A method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine.
By employing a nanofiltration-forward osmosis-high-pressure reverse osmosis-electrolysis-carbon dioxide mineralization method, the problem of efficient utilization of raw brine and lithium precipitation mother liquor from carbonate-type salt lakes has been solved, enabling the preparation of battery-grade lithium carbonate, reducing energy consumption and costs, and making it suitable for industrialization.
Patent Information
- Application Number
- CN202611430336.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
The utilization of carbonate-type brine and lithium precipitation mother liquor in existing technologies is complicated by high energy consumption and high cost. Carbon dioxide capture and storage require a two-step method, and there are no reports of using lithium carbonate mother liquor to capture carbon dioxide and co-produce battery-grade lithium carbonate.
A method of nanofiltration-forward osmosis primary concentration-high-pressure reverse osmosis secondary concentration-electrolysis-carbon dioxide mineralization is used to pretreat carbonate brine. After that, lithium and carbonate are separated by a membrane separation system. The lithium solution is concentrated by forward osmosis and high-pressure reverse osmosis systems. An alkaline environment is maintained by electrolysis using an ion-exchange membrane or bipolar membrane. Carbon dioxide gas is introduced to carry out a co-precipitation reaction to prepare battery-grade lithium carbonate.
This method achieves efficient and comprehensive recovery of lithium and hydroxide ions from carbonate-type salt lake raw brine and lithium carbonate mother liquor, simplifies the process, reduces production costs, reduces pollution, and is suitable for industrial-scale promotion.
Smart Images

Figure CN123102123A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of comprehensive utilization of salt lake resources, specifically relating to a method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate brine. Background Technology
[0002] Lithium (Li) is the lightest metallic element in nature, silvery-white in color, and possesses unique physicochemical properties such as high specific heat, high electrical conductivity, and strong chemical reactivity. It has a wide range of applications. Currently, the use of metallic lithium and its compounds in traditional industrial fields such as glass ceramics, electrolytic aluminum, lubricating greases, air conditioning and refrigeration, organic synthesis, metallurgy, chemicals, pharmaceuticals, and reagents continues to grow. Its applications in energy, military, aerospace, and nuclear industries, including aluminum-lithium alloys, lithium batteries, and nuclear fusion, are also expanding rapidly. Therefore, it is known as "industrial MSG" and is considered an important strategic material by many countries. Due to its application in lithium batteries, it is also hailed as an "energy metal that drives world progress." In nature, lithium resources are mainly found in solid ores and liquid brines. The important position of brine lithium resources in global lithium resource development has been established for nearly 30 years, and its application and extraction of lithium compounds have attracted the attention of the lithium resource development industry. Internationally, the trend in lithium salt production is to primarily extract lithium from salt lakes, supplemented by ore extraction. In my country, lithium extraction from salt lake brine offers advantages such as abundant resources and low cost. Furthermore, with the increasing depletion of solid lithium ore resources, salt lake brine has gradually become a major source of lithium. Currently, the mainstream processes for lithium extraction from high magnesium-to-lithium ratio salt lakes mainly include: salt field processing, magnesium-lithium separation, impurity removal from lithium-containing solutions, and lithium carbonate precipitation conversion. Lithium carbonate precipitation conversion involves adding sodium carbonate solution to a lithium-rich solution to prepare lithium carbonate through a precipitation reaction. The solution after solid-liquid separation is called lithium carbonate mother liquor. The lithium content in the mother liquor is still 1-2 g / L, and the carbonate content is 15-25 g / L, representing important lithium and carbonate resources. Currently, the lithium carbonate mother liquor from salt lakes is mostly wasted and piled up, and its comprehensive utilization is not well achieved.
[0003] Currently, the mainstream carbon dioxide capture technologies include liquid-phase absorption and solid-phase adsorption. Liquid amine absorption is the main method for industrial-scale carbon dioxide capture, and while it is technologically mature and has high practical value, its high energy consumption, the corrosiveness of amine solvents, and the resulting secondary pollution are significant concerns. Solid-phase adsorption is a second-generation carbon dioxide capture technology based on solid adsorbent materials. Based on the operating temperature of the adsorbent, solid carbon dioxide adsorbents can be classified into three types: high-temperature adsorbents (>400℃), medium-temperature adsorbents (200-400℃), and low-temperature adsorbents (<200℃). Compared to liquid-phase absorption, solid-phase adsorption offers lower energy consumption, lower pollution, and lower cost. However, due to its later development and lower technological maturity, its large-scale industrial application requires further research and verification.
