A three-dimensional heat-pressing molding process for safety pants

By combining zoned temperature-controlled hot pressing molds and arc molds with infrared preheating and rapid cooling processes, the problems of unstable parameters and poor material adaptability in the hot pressing and shaping of three-dimensional enclosures have been solved, achieving stable arc shaping and efficient production of enclosures.

CN123101331APending Publication Date: 2026-11-17HUBEI TIANJIAO SANITARY PRODUCTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611270807.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The existing hot-pressing and shaping process for three-dimensional enclosures lacks precise control, resulting in over- or under-pressing, which fails to form a continuous and uniform arc-shaped shaping trajectory, and the internal stress of the material is not fully released. Furthermore, the process has poor adaptability, affecting product quality and leak-proof performance.

Method used

The process employs zoned temperature-controlled hot pressing molds, gradient pressurization, rapid cooling, and online detection feedback. Combined with arc-shaped molds and infrared preheating, it achieves precise hot pressing and rapid cooling of three-dimensional enclosures, adapting to different material specifications.

Benefits of technology

This design achieves a stable arc shape at the base of the enclosure, improving the product's leak-proof performance and material retention rate, shortening the changeover and adjustment time, and reducing the product defect rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123101331A_ABST
    Figure CN123101331A_ABST
Patent Text Reader

Abstract

This invention relates to a hot-pressing and shaping process for three-dimensional protective covers on sanitary products, belonging to the field of hygiene product manufacturing technology. The process includes the following steps: S1, material preparation; S2, preheating: using an infrared preheating device to preheat the area to be hot-pressed on the three-dimensional protective cover blank; S3, hot-pressing and shaping: using an arc-shaped hot-pressing mold to hot-press the base of the preheated three-dimensional protective cover; S4, zoned pressure holding: reducing the pressure of the hot-pressing mold to 0.05MPa~0.15MPa; S5, cooling and shaping: using a cooling air knife or cooling roller at a temperature of 5℃~15℃ to cool the hot-pressed area; S6, online detection: detecting the width, height, and surface temperature of the protective cover after hot pressing. This hot-pressing and shaping process for three-dimensional protective covers on sanitary products, by using an arc-shaped hot-pressing mold to hot-press the base of the protective cover, creates an upward-curving arc-shaped shaping area at the base, which is more ergonomic than traditional flat pressing; combined with zoned pressure holding and rapid cooling, it effectively eliminates internal stress in the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hygiene product manufacturing technology, specifically to a hot-pressing and shaping process for three-dimensional protective covers of sanitary trousers. Background Technology

[0002] As a type of one-piece disposable absorbent underwear, the "safety panty" is favored by consumers for its ease of wear and excellent leak-proof performance. The 3D protective barrier is the core structure of the safety panty's leak-proof design. It is typically made of hydrophobic non-woven fabric wrapped around elastic spandex fibers, arranged longitudinally along both sides of the crotch area. When worn, it stands up to form a barrier, preventing liquid leakage. To ensure that the 3D protective barrier maintains its stable shape during storage, transportation, and wear, the base of the barrier usually requires heat-pressing and shaping.

[0003] The existing hot-pressing and shaping process for three-dimensional protective barriers has the following main shortcomings: First, parameters such as hot-pressing temperature, pressure, and time rely heavily on operational experience for setting, lacking precise control. This can lead to over-pressing, causing the nonwoven fabric to become brittle or even melt, or under-pressing, resulting in the barrier becoming loose and losing its elasticity. Second, traditional hot-pressing molds are mostly planar pressing structures, which cannot form a continuous and uniform arc-shaped shaping trajectory at the base of the barrier. The barrier is prone to springing back after folding, affecting the product's appearance and leak-proof effect. Third, the lack of a rapid cooling and shaping stage after hot pressing means that the material's internal stress is not fully released, making the barrier prone to deformation during subsequent packaging processes. Fourth, different material combinations (such as different weights of nonwoven fabric and different denier spandex yarns) require different hot-pressing parameters. The existing process has poor adaptability and long adjustment times for changeovers.

