Diaphragms for Electrochemical Devices and Their Manufacturing Methods
By dry-manufacturing porous polymer matrix separators and employing uniaxial stretching and inorganic particle coating to optimize the pore structure, the shortcomings of lithium secondary battery separators in high output performance are solved, achieving reduced resistance and improved output performance.
Patent Information
- Application Number
- CN202580026939.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-10-11
- Filing Date
- 2025-09-26
- Publication Date
- 2026-11-10
AI Technical Summary
Existing lithium-ion battery separators have shortcomings in terms of high output performance, especially in hybrid electric vehicles. Current wet manufacturing methods use harmful solvents and are difficult to operate. Dry-manufactured porous substrates have advantages in battery output performance, but the pore structure design needs further optimization.
A porous polymer matrix membrane is manufactured using a dry process. Through a uniaxial stretching process of polyolefin resin, a pore structure with microfibers in non-parallel directions of the main chain is formed, ensuring that the pore volume ratio with a pore size greater than 100 nm is more than 3%. An inorganic particle and adhesive polymer coating is then applied to the surface to optimize the aspect ratio and air permeability of the pores.
Significantly reduces resistance, improves the output performance and mechanical strength of electrochemical devices, and achieves high output characteristics and safety.
Smart Images

Figure CN123076969A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a diaphragm, a method for manufacturing the diaphragm, and an electrochemical device comprising the diaphragm. More specifically, this invention relates to a diaphragm manufactured by a dry process.
[0002] This application is based on and claims priority to Korean Patent Application No. 2024-0138628, filed with the Korean Intellectual Property Office on October 11, 2024, the disclosure of which is incorporated herein by reference in its entirety. Background Technology
[0003] Lithium-ion batteries are widely used as power sources for mobile electronic devices, including laptops, mobile phones, digital cameras, and camcorders. Recently, lithium-ion batteries have seen widespread adoption, including in vehicles, due to their high energy density.
[0004] Lithium-ion batteries are manufactured by placing an electrode assembly, including a positive electrode, a separator, and a negative electrode, into a battery casing, injecting electrolyte, and sealing the casing. Separators for lithium-ion batteries typically comprise a polyolefin-based porous substrate.
[0005] On the other hand, methods for manufacturing porous substrates mainly employ wet and dry processes. The wet process involves mixing polymer materials with plasticizers, extruding the mixture to form sheets, and removing the plasticizer from the sheets to form pores. In the wet process, the pore size is determined by the type of plasticizer and its compatibility with the polymer material, thus offering the advantage of uniform pore size. However, this process becomes difficult to operate when the polymer material changes, and the solvents used to extract the plasticizer are harmful to humans and the environment.
[0006] The dry process involves manufacturing a precursor polymer film through extrusion and then stretching the polymer film with controlled fiber orientation via heat treatment to tear the fibers and create pores. Unlike the wet process, the dry process does not use extraction solvents used for plasticizer extraction, thus offering the advantage of being environmentally friendly.
[0007] On the other hand, high output performance is important for lithium-ion batteries used in hybrid electric vehicles (HEVs) to assist engine power in a low-efficiency range. Due to material and process characteristics, dry-processed separators using porous substrates have a more favorable impact on battery output performance compared to wet-processed separators. Therefore, there is a need to develop dry-processed separators with high output performance suitable for electrochemical devices. Summary of the Invention
[0008] Technical issues
[0009] The present invention aims to provide a diaphragm for achieving high output performance when used in an electrochemical device and a method thereof.
[0010] Specifically, the present invention aims to provide a separator substrate for reducing the resistance of a separator to reduce the resistance of an electrochemical device (e.g., a lithium secondary battery), a method for manufacturing the same, a separator using the same, and an electrochemical device comprising the same.
[0011] Technical solution
[0012] To achieve the above objectives, according to one aspect of the present invention, a diaphragm with the following embodiments is provided.
[0013] The diaphragm according to the first embodiment includes: A porous polymer matrix containing polyolefin resins. The porous polymer matrix comprises: Polyolefin resin backbone, Microfibers extending in a direction not parallel to the extension direction of the main chain, and Pores exist between the microfibers. Based on the total volume of the pores, the volume of pores with a diameter of 100 nm or more accounts for more than 3%.
[0014] According to the second embodiment, in the first embodiment... The polyolefin resin may include polypropylene resin, and Based on the total weight of the porous polymer matrix, the weight of the polypropylene resin can be 95% or more.
[0015] According to the third embodiment, in the first or second embodiment... The cross-section of the hole can contain an elliptical shape with an aspect ratio greater than 1, and the aspect ratio is defined by the following formula 1: Formula 1 Aspect ratio = [(length in the extension direction of the microfiber (a)) / (length in the extension direction of the main chain (b))]).
[0016] According to the fourth embodiment, in any one of the first to third embodiments, Based on the total volume of the pores, the volume of pores with a diameter of 100 nm or more can be 4% to 10%.
[0017] According to the fifth embodiment, in any one of the first to fourth embodiments, The maximum water pressure difference (ΔP) of the porous polymer matrix can be above 1,550 psi.
[0018] The maximum water pressure difference can represent the difference between the highest and lowest water pressures in the water pressure-water saturation diagram, which is obtained by injecting water into a porous polymer matrix at a constant rate to achieve 100% volume water saturation.
[0019] According to the sixth embodiment, in any one of the first to fifth embodiments, The maximum water pressure differential of the porous polymer matrix can be above 1,600 psi.
[0020] According to the seventh embodiment, in any one of the first to sixth embodiments... The flow rate of the porous polymer matrix can be above 150, and the flow rate is defined by the following formula 2: Formula 2 u=κΔPL u represents the permeability coefficient of the porous polymer matrix. κ is the Gurley permeability of the porous polymer matrix. ΔP represents the maximum water pressure difference in the porous polymer matrix, and L is the thickness of the porous polymer matrix.
[0021] According to the eighth embodiment, in any one of the first to seventh embodiments, The thickness of the porous polymer matrix can be from 5 μm to 14 μm.
[0022] According to the ninth embodiment, in any one of the first to eighth embodiments, The membrane may further comprise a porous coating present on at least one surface of the porous polymer matrix, and The porous coating may contain inorganic particles and binder polymers.
[0023] According to another aspect of the present invention, an electrochemical device according to the following embodiments is provided.