[0004] The utilization of carbonate-type brine and lithium precipitation mother liquor in the existing technology has the following problems: (1) The existing utilization method of lithium extraction mother liquor from brine is complicated. It is necessary to first remove carbonate ions with hydrochloric acid and then add alkali to adjust its pH, which consumes acid and alkali. The lithium evaporation and concentration process has high energy consumption and high cost; (2) Currently, carbon dioxide capture and storage requires a two-step method. Most of the mineralized carbon dioxide is stored and cannot be utilized, which is costly and has a long process flow; (3) There are no reports on using lithium carbonate mother liquor to capture carbon dioxide and extract lithium resources from lithium carbonate mother liquor; (4) There are no reports on using ion membrane electrolysis and bipolar membrane electrolysis to provide an alkaline environment to capture carbon dioxide and co-produce battery-grade lithium carbonate. Summary of the Invention
[0005] The main objective of this invention is to provide a method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine, thereby overcoming the shortcomings of the prior art.
[0006] To achieve the aforementioned objectives, the technical solution adopted by this invention includes: This invention provides a method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine, comprising: The carbonate brine is pretreated and then separated by nanofiltration using a membrane separation system to obtain a lithium-containing solution and a carbonate-containing concentrate; wherein the carbonate brine includes carbonate-type salt lake raw brine and / or lithium carbonate precipitation mother liquor; The lithium-rich solution was concentrated using a forward osmosis system to obtain a primary concentrate and forward osmosis desalinated water. The primary concentrate is subjected to secondary concentration treatment using a high-pressure reverse osmosis system to obtain a secondary concentrated lithium-rich solution and reverse osmosis desalinated water. The secondary concentrated lithium-rich solution is subjected to ion-exchange membrane electrolysis or bipolar membrane electrolysis to maintain the solution in an alkaline environment, while lithium ions in the solution are enriched to obtain an alkaline lithium-rich solution. Furthermore, carbon dioxide gas is introduced into the alkaline lithium-rich solution to carry out a co-precipitation reaction for nucleation, aging, filtration, washing, and drying to obtain battery-grade lithium carbonate product.
[0007] Compared with existing technologies, the advantages of this invention are as follows: This invention uses carbonate-type brine and lithium carbonate mother liquor as raw materials, and employs a nanofiltration-forward osmosis primary concentration-high-pressure reverse osmosis secondary concentration-electrolysis-carbon dioxide mineralization-battery-grade lithium carbonate crystallization control technology to extract lithium and capture carbon dioxide from carbonate-type brine and lithium carbonate mother liquor to prepare battery-grade lithium carbonate. This achieves efficient and comprehensive recovery and utilization of lithium and hydroxide ions in carbonate-type brine and lithium carbonate mother liquor. The use of electrolysis provides an alkaline system for capturing carbon dioxide, avoiding the addition of chemical raw materials such as sodium hydroxide. Using carbon dioxide as a raw material to prepare battery-grade lithium carbonate avoids the addition of sodium carbonate chemical reagents, simplifying the process flow of carbon dioxide capture and storage and battery-grade lithium carbonate preparation, and reducing the production cost of capturing and mineralizing carbon dioxide to co-produce lithium carbonate. This technology has the advantages of being green, efficient, energy-saving, low-investment, low-energy consumption, and low-pollution. Furthermore, the process equipment is simple, the operation process is short, and it is easy to control, making it suitable for industrial-scale promotion. Attached Figure Description
[0008] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0009] Figure 1 This is a process flow diagram of a typical embodiment of the present invention, which utilizes carbonate brine to capture mineralized carbon dioxide and co-produce battery-grade lithium carbonate. Detailed Implementation
[0010] Specifically, as one aspect of the technical solution of this invention, a method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine includes: The carbonate brine is pretreated and then separated by nanofiltration using a membrane separation system to obtain a lithium-containing solution and a carbonate-containing concentrate; wherein the carbonate brine includes carbonate-type salt lake raw brine and / or lithium carbonate precipitation mother liquor; The lithium-rich solution was concentrated using a forward osmosis system to obtain a primary concentrate and forward osmosis desalinated water. The primary concentrate is subjected to secondary concentration treatment using a high-pressure reverse osmosis system to obtain a secondary concentrated lithium-rich solution and reverse osmosis desalinated water. The secondary concentrated lithium-rich solution is subjected to ion-exchange membrane electrolysis or bipolar membrane electrolysis to maintain the solution in an alkaline environment, while lithium ions in the solution are enriched to obtain an alkaline lithium-rich solution. Furthermore, carbon dioxide gas is introduced into the alkaline lithium-rich solution to carry out a co-precipitation reaction for nucleation, aging, filtration, washing, and drying to obtain battery-grade lithium carbonate product.
