2CO3, which are commonly known in the art. Based on the total weight of the positive electrode active material, the content of the irreversible compensation additive may be from 1% to 50% by weight, but this disclosure is not limited thereto.
[0070] The positive electrode active material layer in the exemplary embodiment may also include an adhesive and optional conductive materials, fillers, etc.
[0071] There are no particular limitations on the conductive material, as long as it is conductive and will not cause chemical changes in the battery. Examples of conductive materials include graphite, such as natural or artificial graphite; carbon blacks, such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal cracking black; conductive fibers, such as carbon fibers and metal fibers; metal powders, such as fluorinated carbon, aluminum, and nickel powder; conductive whiskers, such as zinc oxide and potassium titanate; conductive metal oxides, such as titanium oxide; or conductive polymers, such as polyphenylene derivatives.
[0072] The adhesive is used to adhere the positive electrode active material particles well to each other and to adhere the positive electrode active material well to the current collector, and representative examples may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited thereto.
[0073] The lithium metal battery according to an exemplary embodiment may also include a separator formed between the negative electrode and the positive electrode.
[0074] For example, the electrolyte composition for lithium metal batteries described above can be impregnated into a separator, which could mean that the electrolyte is located in the pores within the separator.
[0075] In an exemplary embodiment, the electrolyte composition may be in the form of a porous separator impregnated between the negative and positive electrodes. Here, the separator separates the negative and positive electrodes and provides a path for the movement of lithium ions. Any separator can be used without particular limitation, as long as it is a separator commonly used in lithium batteries. That is, a separator with excellent electrolyte retention and low resistance to the movement of ions in the electrolyte can be used. For example, the separator may be selected from glass fiber, polyester, Teflon (tetrafluoroethylene), polyethylene, polypropylene, polytetrafluoroethylene (PTFE), or combinations thereof, and may be of nonwoven or woven type. For example, for lithium-ion batteries, polyolefin polymer separators (such as polyethylene, polypropylene, etc.) are primarily used, and coated separators containing ceramic components or polymer materials can be used to ensure heat resistance or mechanical strength, and may be selectively used in single-layer or multi-layer structures.
[0076] In an exemplary embodiment, a solid electrolyte interphase (SEI) layer can be formed on the lithium metal electrode. The SEI layer can be formed by a reaction that occurs on the surface of the negative electrode active material during the initial charging process of the solid electrolyte battery, thereby preventing the degradation of the negative electrode and improving battery life.
[0077] Specifically, the solid electrolyte interface layer can have a thickness ranging from 10 nm to 1 μm. The thickness of this solid electrolyte interface layer can vary depending on the content of the SEI forming agent and dissociation-inducing additive in the electrolyte composition for lithium metal batteries. When the electrolyte composition according to an embodiment of the present invention is applied, the solid electrolyte interface layer can be formed on the lithium metal electrode to an optimal thickness, for example, in the range of 10 to 30 nm or 15 to 25 nm, thereby achieving excellent battery life characteristics.
[0078] In an exemplary embodiment, the SEI layer may comprise LiF and Li3N. Specifically, the dissociation-inducing additive anion (F... - It can dissociate and react with the lithium anode to form a LiN and Li3F-rich SEI layer. The SEI layer contains LiF and Li3N components, thus exhibiting superior mechanical properties and maintaining uniformity compared to existing natural SEIs. It also induces uniform lithium deposition and is chemically stable, thereby reducing the reduction of byproducts in the reduction voltage range (<3.0), thus protecting the lithium anode.
[0079] Example
[0080] Embodiments of this disclosure will be described in detail below to enable them to be readily practiced by those skilled in the art. However, this disclosure may be implemented in various different forms and is not limited to the embodiments provided herein.
[0081] Comparative Example 1
[0082] A high-concentration lithium salt ether electrolyte was prepared such that the molar ratio of LiFSI:DME:TTE was 1 mol:2.4 mol:2.4 mol. Specifically, the LiFSI salt was dissolved in DME / TTE solvent at a concentration of 4.62 M.
[0083] Comparative Example 2
[0084] LiPF6 was dissolved at a concentration of 1M in a 1:1 (v:v) EC:DEC solvent mixture. 1 wt% VC and 10 wt% FEC were added as additives, along with 1 wt% LiNO3 as an SEI forming agent and 0.2 wt% CuF2 as a dissociation inducing additive. The mixture was then thoroughly stirred to prepare the electrolyte composition.
[0085] Comparative Example 3
[0086] 1% by weight of LiNO3 as an SEI forming agent and 0.2% by weight of CuF2 as a dissociation inducing additive were added to the ether electrolyte of Comparative Example 1, and the mixture was stirred thoroughly to prepare an electrolyte composition.
[0087] Example 1
[0088] The electrolyte composition was prepared in the same manner as in Comparative Example 1, except that 1% by weight of LiNO3 as an SEI forming agent and 0.5% by weight of CuF2 as a dissociation inducing additive were added.