[0024] The electrochemical device according to the tenth embodiment may include: The diaphragm according to any one of the first to ninth embodiments, The first electrode and the second electrode are respectively located on the two surfaces of the diaphragm. Electrolytes, and A housing that contains the diaphragm, the first electrode, the second electrode, and the electrolyte.
[0025] According to another aspect of the present invention, a method for manufacturing a diaphragm is provided according to the following embodiments.
[0026] The method for manufacturing a diaphragm according to the eleventh embodiment may include: The process used to obtain a porous polymer matrix, The process for obtaining a porous polymer matrix may include the following steps: (S1) A polyolefin resin is fed into an extruder to obtain an extrudate; (S2) The extrudate is thermoformed to obtain a polymer sheet; (S3) The polymer sheet is subjected to low-temperature stretching, followed by high-temperature stretching; and (S4) The stretched sheet is heat-treated. In step (S3), both the low-temperature stretching and the high-temperature stretching are uniaxial stretching processes, and they are performed in parallel directions. The low-temperature stretching is performed with a stretching ratio of less than 50%, compared to the high-temperature stretching ratio. The stretch ratio is the ratio of the length of the polymer sheet after stretching to the length of the polymer sheet before stretching.
[0027] According to the twelfth embodiment, in the eleventh embodiment... The low-temperature stretching ratio can be below 1.05 times.
[0028] According to the thirteenth embodiment, in the eleventh or twelfth embodiment, The high-temperature stretching ratio can be more than 2 times.
[0029] According to the fourteenth embodiment, in any one of the eleventh to thirteenth embodiments, The thermoforming and the heat treatment can be performed at different temperatures.
[0030] According to the fifteenth embodiment, in any one of the eleventh to fourteenth embodiments, The low-temperature stretching can be performed at a temperature lower than the thermoforming temperature. The high-temperature stretching can be performed at a temperature equal to or higher than the thermoforming temperature, and The heat treatment can be performed at a higher temperature than high-temperature stretching.
[0031] According to the sixteenth embodiment, in any one of the eleventh to fifteenth embodiments, The process for obtaining a porous polymer matrix may be a process that does not use at least one of a diluent and a plasticizer.
[0032] According to the seventeenth embodiment, in any one of the eleventh to sixteenth embodiments, The method of manufacturing the diaphragm may further include the step of forming a porous coating on at least one surface of a porous polymer matrix, the porous coating comprising inorganic particles and a binder polymer.
[0033] Beneficial effects
[0034] According to one embodiment of the invention, the diaphragm can reduce resistance by changing the pore characteristics on the surface of a porous polymer matrix, thereby significantly improving the output performance of the electrochemical device using it.
[0035] Therefore, electrochemical devices using diaphragms can have reduced resistance and excellent high output characteristics. Attached Figure Description
[0036] Figure 1 This is a diagram illustrating the structure of a porous polymer matrix according to an embodiment of the present invention.
[0037] Figure 2 This is a diagram illustrating the pore shape in a porous polymer matrix according to an embodiment of the present invention. Detailed Implementation
[0038] The present invention will be described in detail below.
[0039] Unless the context clearly indicates otherwise, the term "comprising" as used in this specification specifies the presence of the stated element, but does not exclude the presence or addition of one or more other elements.
[0040] In this specification, "A and / or B" means A or B, or both.
[0041] Some of the terminology used herein is provided for convenience and is not intended to limit the invention. Furthermore, terms such as “upper,” “lower,” “left,” “right,” “front,” “rear,” “inner,” and “outer” respectively indicate directions in the drawings, or directions toward or away from the geometric center of the device, system, or its components.
[0042] This invention relates to a diaphragm for an electrochemical device, a method for manufacturing the diaphragm thereto, and an electrochemical device comprising the diaphragm.
[0043] In this invention, an electrochemical device refers to a device that converts chemical energy into electrical energy through an electrochemical reaction, and includes both primary and secondary batteries. Secondary batteries are capable of being charged and discharged, and include lithium-ion batteries, nickel-cadmium batteries, or nickel-metal hydride batteries.
[0044] The diaphragm for an electrochemical device according to one aspect of the present invention will now be described in detail.
[0045] diaphragm
[0046] The diaphragm according to one aspect of the invention contains a porous polymer matrix comprising a polyolefin resin.
[0047] In one embodiment of the present invention, the polyolefin resin may include, but is not limited to, any polyolefin resin used as a raw material for a diaphragm in an electrochemical device. For example, the polyolefin resin may include, but is not limited to, polyethylene resin, polypropylene resin, polyethylene-polypropylene copolymer resin, or mixtures thereof.
[0048] According to one embodiment of the present invention, the polyolefin resin may comprise polypropylene resin in terms of the mechanical strength of the porous polymer matrix.
[0049] In one embodiment of the present invention, when the porous polymer matrix contains polypropylene resin as a polyolefin resin, the content of polypropylene resin can be 50% by weight or more based on the total weight of the porous polymer matrix. Specifically, the weight of polypropylene resin can be 70% by weight or more, 80% by weight or more, 90% by weight or more, or 95% by weight or more based on the total weight of the porous polymer matrix. For example, the weight of polypropylene resin can be 98% by weight or more, 99% by weight or more, 99.9% by weight or more, or 100% by weight based on the total weight of the porous polymer matrix.
[0050] In one embodiment of the present invention, the porous polymer matrix may contain only polypropylene resin as a polyolefin resin, but the present invention is not limited thereto.
[0051] In this specification, the weight of polypropylene resin in the porous polymer matrix can be measured by known methods for measuring the weight of polymer materials, and such methods are not limited to any particular method. For example, the weight percentage of polypropylene resin contained in the porous polymer matrix can be measured by measuring the change in mass of the sample during heating using a known thermogravimetric analyzer (TGA), but the invention is not limited thereto. The TGA analysis method can be performed, for example, using a SINCO TGA N-1000 (SINCO) at a heating rate of 0.01 °C / min to 300 °C / min in the range of 20 °C to 950 °C, using nitrogen or air as a purge gas, but the invention is not limited thereto.
[0052] In one embodiment of the present invention, a porous polymer matrix can be manufactured by using a dry process with a polyolefin resin.
[0053] Therefore, a porous polymer matrix can have a structure comprising a polyolefin resin backbone, microfibers extending in a direction not parallel to the extension direction of the backbone, and pores existing between the microfibers.