[0011] In some preferred embodiments, the method specifically includes: Pretreatment of carbonate brine removes mud, sand and organic impurities to obtain pretreated brine. The pretreated brine is diluted to obtain diluted brine; Furthermore, the diluted brine is introduced into a membrane separation system for the separation of carbonate and lithium to obtain a lithium-containing solution and a carbonate-containing concentrate; wherein the carbonate-containing concentrate is discharged into the salt field for subsequent use.
[0012] Furthermore, the lithium ion concentration in the raw brine of the carbonate-type salt lake is 0.7~2.0 g / L, and the carbonate concentration is 30~40 g / L.
[0013] Furthermore, the lithium ion concentration in the lithium carbonate precipitation mother liquor is 1~3.0 g / L, and the carbonate concentration is 15~25 g / L.
[0014] Furthermore, the pretreatment includes, but is not limited to, any one of ultrafiltration, ceramic filtration, and polyceramic membrane filtration.
[0015] Furthermore, the turbidity of the pretreated brine is less than 3 NTU.
[0016] Furthermore, when the carbonate brine is the original brine of a carbonate salt lake, the lithium concentration in the diluted brine is 0.07~0.25g / L, the carbonate concentration is 3~8g / L, and the sulfate concentration is 0.7~1.5g / L.
[0017] Furthermore, when the carbonate-type brine is a lithium carbonate precipitation mother liquor, the lithium concentration in the diluted brine is 0.06~0.5 g / L, and the carbonate concentration is 1~5 g / L.
[0018] Furthermore, the membrane separation system includes a nanofiltration separation unit, which is a multi-stage nanofiltration system. The nanofiltration separation unit adopts a multi-stage, multi-segment series configuration. The nanofiltration membrane used in the membrane separation system is any one or more combinations of DK membranes, DL membranes, and NF membranes, and is not limited thereto.
[0019] Furthermore, the nanofiltration membrane ratio between different segments of the nanofiltration separation unit in the membrane separation system is in the range of 1:1 to 7:1, preferably 2:1 to 5:1.
[0020] Furthermore, the operating pressure of the nanofiltration separation unit in the membrane separation system is 0.5~5.0MPa, preferably 3.0~4.0MPa.
[0021] Furthermore, the lithium-containing solution (nanofiltration desalination) contains 0.5~1.5 g / L of lithium ions.
[0022] In some preferred embodiments, the lithium ion concentration in the primary concentrate is 2~5.0 g / L and the carbonate concentration is 0.01~0.5 g / L.
[0023] In some preferred embodiments, the forward osmosis draw solution used in the forward osmosis system includes, but is not limited to, a saturated magnesium chloride or saturated sodium chloride solution prepared from magnesium chloride or sodium chloride from a brine lake.
[0024] In some preferred embodiments, the forward osmosis freshwater is used for diluting carbonate-type brine.
[0025] In some preferred embodiments, the lithium ion content in the forward osmosis freshwater is 0.005~0.10 g / L.
[0026] In some preferred embodiments, the volume ratio of the forward osmosis desalination water to the primary concentrate is 2.0:1 to 4:1.