[0004] Therefore, there is an urgent need for a three-dimensional hot-pressing and shaping process for protective trousers that can precisely control hot-pressing parameters, form an arc-shaped shaping trajectory, be equipped with cooling and shaping, and have strong process adaptability. This invention aims to provide a three-dimensional hot-pressing and shaping process for protective trousers that solves problems such as unstable hot-pressing quality, easy springback deformation of the protective trousers, and difficulty in shape change adjustments in existing processes by using technologies such as zoned temperature-controlled hot-pressing molds, gradient pressurization, rapid cooling, and adaptive parameter adjustment. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a hot-pressing and shaping process for three-dimensional protective covers on safety pants. This process offers advantages such as arc-shaped mold shaping to ensure stable three-dimensional shape of the protective cover, zoned temperature control and gradient pressurization to ensure uniform hot-pressing quality, rapid cooling to eliminate internal stress and prevent rebound deformation, and online detection with closed-loop feedback for automatic parameter adjustment and strong adaptability. It solves the problems in existing processes, such as easy rebound and loosening of the protective cover base after hot pressing, unstable hot-pressing quality, difficulty in adjusting for different materials, and low protective cover shape retention rate leading to reduced side leakage prevention effect.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A heat-pressing and shaping process for a three-dimensional protective trouser cuff includes the following steps: S1. Material preparation: The three-dimensional protective non-woven fabric blank with spandex filaments is conveyed to the hot pressing station; S2. Preheating: An infrared preheating device is used to preheat the area of ​​the three-dimensional protective blank to be hot-pressed. The preheating temperature is 50℃~70℃ and the preheating time is 0.5s~1.5s. S3. Hot pressing and shaping: The preheated three-dimensional enclosure root is hot-pressed using an arc-shaped hot pressing mold. The hot pressing temperature is 100℃~140℃, the hot pressing pressure is 0.2MPa~0.6MPa, and the hot pressing time is 0.8s~2.0s. The working surface of the arc-shaped hot pressing mold is a continuous arc surface that is concave or convex, and the radius R of the arc surface is 50mm~150mm. S4, Zoned Pressure Holding: Reduce the pressure of the hot pressing mold to 0.05MPa~0.15MPa, and hold the pressure for 0.5s~1.0s; S5. Cooling and Shaping: Cooling air knives or cooling rollers with a temperature of 5℃~15℃ are used to cool the hot-pressed area for 1.0s~2.5s. After cooling, the temperature at the root of the enclosure drops to below 40℃. S6. Online detection: Detect the width, height and surface temperature of the enclosure after hot pressing.

[0007] Furthermore, the arc-shaped hot pressing mold has an arc width of 8mm to 15mm, and multiple protrusions or patterns are provided on the arc surface to form dot-like or grid-like hot pressing marks on the surface of the non-woven fabric.

[0008] Furthermore, the hot press mold is equipped with a zoned heating element, which is divided into three heating zones along the length of the mold: front, middle, and rear. The temperature of each heating zone can be set independently, and the temperature difference is controlled within ±5℃.

[0009] Furthermore, the hot-pressing temperature in S3 is positively correlated with the denier of the spandex filament and the basis weight of the nonwoven fabric: when the denier of the spandex filament increases by 10D, the hot-pressing temperature increases by 3℃~5℃; when the basis weight of the nonwoven fabric increases by 5g / m², the hot-pressing temperature increases by 2℃~4℃.

[0010] Furthermore, in S5, the angle between the air outlet of the cooling air knife and the surface of the three-dimensional enclosure is 30° to 60°, and the cooling gas is dry compressed air or nitrogen.

[0011] Furthermore, the online detection results in S6 are fed back to the hot-pressing parameter control system in step three. When the height of the enclosure is detected to exceed the set range, the hot-pressing temperature or pressure is automatically fine-tuned.

[0012] Furthermore, in S2, the infrared preheating device has a power of 1.0kW to 2.5kW, and the surface temperature of the billet rises to 40℃ to 60℃ after preheating.

[0013] Furthermore, after the S3 hot pressing, an upward-curving arc-shaped shaping area is formed at the root of the guard, and the arc surface of the arc-shaped shaping area matches the arc surface of the arc-shaped hot pressing mold.

[0014] Furthermore, in S5, multiple cooling air knives are spaced apart along the length of the three-dimensional enclosure, with a spacing of 50mm to 150mm between adjacent cooling air knives, and each cooling air knive is independently controlled to open / close and control airflow.

[0015] Furthermore, the online inspection in S6 uses a CCD vision inspection system to detect the height of the fence and the clarity of the hot pressing marks, and automatically marks or removes unqualified products.