[0054] Figure 1 This is a diagram illustrating the structure of a porous polymer matrix according to an embodiment of the present invention. (Reference) Figure 1The porous polymer matrix 200 has a structure comprising a main chain 201 of polyolefin resin, microfibers 202 extending in a direction not parallel to the extension direction of the main chain, and pores 203 present between the microfibers.
[0055] According to one embodiment of the invention, in the manufacture of a porous polymer matrix, during the stretching of a polyolefin sheet, microfibers may extend in a direction from which the polyolefin backbone is stretched, resulting in pores between the microfibers in the structure, but the invention is not limited thereto.
[0056] According to one embodiment of the invention, the direction that is not parallel to the extension direction of the main chain (i.e., the extension direction of the microfibers) can preferably be parallel to the stretching direction in the fabrication of the porous polymer matrix.
[0057] For example, during the fabrication of a porous polymer matrix, when the polymer sheet is uniaxially stretched in the longitudinal direction (MD), the extension direction of the microfibers can preferably be parallel to the MD direction.
[0058] In this specification, "longitudinal" refers to the direction parallel to the direction of operation of the manufacturing process of the porous polymer matrix. The longitudinal direction can be identified by the orientation of the polymer fibers. For example, when the porous polymer matrix is uniaxially stretched in the longitudinal direction, the microfibers may extend in a direction parallel to the longitudinal direction, and when the porous polymer matrix is uniaxially stretched in the transverse (TD) direction, the microfibers may extend in a direction parallel to the TD direction perpendicular to the longitudinal direction. The orientation of the polymer fibers can be identified by observing the surface of the porous polymer matrix using an optical microscope (e.g., SEM), but the measurement method is not limited to this.
[0059] According to one embodiment of the invention, in terms of mechanical strength, the porous polymer matrix can preferably be manufactured by uniaxial stretching, so that the cross-sectional shape of the pores between the microfibers can be an elliptical shape elongated in the stretching direction.
[0060] For example, the cross-section of the pores between microfibers can contain an elliptical shape with an aspect ratio greater than 1 according to Equation 1 below.
[0061] Formula 1
[0062] Aspect ratio = [(Length of microfiber in the extension direction (a)) / (Length of main chain in the extension direction (b))]
[0063] Figure 2 This is a diagram illustrating the shape of the hole 203 according to one embodiment of the present invention. Figure 2 The diagram shows the extension direction of the microfiber (a) and the extension direction of the main chain (b), and the pores may have an elliptical shape with an aspect ratio greater than 1, for example 3 to 100, 5 to 50, 5 to 30 or 10 to 20, but the invention is not limited thereto.
[0064] In this specification, the aspect ratio of the pores between microfibers can be measured using SEM images of the surface of the diaphragm or porous polymer matrix, but the measurement method is not limited to this.
[0065] As described above, according to one embodiment of the present invention, a porous polymer matrix may have the following structure, comprising: a polyolefin resin backbone, microfibers extending in a direction not parallel to the extension direction of the backbone, and pores present between the microfibers, wherein the cross-section of the pores may have an elliptical shape with an aspect ratio greater than 1 according to Formula 1 above.
[0066] In this case, according to one aspect of the invention, the porous polymer matrix is characterized in that the volume of pores with a diameter of 100 nm or more is more than 3% of the total pore volume.
[0067] According to one embodiment of the invention, the porous polymer matrix contains a plurality of pores, and in this case, when the pore size is extremely small, lithium-ion and electron transport decreases, resulting in an increase in the battery's resistance. Furthermore, the separator according to one embodiment of the invention may have a porous coating on at least one surface of the porous polymer matrix, the porous coating comprising inorganic particles and a binder polymer, and in this case, when the pore size of the porous polymer matrix is extremely small, the inorganic particles and / or the binder polymer may block the pores in the porous polymer matrix, resulting in a higher resistance value for the separator and battery using it, and consequently, poorer battery output performance.
[0068] Therefore, according to one embodiment of the present invention, in order to solve the above-mentioned problems, a porous polymer matrix containing a sufficient number of pores with a pore size of 100 nm or more is used.
[0069] In this specification, based on pore size, pores present on / on a surface of a porous polymer matrix can be classified, for example, as macropores with a diameter of 100 nm or more and micropores with a diameter of less than 100 nm.
[0070] In this specification, the volume ratio of macropores and / or micropores on a surface of a porous polymer substrate can be measured using an Aquapore water immersion porosimeter (Poretech Instrument, WMI-5K). Specifically, the measurement method evaluates the total volume of pores with a diameter greater than 100 nm using a water saturation-pressure map, which is obtained by injecting water into the porous polymer matrix at a constant rate to achieve 100% water saturation by volume.
[0071] In one embodiment of the present invention, the volume of pores with a diameter of 100 nm or more in the porous polymer matrix is 3% or more of the total pore volume. For example, the volume of pores with a diameter of 100 nm or more in the porous polymer matrix can be 3% or more of the total pore volume, specifically 3% to 15%, 3.5% to 12%, 4% to 10%, 4% to 8%, 4% to 6%, 4% to 5%, or 4.5% to 5%. When the macropore volume in the porous polymer matrix falls within the above range, the resistance of the diaphragm and the electrochemical device using it can be reduced, and therefore, it may have a beneficial effect on high output performance, but the present invention is not limited thereto.
[0072] In one embodiment of the present invention, when the number of macropores in the porous polymer matrix is too large or the diameter of the macropores is extremely large, the insulation properties of the membrane may decrease. Therefore, the diameter of the macropores and micropores in the porous polymer matrix can be further controlled.
[0073] For example, when a water pressure-water saturation diagram is obtained by injecting water into a porous polymer matrix at a constant rate to achieve 100% volume water saturation, the lowest water pressure in the diagram indicates that water fills the largest pores, and the highest water pressure indicates that water fills the smallest pores. Therefore, according to one embodiment of the invention, the maximum water pressure difference (ΔP) of the porous polymer matrix can be 1,550 psi or higher. In this case, the maximum water pressure difference represents the difference between the highest and lowest water pressures in the water pressure-water saturation diagram.
[0074] In one embodiment of the invention, the maximum water pressure differential (ΔP) of the porous polymer matrix can be 1,550 psi or higher, for example, 1,600 psi or higher. Specifically, the maximum water pressure differential (ΔP) of the porous polymer matrix can be 1,550 psi to 2,000 psi, 1,550 psi to 1,800 psi, 1,600 psi to 1,700 psi, 1,600 psi to 1,650 psi, or 1,620 psi to 1,650 psi, but the invention is not limited thereto.