[0027] In some preferred embodiments, the forward osmosis system uses a forward osmosis membrane including a CTA membrane and / or a TFC membrane, but is not limited thereto.
[0028] In some preferred embodiments, the secondary concentration unit in the high-pressure reverse osmosis system is in the form of two stages connected in series, each stage containing a different number of reverse osmosis membranes, and the ratio of reverse osmosis membranes between different stages is 1:1 to 7:1; the operating pressure in the secondary concentration unit process is 1.0 to 10.0 MPa.
[0029] In some preferred embodiments, the lithium ion content in the secondary concentrated lithium-rich solution is 5~10 g / L.
[0030] In some preferred embodiments, the lithium ion content in the reverse osmosis freshwater is 0.005~0.10 g / L.
[0031] In some preferred embodiments, the volume ratio of the secondary concentrated lithium-rich solution to the primary concentrated solution is 0.5:1 to 6:1.
[0032] In some preferred embodiments, the reverse osmosis membranes used in the high-pressure reverse osmosis system include, but are not limited to, Dow BW membranes and / or SW membranes.
[0033] In some preferred embodiments, the method specifically includes: The secondary concentrated lithium-rich solution is electrolyzed using an electrolysis system to maintain the pH value of the solution between 10 and 14, while lithium ions are enriched in the solution to obtain an alkaline lithium-rich solution. Furthermore, carbon dioxide gas is introduced into the alkaline lithium-rich solution, and a dispersant is added simultaneously. The co-precipitation reaction is carried out under the conditions of pH value of 10-14, ultrasonic frequency of 10-50 kHz, ultrasonic power of 100-1000 W, stirring speed of 50-200 rpm, and reaction temperature of 80-110°C. The resulting products are then aged, filtered, washed, and dried to obtain battery-grade lithium carbonate.
[0034] Furthermore, the alkaline lithium-rich solution Li + The concentration is 10~20 g / L.
[0035] Furthermore, the carbon dioxide gas originates from the carbon dioxide flue gas emitted by the combustion of natural gas boilers or coal boilers powered by the salt lake enterprise.
[0036] Furthermore, the flow rate of the carbon dioxide gas introduced is 0.5~10 L / min.
[0037] Furthermore, the carbon dioxide gas is introduced for 20 to 50 minutes.
[0038] Furthermore, the carbon dioxide gas is introduced into the alkaline lithium-rich solution via an aeration device.
[0039] Furthermore, the dispersant includes polyethylene glycol and / or ethanol dispersants.
[0040] Furthermore, the coprecipitation reaction takes 40 to 90 minutes.
[0041] Furthermore, the aging time is 20-40 minutes.
[0042] In some preferred embodiments, the main content of the battery-grade lithium carbonate product is lithium carbonate ≥ 99.5 wt%, Cl - ≤40ppm, Na + ≤150ppm, Mg 2+ ≤90ppm, Ca 2+ ≤50ppm, particle size less than 8μm.
[0043] The process flow diagram of the present invention for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine is as follows: Figure 1As shown, the process steps are as follows: Dilute the raw brine of a carbonate-type salt lake and the lithium-precipitated mother liquor to obtain diluted brine. Separate carbonate and lithium ions from the diluted brine using a membrane separation system to obtain a lithium-containing solution. Perform a first-stage forward osmosis concentration treatment on the lithium-containing solution to obtain a first-stage concentrate and forward osmosis desalinated water. Perform a second-stage high-pressure reverse osmosis concentration treatment on the first-stage concentrate to obtain a second-stage concentrated lithium-rich solution and reverse osmosis desalinated water. Electrolyze the second-stage concentrate, continuously maintaining an alkaline environment. Introduce carbon dioxide gas at a certain pressure into the alkaline solution to capture carbon dioxide and prepare battery-grade lithium carbonate.
[0044] In some preferred embodiments, the method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine includes: (1) Nanofiltration method for separating carbonate and lithium After pretreatment, the raw brine of carbonate-type salt lake and lithium precipitation mother liquor are diluted to obtain diluted brine. The diluted brine is then separated from lithium by a membrane separation system to obtain a lithium-containing solution and a carbonate-containing concentrate. The lithium-containing solution enters the next process, while the carbonate-containing brine is discharged to the salt field for comprehensive recycling.