[0089] Experimental Example 1: Battery Life Characteristics
[0090] 1) Coin cell (2032 type) were fabricated using the electrolyte compositions of Comparative Example 1 and Example 1, and charge / discharge tests were performed. Specifically, the LFP (source: LG New Energy) as the working electrode and a 45 μm thick lithium electrode as the counter electrode were positioned so that they faced each other. A polyethylene (PE) separator was inserted between the two electrodes, and then 60 μL of the electrolyte compositions of Comparative Example 1 and Example 1 were injected into each electrode and sealed to fabricate respective 2032 coin-type LFP|Li full cell samples. For the fabricated cells, the first two cycles were pre-activated at 0.1 C / 0.1 C conditions, followed by repeated 0.5 C charge and 0.5 C discharge cycles, and the discharge capacity over time (cycles) was measured. The results are shown in... Figure 1 middle.
[0091] refer to Figure 1 It can be confirmed that, in the case of a high concentration of lithium salt ether electrolyte, Example 1, with the addition of an SEI forming agent (LiNO3) and a dissociation inducing additive (CuF2), shows the formation of a stable SEI composed of LiF and Li3N components that is beneficial to the lithium anode, thereby reducing side reactions with the electrolyte and suppressing dendritic lithium deposition, resulting in excellent cycle life characteristics.
[0092] 2) Additionally, when an SEI forming agent (LiNO3) and a dissociation-inducing additive (CuF2) were added, capacity retention was measured under the same charge / discharge cycle conditions based on salt concentration and dosage. The results are shown in... Figure 2 middle.
[0093] refer to Figure 2 In Comparative Example 2, the low-concentration lithium salt carbonate electrolyte, using the solvent and additive composition (1.0 wt% LiNO3, 0.2 wt% CuF2) under previously studied conditions, exhibited a sharp decrease in capacity retention within 100 cycles. It was also confirmed that even in Comparative Example 3, where the same additive composition was applied to a high-concentration lithium salt ether electrolyte, capacity retention decreased within 300 cycles. On the other hand, Example 1, with a high-concentration lithium salt ether electrolyte containing 0.5 wt% dissociation-inducing additive, demonstrated an improvement in capacity retention of over 70% and single-cell life within approximately 400 cycles.
[0094] Although preferred embodiments of the present disclosure have been shown and described above, the scope of the present disclosure is not limited thereto, and those skilled in the art can make many other variations and modifications to the embodiments using the basic principles of the invention as defined in the appended claims, which also fall within the spirit and scope of the invention.
Claims
1. An electrolyte composition for lithium metal batteries, comprising: Electrolytes containing lithium salts, non-aqueous ether-based organic solvents, and organic antisolvents; SEI forming agents containing LiNO3; and Dissociation-inducing additives The dissociation-inducing additive is an ionic additive having a fluorine group, represented by Formula 1, and the cation (A) of the dissociation-inducing additive is... n+ NO3 - The binding strength is greater than that of lithium ions (Li). + NO3 - The bonding strength, [Formula 1] OF n in, A includes any one of Cu, Au, Ag, Pt, and Zn.
2. The electrolyte composition for lithium metal batteries according to claim 1, The lithium salt is dissolved in the electrolyte to have a concentration in the range of 2 to 5 M.
3. The electrolyte composition for lithium metal batteries according to claim 1, The ether-based organic solvent comprises one or more solvents selected from dimethoxyethane (DME), 1,2-diethoxyethane (EGDEE), dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, and diethylene glycol dimethyl ether.
4. The electrolyte composition for lithium metal batteries according to claim 1, The organic antisolvent exhibits at least 10 times lower solubility for the lithium salt than the non-aqueous organic solvent.
5. The electrolyte composition for lithium metal batteries according to claim 1, The organic antisolvent comprises one or more selected from the group consisting of: 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), ethylene glycol bis(1,1,2,2-tetrafluoroethyl) ether (TFEE), bis(2,2,2-trifluoroethyl) ether (BTFE), 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (TFTFE), methoxynonfluorobutane (MOFB), 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (OTE), and ethoxynonfluorobutane (EOFB).
6. The electrolyte composition for lithium metal batteries according to claim 1, The content of the SEI forming agent is in the range of 0.5 to 1.5% by weight, based on the total weight of the electrolyte for lithium secondary batteries.
7. The electrolyte composition for lithium metal batteries according to claim 1, The content of the dissociation-inducing additive is in the range of 0.3 to 1.0% by weight, based on the total weight of the electrolyte for lithium secondary batteries.
8. The electrolyte composition for lithium metal batteries according to claim 1, The content of the dissociation-inducing additive is in the range of greater than 0.4% to less than or equal to 0.6% by weight, based on the total weight of the electrolyte for lithium secondary batteries.
9. The electrolyte composition for lithium metal batteries according to claim 1, Based on the total weight of the electrolyte for lithium secondary batteries, the content of the SEI forming agent is in the range of 0.5 to 1.5% by weight, and the content of the dissociation inducing additive is in the range of greater than 0.5% to less than or equal to 1.0% by weight.
10. A lithium metal battery, comprising: The electrolyte composition for lithium metal batteries according to any one of claims 1 to 9; Lithium metal electrode; and The SEI layer formed on the lithium metal electrode, The SEI layer contains LiF and Li3N.
Citation Information
Patent Citations
Method and Apparatus for Video Encoding and Decoding Using Geometric Partitioning Mode