[0075] According to one embodiment of the present invention, the permeability coefficient per unit area of a porous polymer matrix can be measured according to the following formula 2.
[0076] Formula 2
[0077] u=κΔPL
[0078] u represents the permeability coefficient of the porous polymer matrix. κ is the gravimetric permeability of the porous polymer matrix. ΔP represents the maximum water pressure difference in the porous polymer matrix, and L is the thickness of the porous polymer matrix.
[0079] Regarding Equation 2, according to one embodiment of the invention, the Gryllium permeability of the porous polymer matrix can be calculated as the reciprocal of the Gryllium value of the diaphragm measured by conventional methods (1 / Gryllium, cc / s). For example, the Gryllium value of the porous polymer matrix can be measured by using a Gryllium permeability meter according to ASTM D726-94, measuring the time (sec) required for 100 cc of air at a pressure of 12.2 inches of H2O to pass through a 1 square inch diaphragm substrate.
[0080] According to one embodiment of the invention, the thickness of the porous polymer matrix can be measured using methods commonly used to measure membrane thickness. For example, the thickness of the porous polymer matrix can be measured using a Mitutoyo thickness gauge.
[0081] According to one embodiment of the present invention, based on Formula 2 above, the porous polymer matrix can exhibit a per unit area (1 cm²) 2 Transmittance coefficient is 150cm 3 ·psi·μm / sec or higher, for example, 150 to 300cm 3 ·psi·μm / sec, 155 to 200cm 3 ·psi·μm / sec, 160 to 180cm 3 •psi·μm / sec, 165 to 170cm 3 •psi·μm / sec, or 166 to 170cm 3 •psi·μm / sec, but the present invention is not limited thereto.
[0082] In one embodiment of the invention, the porous polymer matrix may have a thickness of, for example, 5 μm to 14 μm. Specifically, the thickness of the porous polymer matrix may be, for example, 8 μm to 14 μm, 8 μm to 12 μm, 10 μm to 12 μm, or 11 μm to 12 μm, but the thickness is not limited thereto.
[0083] According to one embodiment of the invention, the membrane may contain only a porous polymer matrix, without a coating containing inorganic particles and binder polymers. In other words, the membrane may contain only a porous polymer matrix.
[0084] According to another embodiment of the invention, the diaphragm may also include a porous coating on at least one surface of a porous polymer matrix, the porous coating comprising inorganic particles and / or binder polymers.
[0085] According to another embodiment of the invention, the diaphragm may comprise a porous polymer matrix and an adhesive adhesion layer.
[0086] According to another embodiment of the invention, the diaphragm may comprise a porous polymer matrix, a porous coating (comprising inorganic particles and / or a binder) on at least one surface of the porous polymer matrix, and an adhesive adhesion layer (comprising an adhesive) on one surface of the porous coating. Here, one surface of the porous coating refers to the contact surface between the diaphragm and the electrode when the diaphragm is attached to the electrode.
[0087] In one embodiment of the invention, the diaphragm may comprise a porous polymer matrix, a porous coating (containing inorganic particles) on at least one surface of the porous polymer matrix, and an adhesive adhesion layer (containing an adhesive) on one surface of the porous coating. Here, one surface of the porous coating refers to the contact surface between the diaphragm and the electrode when the diaphragm is attached to the electrode.
[0088] In one embodiment of the invention, the porous coating may comprise a large number of inorganic particles and a binder polymer for holding the inorganic particles together, thereby enhancing the safety of the membrane. The inorganic particles can improve the heat resistance of the membrane, and the binder polymer can impart adhesive strength to the membrane surface.
[0089] In this case, when the porous polymer matrix with the porous coating is made of polymer fibers that do not contain macropores of the above-mentioned size, or is made of polymer fibers that are very tightly packed together with a low percentage of total macropore volume, the resistance of the diaphragm may increase, and the porous polymer matrix may be filled with a smaller amount of porous coating forming slurry, resulting in low adhesion strength at the interface between the porous polymer matrix and the porous coating, but the invention is not limited thereto.
[0090] In the following text, for illustrative purposes, the construction of porous coatings will be described. However, the construction of porous coatings is not limited to this.
[0091] In one embodiment of the invention, the porous coating may comprise inorganic particles and / or a binder polymer, and the inorganic particles may be coated with the binder polymer on all or at least a portion of the surface. In this case, the inorganic particles are held together face-to-face and / or point-to-point by the binder polymer as a medium.
[0092] For example, inorganic particles and binder resin can be included in a porous coating in a weight ratio of 95:5 to 70:30. The porous coating has the structural characteristics of a porous layer with multiple pores inside, wherein the pores are interconnected to allow gas or liquid to pass through from one side to the other.
[0093] In one embodiment of the invention, the porous coating may be formed by a safety-reinforced diaphragm (SRS) manufacturing method, a ceramic-coated diaphragm (CCS) manufacturing method, or any other known manufacturing method, but the invention is not limited thereto.
[0094] In one embodiment of the invention, the porous coating may have a multilayer structure comprising a first layer containing inorganic particles and located near a porous polymer matrix, and a second layer containing an adhesive polymer and located on the first layer, but the invention is not limited thereto.
[0095] In one embodiment of the invention, the inorganic particles are not limited to specific particles and may include any electrochemically stable particles. That is, the inorganic particles used in the present invention are not limited to specific types and may include any type of inorganic particles that do not drive oxidation and / or reduction reactions within the operating voltage range of the applied electrochemical device (e.g., 0 to 5 V relative to Li / Li+). Non-limiting examples of inorganic particles may include: BaTiO3, Pb(Zr,Ti)O3(PZT), Pb... 1-x La x Zr 1-y Ti y O3(PLZT, 0) <x<1,0<y<1)、Pb(Mg 1 / 3 Nb 2 / 3 At least one of the following: O3-PbTiO3 (PMN-PT), hafnium dioxide (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, or TiO2.
[0096] In one embodiment of the present invention, the average particle size (D) of inorganic particles is... 50 The average particle size (D) of the inorganic particles can preferably be, for example, 100 nm or more. Specifically, the average particle size (D) of the inorganic particles can be... 50 The average particle size can be from 100 nm to 1 μm, or from 100 nm to 500 nm. When the average particle size of the inorganic particles falls within the above range, it can have a beneficial effect on suppressing the increase in the resistance of the diaphragm, but the present invention is not limited thereto.