[0016] Compared with the prior art, the present invention provides a heat-pressing and shaping process for three-dimensional protective trousers, which has the following beneficial effects: 1. The 3D heat-pressing molding process used in these reassurance pants involves applying heat to the base of the reassurance using an arc-shaped hot-pressing mold. This creates an upward-curving arc-shaped molding area at the base, which is more ergonomic than traditional flat pressing. The reassurance naturally stands up when worn, preventing it from rolling inward or outward. Combined with zoned pressure holding and rapid cooling, it effectively eliminates internal material stress. The reassurance retains over 95% of its height in compression rebound tests (compared to approximately 80% with traditional methods).

[0017] 2. The three-dimensional heat-pressing and shaping process of this safety pants utilizes independent temperature control in different zones, infrared preheating, gradient pressurization, and parameter-material characteristic correlation adjustment to enable the process to quickly adapt to products of different specifications (different spandex deniers and non-woven fabric weights). Changeover time is reduced from 30 minutes in the traditional process to less than 5 minutes, greatly improving the flexibility of the production line.

[0018] 3. The three-dimensional heat-pressing process of this safety pants integrates online visual inspection and infrared temperature measurement to monitor the heat-pressing effect in real time and feed the data back to the control system. It automatically fine-tunes the heat-pressing parameters, effectively avoiding the fluctuation of the setting quality caused by the fluctuation of ambient temperature and the difference of material batches. The product defect rate is reduced from 3% to 5% of the traditional process to less than 0.5%. Attached Figure Description

[0019] Figure 1 This is a process flow diagram of the hot pressing and shaping process for the three-dimensional protective gaiter of the safety pants according to the present invention. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Example 1: Standard style 3D protective gaiter heat-pressed and shaped Please see Figure 1 The three-dimensional heat-pressing and shaping process for the safety pants in this embodiment includes the following steps: S1. Material preparation: The composite three-dimensional protective blank is conveyed at a linear speed of 80m / min and aligned with the hot pressing station by the correction device.

[0022] S2. Preheating: The infrared preheating device has a power of 1.5kW, a preheating temperature of 60℃, a preheating time of 1.0s, and the surface temperature of the billet rises to about 50℃.

[0023] S3. Hot Pressing and Shaping: The working surface of the arc-shaped hot press mold is a concave arc surface with a radius R = 100mm and a width of 12mm. The surface is decorated with diamond-shaped raised dots. The hot pressing temperature is 120℃, the pressure is 0.4MPa, and the time is 1.2s. The mold is divided into three heating zones: the front zone is 118℃, the middle zone is 121℃, and the rear zone is 119℃, with the temperature difference controlled within ±2℃.

[0024] S4. Zoned pressure holding: The mold pressure is reduced to 0.1MPa and held for 0.8s to allow heat to penetrate evenly to each layer of the nonwoven fabric.

[0025] S5. Cooling and Shaping: The angle between the cooling air knife outlet and the surface of the enclosure is 45°, the cooling air temperature is 8℃, the air pressure is 0.3MPa, the cooling time is 2.0s, and the temperature at the root of the enclosure drops to 35℃ after cooling.

[0026] S6. Online inspection: The visual inspection system measures the height (standing height) of the fence to be 12±1mm and the width to be 10±0.5mm. The infrared thermometer measures the surface temperature to be 32℃~38℃. All are qualified.

[0027] Shaping effect: After placing 100 pieces of the product in a 40℃ oven for 72 hours, the average height retention rate of the protective cover was 96.5%, with no burns or brittleness.

[0028] Example 2: Heightened (Leak-proof Enhanced) Protective Enclosure Heat Pressing and Shaping This embodiment is used to produce plus-size or nighttime safety pants, with the weight of the three-dimensional protective non-woven fabric increased to 22g / m², and the spandex yarn is 550D, with 6 yarns on each side.

[0029] The process parameters are adjusted as follows: Preheating temperature: 65℃; Preheating time: 1.2s; Hot pressing temperature 135℃ (increased due to thicker material and coarser spandex), pressure 0.55MPa, time 1.8s; The radius of the mold arc surface R = 120mm (to accommodate wider enclosures); The cooling air knife temperature is 10℃, and the cooling time is 2.5s.

[0030] Shaping effect: The initial height of the guardrail is 15mm. After 72 hours of high-temperature storage, the height retention rate is 94.8%, with no rebound deformation.

[0031] Example 3: Thin and lightweight (ultra-flexible) protective fence heat-pressing and shaping This embodiment is used to produce ultra-thin summer-style safety pants, with a non-woven fabric weight of 15g / m², 280D spandex yarn, and 3 yarns on each side.