[0097] The particle size of inorganic particles can be measured using known particle size measurement methods, such as the Malvern Particle Size Analyzer (PSA). Furthermore, the average particle size (D...) 50 The particle size distribution (PPD) refers to the particle size at the 50% point of the cumulative particle size distribution and can be measured by laser diffraction. In this case, the laser diffraction particle size measurement device can be, for example, the Microtrac S3500.
[0098] In one embodiment of the invention, the adhesive polymer may include, for example, a polyvinylidene fluoride (PVdF) based resin. In one embodiment of the invention, the PVdF based resin may include at least one of the following: a homopolymer of vinylidene fluoride (i.e., polyvinylidene fluoride), a copolymer of vinylidene fluoride and a polymerizable monomer, and mixtures thereof. In one embodiment of the invention, the monomer may include, for example, a fluorinated monomer and / or a chlorinated monomer. Non-limiting examples of fluorinated monomers may include at least one of the following: vinyl fluoride; trifluoroethylene (TrFE); vinyl chlorofluoroethylene (CTFE); 1,2-difluoroethylene; tetrafluoroethylene (TFE); hexafluoropropylene (HFP); perfluoro(alkyl vinyl) ethers, such as perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE), and perfluoro(propyl vinyl) ether (PPVE); perfluoro(1,3-dioxacyclopentene); or perfluoro(2,2-dimethyl-1,3-dioxacyclopentene) (PDD).
[0099] In one embodiment of the invention, in addition to the foregoing, the adhesive polymer may also include oil-based or water-based adhesives, or mixtures thereof, which can be used in porous coatings, but is not limited thereto.
[0100] In one embodiment of the present invention, the total thickness of the porous coating within the diaphragm may be, for example, 0.5 μm to 50 μm, specifically 0.5 μm to 10 μm, 0.5 μm to 5 μm, or 3 μm to 4.5 μm, but the present invention is not limited thereto.
[0101] Methods for manufacturing diaphragms
[0102] According to another aspect of the present invention, an example of a method for manufacturing the above-described diaphragm is provided.
[0103] The method for manufacturing the diaphragm is an example of the method for manufacturing the diaphragm described above, and the method for manufacturing the diaphragm is not limited to the method described below.
[0104] A method for manufacturing a diaphragm according to one aspect of the present invention includes obtaining a porous polymer matrix by a dry process.
[0105] Specifically, in this specification, the dry process refers to a method of using an extruder to melt a polymer resin, extruding the molten resin to form a film, and stretching it to form pores.
[0106] More specifically, the dry process refers to a process that does not use at least one of diluents and plasticizers (preferably neither diluents nor plasticizers, which are used to form pores in / on the polymer film in the wet process). Therefore, the need for mixing and extraction steps of diluents used in the wet process can be eliminated, thus providing an environmentally friendly manufacturing method, but the invention is not limited thereto.
[0107] According to one embodiment of the present invention, the process for obtaining a porous polymer matrix may include the following steps: (S1) A polyolefin resin is fed into an extruder to obtain an extrudate; (S2) The extrudate is thermoformed to obtain a polymer sheet; (S3) The polymer sheet is stretched at a low temperature and then stretched at a high temperature. (S4) Heat treat the stretched sheet.
[0108] In one embodiment of the invention, the porous polymer matrix may contain only polypropylene resin in terms of mechanical strength. For this purpose, the polyolefin resin may contain polypropylene resin, and step (S1) may include feeding the polypropylene resin into an extruder and melt-blending it.
[0109] According to one embodiment of the invention, the melt-blended polyolefin resin can be extruded through step (S1), and the extrudate can be formed into a polymer sheet through step (S2). Extrusion can be performed using a flat die (e.g., a T-die or a hanger die) and can be formed using a roll-to-roll forming machine.
[0110] Subsequently, the resulting polymer sheet can be stretched at least twice under different temperature conditions.
[0111] Specifically, step (S3) includes stretching the polymer sheet at a low temperature (low-temperature stretching) and then stretching it at a high temperature (high-temperature stretching). Step (S3) may include stretching the obtained polymer sheet at a low temperature to rapidly cool the polymer sheet, thereby increasing the number of pores, and then stretching it at a higher temperature to increase the size of the pores formed during the low-temperature stretching. Therefore, the macropore volume in the obtained porous polymer matrix can be increased through step (S3), but the mechanism of the invention is not limited thereto.
[0112] In one embodiment of the present invention, the mechanical strength and puncture strength of the polymer sheet can be improved by a stretching process.
[0113] In this case, according to one embodiment of the invention, since the porous polymer matrix is uniaxially stretched, the low-temperature stretching and high-temperature stretching are preferably performed in parallel directions. More specifically, each of the low-temperature stretching and high-temperature stretching can be performed in the longitudinal direction (MD).
[0114] In one embodiment of the invention, when a porous polymer matrix is biaxially stretched, the resulting porous polymer matrix can have a porosity greater than 70% by volume, causing wrinkles, resulting in an undesirable surface appearance, and the porous polymer matrix cannot be used in the assembly of electrochemical devices. Therefore, according to one embodiment of the invention, preferably, the porous polymer matrix can be manufactured by uniaxial stretching, and its porosity can be less than 70% by volume.
[0115] In one embodiment of the invention, stretching can be performed by sequential or simultaneous roller stretching or tenter stretching.
[0116] According to one aspect of the invention, in order to increase the macropore volume while maintaining the mechanical strength of the obtained porous polymer matrix, low-temperature stretching is performed at a stretching ratio of less than 50% compared to the high-temperature stretching ratio.
[0117] In this specification, the stretch ratio in step (S3) refers to the ratio of the length of the stretched polymer sheet to the length of the unstretched polymer sheet. In other words, the stretch ratio can be calculated as the ratio of (length of the stretched polymer sheet / length of the unstretched polymer sheet).
[0118] In one embodiment of the invention, low-temperature stretching can be a key step in determining the number of pores in the porous polymer matrix. Specifically, when a first stretching process is performed at low temperature after obtaining the polyolefin sheet, the amorphous structure of the fibers breaks to form small pores. In this case, if the low-temperature stretching ratio is too high, the polyolefin sheet may be torn, or the porosity of the porous polymer matrix may have negative consequences. Therefore, low-temperature stretching can preferably be performed at a stretching ratio range smaller than the high-temperature stretching ratio. Specifically, the low-temperature stretching ratio can preferably be less than 50% of the high-temperature stretching ratio.
[0119] In one embodiment of the present invention, the low-temperature stretching ratio can be less than 1.05 times, for example, 1.0 times to 1.03 times, but the present invention is not limited thereto.
[0120] In one embodiment of the invention, high-temperature stretching can be a key step in determining the pore size in the porous polymer matrix. Specifically, when a sheet with small pores formed during a low-temperature stretching process is further stretched at a high temperature, the size of the already formed small pores can be increased to form multiple large pores. In this case, when the high-temperature stretching ratio is extremely small, the total volume of large pores in the porous polymer matrix may be insufficient, leading to an increase in the resistance of the membrane. Therefore, high-temperature stretching can preferably be performed at a stretching ratio range larger than the aforementioned low-temperature stretching ratio.
[0121] In one embodiment of the present invention, the high-temperature stretching ratio can be more than 2 times, and can be, for example, 2.0 times to 2.1 times, but the present invention is not limited thereto.
[0122] In one embodiment of the invention, the stretching temperature may be varied according to the melting point of the polymer used (e.g., polypropylene resin), and the invention is not limited thereto.
[0123] In one embodiment of the present invention, in order to increase the macropore volume of the porous polymer matrix, thermoforming and heat treatment processes can be performed at different temperatures before / after the stretching step (S3).
[0124] In particular, in one embodiment of the invention, low-temperature stretching can preferably be performed at a temperature lower than the preceding thermoforming temperature, and high-temperature stretching can preferably be performed at a temperature higher than the preceding low-temperature stretching. Specifically, high-temperature stretching can be performed at a temperature equal to or higher than the preceding thermoforming temperature, and more specifically, high-temperature stretching can be performed at a temperature higher than the thermoforming temperature, but the invention is not limited thereto.
[0125] Furthermore, in one embodiment of the invention, heat setting is a process used to remove residual stress in the polymer sheet after stretching, and can preferably be performed at a higher temperature than the preceding thermoforming, low-temperature stretching and high-temperature stretching processes.
[0126] According to one embodiment of the present invention, step (S1) can be performed at a temperature above 200°C to melt the polyolefin resin.
[0127] According to one embodiment of the invention, the subsequent step (S2) may be performed, for example, at a temperature of 140°C to 160°C (e.g., 140°C to 150°C, or 145°C to 150°C) to cool the obtained extrudate and form the extrudate into a sheet.
[0128] According to one embodiment of the invention, the low-temperature stretching in step (S3) can be performed, for example, at a temperature of 90°C to 135°C (e.g., 90°C to 120°C, 95°C to 110°C, or 100°C to 110°C) to rapidly cool the thermoformed polymer sheet while increasing the number of pores. When low-temperature stretching is performed at the above temperatures, it can have a beneficial effect on the air permeability and mechanical strength of the obtained polymer sheet, but the invention is not limited thereto. For example, as the stretching temperature increases, the air permeability of the polymer sheet increases, resulting in low mechanical strength and poor stability.
[0129] According to one embodiment of the invention, the high-temperature stretching in step (S3) can be performed, for example, at a temperature of 140°C to 160°C (e.g., 140°C to 150°C or 145°C to 150°C) to further stretch the low-temperature stretched polymer sheet at a higher temperature to increase the pore size. When high-temperature stretching is performed at the above temperatures, it can have a beneficial effect on the air permeability and mechanical strength of the obtained polymer sheet, but the invention is not limited thereto. For example, as the stretching temperature increases, the air permeability of the polymer sheet increases, resulting in lower mechanical strength and poor stability.
[0130] According to one embodiment of the present invention, step (S4) may include heat setting at a temperature higher than that of (S1) to (S3) to remove residual stress in the stretched polymer sheet and increase mechanical strength, and the heat setting temperature may be, for example, 150°C to 170°C, 150°C to 165°C, 150°C to 160°C or 155°C to 160°C, but the present invention is not limited thereto.
[0131] According to one embodiment of the present invention, the method of manufacturing a diaphragm may further include step (S5) after obtaining a porous polymer matrix: forming a porous coating on at least one surface of the porous polymer matrix.
[0132] In one embodiment of the present invention, step (S5) may include: dispersing or dissolving the adhesive polymer in a solvent to prepare an adhesive solution, and adding inorganic particles to the adhesive solution to prepare a coating slurry.
[0133] Non-limiting examples of solvents used to prepare coating slurries may include one or more mixtures of the group consisting of water, acetone, tetrahydrofuran, dichloromethane, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP) and cyclohexane, but the invention is not limited thereto.
[0134] In one embodiment of the invention, the slurry can be coated onto a porous polymer matrix using any commonly used coating method known in the art, such as dip coating, die coating, roll coating, comma coating, or a combination thereof. Furthermore, the drying can be performed using any commonly used drying method (e.g., including but not limited to natural drying or air drying).
[0135] Electrode assemblies and electrochemical devices
[0136] According to another aspect of the present invention, an electrode assembly is provided, the electrode assembly comprising: the aforementioned diaphragm, and a first electrode and a second electrode respectively present on two surfaces of the diaphragm.
[0137] According to another aspect of the present invention, an electrochemical device is provided, the electrochemical device comprising: the aforementioned diaphragm, a first electrode and a second electrode respectively present on two surfaces of the diaphragm, an electrolyte, and a housing therein.
[0138] The first electrode and the second electrode can each be either positive or negative.
[0139] In one embodiment of the present invention, the positive electrode and the negative electrode may each include a current collector coated with an electrode active material, or may be a separate metal plate without a current collector or a membrane containing an active material, and there are no particular limitations on their size or shape or the type of active material.
[0140] For example, an electrochemical device according to one embodiment of the present invention may include an NCM-based active material as a positive electrode and a graphite-based active material as a negative electrode, but the present invention is not limited thereto.
[0141] Furthermore, in one embodiment of the invention, the electrochemical device may include, for example, a primary battery, a secondary battery, a supercapacitor, or an electric double-layer capacitor. More specifically, the secondary battery may be a lithium-ion secondary battery.
[0142] In one embodiment of the invention, the housing may include any commonly used battery housing and is not limited to a specific shape; it may have any shape suitable for the battery application. For example, the housing may have a cylindrical, prismatic, bag-shaped, or coin-shaped shape similar to a can.