[0032] Process parameters: Preheating temperature 55℃, preheating time 0.8s; Hot pressing temperature 105℃ (to prevent burns to thin materials), pressure 0.25MPa, time 0.9s; The radius of the mold arc surface R = 70mm; The cooling air knife temperature is 12℃, and the cooling time is 1.5s.

[0033] Shaping effect: The height retention rate of the guardrail is 97.2%, and the non-woven fabric is not brittle or wrinkled.

[0034] Example 4: Online Feedback Adaptive Adjustment Example During production, visual inspection revealed that the guard height of five consecutive products was 10mm (below the target of 12±1mm), leading the system to determine insufficient hot pressing. The control program automatically increased the hot pressing temperature from 120℃ to 126℃ (increasing by 1.5℃ each time), while simultaneously increasing the pressure from 0.40MPa to 0.45MPa. After adjustment, the guard height of 10 products was restored to 11.5mm~12.5mm. The entire adaptive process was completed within 30 seconds without machine downtime.

[0035] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0036] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A heat-pressing and shaping process for three-dimensional protective cuffs on safety pants, characterized in that, Includes the following steps: S1. Material preparation: The three-dimensional protective non-woven fabric blank with spandex filaments is conveyed to the hot pressing station; S2. Preheating: An infrared preheating device is used to preheat the area of ​​the three-dimensional protective blank to be hot-pressed. The preheating temperature is 50℃~70℃ and the preheating time is 0.5s~1.5s. S3. Hot pressing and shaping: The preheated three-dimensional enclosure root is hot-pressed using an arc-shaped hot pressing mold. The hot pressing temperature is 100℃~140℃, the hot pressing pressure is 0.2MPa~0.6MPa, and the hot pressing time is 0.8s~2.0s. The working surface of the arc-shaped hot pressing mold is a continuous arc surface that is concave or convex, and the radius R of the arc surface is 50mm~150mm. S4, Zoned Pressure Holding: Reduce the pressure of the hot pressing mold to 0.05MPa~0.15MPa, and hold the pressure for 0.5s~1.0s; S5. Cooling and Shaping: Cooling air knives or cooling rollers with a temperature of 5℃~15℃ are used to cool the hot-pressed area for 1.0s~2.5s. After cooling, the temperature at the root of the enclosure drops to below 40℃. S6. Online detection: Detect the width, height and surface temperature of the enclosure after hot pressing.

2. The three-dimensional protective girder heat-pressing and shaping process for safety pants according to claim 1, characterized in that, The arc-shaped hot pressing mold has an arc width of 8mm to 15mm and multiple protrusions or patterns on the arc surface, which are used to form dot-like or grid-like hot pressing marks on the surface of non-woven fabric.

3. The heat-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, The hot press mold is equipped with a zoned heating element, which is divided into three heating zones along the length of the mold: front, middle and rear. The temperature of each heating zone can be set independently, and the temperature difference is controlled within ±5℃.

4. The hot-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, The hot-pressing temperature in S3 is positively correlated with the denier of the spandex filament and the basis weight of the nonwoven fabric: when the denier of the spandex filament increases by 10D, the hot-pressing temperature increases by 3℃~5℃; when the basis weight of the nonwoven fabric increases by 5g / m², the hot-pressing temperature increases by 2℃~4℃.

5. The hot-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, In S5, the angle between the air outlet of the cooling air knife and the surface of the three-dimensional enclosure is 30° to 60°, and the cooling gas is dry compressed air or nitrogen.

6. The hot-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, The online detection results in S6 are fed back to the hot-pressing parameter control system in step three. When the height of the enclosure is detected to exceed the set range, the hot-pressing temperature or pressure is automatically fine-tuned.

7. The heat-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, In S2, the infrared preheating device has a power of 1.0kW to 2.5kW, and the surface temperature of the billet rises to 40℃ to 60℃ after preheating.

8. The heat-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, After the S3 hot pressing, an upward-curving arc-shaped shaping area is formed at the root of the enclosure, and the arc surface of the arc-shaped shaping area matches the arc surface of the arc-shaped hot pressing mold.

9. The hot-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, In S5, multiple cooling air knives are spaced apart along the length of the three-dimensional enclosure, with a spacing of 50mm to 150mm between adjacent cooling air knives. Each cooling air knife is independently controlled to open and close and control the airflow.

10. The hot-pressing and shaping process for a three-dimensional protective trouser guard according to claim 1, characterized in that, The online inspection in S6 uses a CCD vision inspection system to detect the height of the fence and the clarity of the hot pressing marks, and automatically marks or removes unqualified products.