[0143] When the electrode assembly is completed, it can be placed in a housing using common methods, and the housing can then be sealed to manufacture an electrochemical device, in which case the electrochemical device can be, for example, a lithium secondary battery.
[0144] As described above, the diaphragm according to one aspect of the invention is characterized by having low resistance through improved resistivity characteristics. Therefore, electrode assemblies and electrochemical devices using this diaphragm can have low resistance and thus high output characteristics.
[0145] The invention will be described in more detail below by way of examples, but the following examples are provided for illustrative purposes and the scope of the invention is not limited thereto.
[0146] Preparation of diaphragm
[0147] Comparative Example 1
[0148] Preparation of porous polymer matrix
[0149] Polypropylene (Daehan Petrochemical, S800M, MI 0.8) is supplied as raw material to the extruder (Korea EM). In a 32 single-screw extruder (L / D=40), the material is then melted to obtain an extrudate at 230°C.
[0150] Polypropylene extruder is formed into sheets as follows: thermoforming is performed using a uniaxial stretching machine at a temperature range of 145°C, followed by a first stretch at a low temperature stretching zone of 100°C with a stretch ratio of 1.08, a second stretch at a high temperature stretching zone of 145°C with a stretch ratio of 2.1, and heat setting at 155°C (stretch ratio = 0.95) to produce a 12 μm thick porous polymer matrix. That is, the stretching process is performed at a ratio of 51% of [(low temperature stretch ratio) / (high temperature stretch ratio)].
[0151] diaphragm coating
[0152] A porous coating consisting of an inorganic layer and an adhesive layer is formed on both surfaces of the prepared porous polymer matrix using the following method.
[0153] First, an alumina dispersion in water (95 wt% solids content) was coated onto both surfaces of a porous polymer matrix and dried to form an inorganic layer with a thickness of 1.5 μm on each surface. Subsequently, a PVDF adhesive solution dissolved in acetone (80 wt% solids content) was coated onto the inorganic layer and dried to form an adhesive layer with a thickness of 0.75 μm on each surface. The total thickness of the porous coating on both surfaces was 4.5 μm.
[0154] Example 1
[0155] The membrane was prepared using the same method as in Comparative Example 1, except that a 12 μm thick porous polymer matrix was prepared by a single stretching operation in a low-temperature stretching zone at a stretching ratio of 1.03 during the fabrication of the porous polymer matrix. That is, the stretching process was performed at a ratio of 49% of [(low-temperature stretching ratio) / (high-temperature stretching ratio)].
[0156] Battery performance evaluation
[0157] Lithium-ion batteries were manufactured using the prepared separator by the following method, and the characteristics of the manufactured batteries were evaluated as follows.
[0158] Preparation of positive electrode
[0159] The positive electrode active material (LiNi) 0.8 Mn 0.1 Co 0.1O2, conductive material (carbon black), and binder resin (PVDF) are mixed with water in a weight ratio of 97.5:0.7:1.8 to prepare a slurry for the positive electrode active material layer, wherein the concentration of the remaining components other than water is 50% by weight. Subsequently, the slurry is coated onto the surface of an aluminum foil (10 μm thick) and dried to manufacture a positive electrode with a positive electrode active material layer (60 μm thick).
[0160] Preparation of negative electrode
[0161] A slurry for the negative electrode active material layer was prepared by mixing graphite-based active material, carbon black, carboxymethyl cellulose (CMC), and binder resin (SBR) with water in a weight ratio of 97.5:0.7:1.1:0.7, wherein the concentration of the remaining components excluding water was 50% by weight. In this case, a 9:1 mixture of artificial graphite and natural graphite was used as the graphite-based active material. Subsequently, the slurry was coated onto the surface of a copper foil (10 μm thick) and dried to manufacture a negative electrode with a negative electrode active material layer (60 μm thick).
[0162] Assembly of electrode components
[0163] The coated diaphragm was placed between the positive and negative electrodes and laminated at 75°C, 9 MPa and 1 s to prepare the electrode assembly.
[0164] Preparation of lithium secondary batteries
[0165] The prepared positive electrode is stamped into a shape with a width of 50 mm and a length of 33 mm. 2 The prepared negative electrode is stamped to a size of 51 × 34 mm (width) × (length). 2 The dimensions of the prepared coated diaphragm were determined by stamping it to a width × length of 56 × 39 mm. 2 The dimensions are the same, and lamination is performed using the same method.
[0166] The laminated electrode assembly was placed in a bag, and an electrolyte consisting of a 1M LiPF6, ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (3 / 7 v / v), and 2% by weight of ethylene carbonate (VC) was injected. The bag was then sealed to prepare a single cell.
[0167] Resistance evaluation
[0168] The prepared single cell was discharged at a 3C rate in CC mode (2.5 V cutoff condition), and the resistance was measured over 500 seconds during the discharge.
[0169] Table 1
[0170] The results above show that, according to one embodiment of the present invention, the battery resistance is improved, thereby improving the battery's output characteristics.
[0171] Evaluation of diaphragm properties
[0172] To investigate whether the difference in battery resistance is caused by the difference in pore characteristics of the porous polymer matrix within the laminated battery, the porous polymer matrix was separated from the electrode assembly after lamination, and the following evaluation was performed.
[0173] The positive and negative electrodes are removed from the electrode assembly, and the porous coating on the membrane surface is also removed. To remove the porous coating, the membrane is immersed in dimethyl carbonate (DMC) solvent and sonicated while maintaining the temperature below 35°C until the porous coating is completely removed.
[0174] Subsequently, the porous polymer matrix was obtained based on the following evaluation.
[0175] Evaluation of the proportion of large pores
[0176] The proportion of pores with a size greater than 100 nm was evaluated using the following method.
[0177] The proportion of macropores in porous polymer matrices was measured using an Aquapore water immersion porosimeter (Poretech Instrument, WMI-5K) under conditions of 150–2,500 psi, surface tension of 72 N / m (20 °C), and contact angle of 120°.
[0178] The macropore ratio is measured as the ratio of the total volume of macropores with a diameter of 100 nm or more to the total pore volume in the porous polymer matrix.
[0179] Evaluation of the pressure difference (ΔP) between pores in a porous polymer matrix
[0180] A predetermined amount of water was injected into a porous polymer matrix using an Aquapore water immersion porosimeter (Poretech Instrument, WMI-5K). After injecting the predetermined amount of water into the pores of the porous polymer matrix until the water saturation reached 100% by volume, a cumulative pore volume map was obtained as a function of the injected water pressure (psi).
[0181] In the corresponding diagram, the more water fills the hole, the higher the water pressure; the lower the water pressure, the larger the hole is filled. Therefore, the lowest water pressure represents the largest hole filled, and the highest water pressure represents the smallest hole filled. In this case, the difference between the lowest and highest water pressures is measured as the pressure differential (ΔP).
[0182] Measurement of air permeability (Grey value) of porous polymer matrix
[0183] The time (in seconds) required for 100 cc of air to pass through a 1 square inch porous polymer matrix under a pressure of 12.2 inches of H2O was measured using a Gly air permeability meter, according to ASTM D726-94 standard.
[0184] Measurement of thickness (L) of porous polymer matrix
[0185] The thickness of the porous polymer matrix was measured using a Mitutoyo thickness gauge.
[0186] Evaluation of the permeability (u) of porous polymer matrices
[0187] The permeability of porous polymer matrices is evaluated according to Equation 1 below.
[0188] Formula 1
[0189] u=κΔPL
[0190] u represents the unit area (1 cm²) of the porous polymer matrix. 2 Transmittance (cm) 3 (·psi·μm / sec).
[0191] κ is the glyph transmittance value, and it is the reciprocal of the glyph value (1 / glyph) (cc / s=cm). 3 / s).
[0192] ΔP is the pressure difference of the porous polymer matrix (psi).
[0193] L is the thickness (μm) of the porous polymer matrix.
[0194] Table 2 below summarizes the evaluation results of the measurement properties.
[0195] Table 2
[0196] The results above show that the separator manufactured according to one embodiment of the present invention exhibits a large pressure difference between macropores and micropores and a macropore ratio of more than 3% after lamination, thus confirming that a high permeability coefficient is maintained. Therefore, it can be inferred that the output characteristics of batteries using it will be improved.
[0197] [List of reference numerals]
[0198] 200: Porous polymer matrix
[0199] 201: Polyolefin backbone
[0200] 202: Microfibers
[0201] 203: Kong
[0202] a: The direction of microfiber extension
[0203] b: The direction of extension of the polyolefin backbone
[0204] MD: Vertical
Claims
1. A membrane comprising: a porous polymer matrix comprising a polyolefin resin, The porous polymer matrix comprises: The main chain of the polyolefin resin. Microfibers, the microfibers extending in a direction not parallel to the extension direction of the main chain, and Pores exist between the microfibers. Based on the total volume of the pores, the volume of pores with a diameter of 100 nm or more accounts for more than 3%.
2. The diaphragm according to claim 1, The polyolefin resin mentioned above includes polypropylene resin, and The polypropylene resin accounts for 95% or more of the total weight of the porous polymer matrix.
3. The diaphragm according to claim 1, The cross-section of the hole comprises an elliptical shape with an aspect ratio greater than 1, and the aspect ratio is defined by the following formula: Formula 1 Aspect ratio = [(length in the extension direction of the microfiber (a)) / (length in the extension direction of the main chain (b))].
4. The diaphragm according to claim 1, Based on the total volume of the pores, the volume of pores with a diameter of 100 nm or more is 4% to 10%.
5. The diaphragm according to claim 1, The maximum water pressure differential (ΔP) of the porous polymer matrix is above 1,550 psi. The maximum water pressure difference refers to the difference between the highest and lowest water pressure in the water pressure-water saturation diagram, which is obtained by injecting water into the porous polymer matrix at a constant rate to achieve 100% water saturation by volume.
6. The diaphragm according to claim 5, The maximum water pressure differential of the porous polymer matrix is above 1,600 psi.
7. The diaphragm according to claim 1, The porous polymer matrix has a permeability of 150 cm⁻¹. 3 For transmittance of psi·μm / sec or higher, the transmittance coefficient is defined as follows: Equation 2: Formula 2 u=κΔPL u represents the permeability coefficient of the porous polymer matrix. κ is the gravimetric permeability of the porous polymer matrix. ΔP represents the maximum water pressure difference in the porous polymer matrix, and L is the thickness of the porous polymer matrix.
8. The diaphragm according to claim 1, The thickness of the porous polymer matrix is 5 μm to 14 μm.
9. The diaphragm according to claim 1, further comprising: a porous coating, the porous coating being present on at least one surface of the porous polymer matrix. The porous coating comprises inorganic particles and a binder polymer.
10. An electrochemical device, the electrochemical device comprising: The diaphragm according to any one of claims 1 to 9; The first electrode and the second electrode are respectively present on the two surfaces of the diaphragm; Electrolytes; and A housing that contains the diaphragm, the first electrode, the second electrode, and the electrolyte.
11. A method for manufacturing a diaphragm, the method comprising: The process used to obtain a porous polymer matrix, The process for obtaining the porous polymer matrix includes the following steps: (S1) A polyolefin resin is fed into an extruder to obtain an extrudate; (S2) The extrudate is thermoformed to obtain a polymer sheet; (S3) The polymer sheet is subjected to low-temperature stretching, followed by high-temperature stretching; and (S4) The stretched sheet is heat-treated. In step (S3), the low-temperature stretching and the high-temperature stretching are each uniaxial stretching processes, and they are performed in parallel directions. The low-temperature stretching is performed with a stretching ratio of less than 50%, compared to the high-temperature stretching ratio. The stretch ratio is the ratio of the length of the polymer sheet after stretching to the length of the polymer sheet before stretching.
12. The method for manufacturing a diaphragm according to claim 11, The low-temperature stretching ratio is less than 1.05 times.
13. The method for manufacturing a diaphragm according to claim 11, The high-temperature stretching ratio is more than 2 times.
14. The method for manufacturing a diaphragm according to claim 11, The thermoforming and the heat treatment are performed at different temperatures.
15. The method for manufacturing a diaphragm according to claim 11, The low-temperature stretching is performed at a temperature lower than the thermoforming temperature. The high-temperature stretching is performed at a temperature equal to or higher than the thermoforming temperature, and The heat treatment is performed at a temperature higher than that of the high-temperature stretching.
16. The method for manufacturing a diaphragm according to claim 11, The process for obtaining the porous polymer matrix is a process that does not use at least one of a diluent and a plasticizer.
17. The method for manufacturing a diaphragm according to claim 11, the method further comprising the following steps: A porous coating is formed on at least one surface of the porous polymer matrix, the porous coating comprising inorganic particles and a binder polymer.