[0045] (2) Forward osmosis first-stage concentration The lithium-containing solution obtained above enters the forward osmosis system for primary concentration to obtain primary concentrate and forward osmosis freshwater, which are then used in the next stage of the process and returned for dilution of raw brine and lithium precipitation mother liquor in carbonate-type salt lakes, respectively.
[0046] (3) High-pressure reverse osmosis secondary concentration The primary concentrate obtained in the previous step enters the high-pressure reverse osmosis system for secondary concentration to obtain a secondary concentrated lithium-rich solution and reverse osmosis desalination. The secondary concentrate then enters the next stage of the process, while the reverse osmosis desalination is blended with the lithium-containing solution after nanofiltration. The residual lithium is then recovered and the desalination is reused through the forward osmosis system.
[0047] (4) Preparation of alkaline solution by electrolysis The secondary concentrate obtained in the previous step is then subjected to ion-exchange membrane electrolysis or bipolar membrane electrolysis to maintain an alkaline environment in the solution.
[0048] (5) Carbon dioxide capture and co-production of battery-grade lithium carbonate A certain flow rate of carbon dioxide gas is introduced into the above solution, and a co-precipitation reaction is carried out under certain pH, ultrasonic, and temperature conditions. After nucleation, aging, filtration, washing, and drying, a solid lithium carbonate product is obtained.
[0049] In some more specific embodiments, the method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine includes: (1) Nanofiltration method for separating carbonate and lithium The raw brine of carbonate-type salt lake and lithium precipitation mother liquor are diluted after pretreatment to obtain diluted brine. The pretreatment removes impurities such as mud and organic matter. The carbonate and lithium are separated through a membrane separation system to obtain lithium-containing solution and carbonate-containing concentrate. The lithium-containing solution enters the next process, while the carbonate-containing brine is discharged to the salt field for comprehensive recycling. The lithium concentration in the raw brine of the carbonate-type salt lake is 0.7~2.0 g / L, and the carbonate concentration is 30~40 g / L; the lithium carbonate precipitation mother liquor has a lithium concentration of 1~3.0 g / L and a carbonate concentration of 15~25 g / L; the pretreatment is one of ultrafiltration, ceramic filtration or polyceramic membrane filtration, and the turbidity of the brine after pretreatment is less than 3 NTU; the lithium concentration in the diluted raw brine of the carbonate type is 0.07~0.25 g / L, the carbonate concentration is 3~8 g / L, and the sulfate concentration is 0.7~1.5 g / L; the lithium carbonate precipitation mother liquor has a lithium concentration of 0.06~0.5 g / L and a carbonate concentration of 1~5 g / L. The nanofiltration separation unit is a multi-stage nanofiltration system. After dilution, the solution undergoes primary nanofiltration, and the permeate then enters the secondary nanofiltration process to further reduce the ratio of divalent ions (such as carbonate) to monovalent ions in the permeate, thereby increasing the lithium-ion concentration. After secondary nanofiltration, the permeate continues into the next stage of nanofiltration to further increase the lithium-ion concentration, and so on, until the carbonate concentration in the solution is reduced to below 0.1 g / L. Each stage of nanofiltration has two key components, meaning the separation unit adopts a multi-stage, multi-segment series configuration. The resulting lithium-containing solution enters the next stage of the process. The nanofiltration membrane ratio between different stages of the separation unit ranges from 1:1 to 7:1, preferably from 2:1 to 5:1. The operating pressure of the separation unit is 0.5 to 5.0 MPa, preferably 3.0 to 4.0 MPa. The lithium-ion content in the nanofiltration permeate is 0.5 to 1.5 g / L. The nanofiltration membrane used is one or two of DK, DL, and NF membranes.
[0050] (2) Forward osmosis first-stage concentration The lithium-containing solution obtained above enters the forward osmosis system for primary concentration, obtaining primary concentrate and forward osmosis desalination water, which are respectively used in the next stage process and returned for dilution of raw brine and lithium precipitation mother liquor from carbonate-type brine lakes. The lithium concentration in the primary concentrate is 2~5.0 g / L, and the carbonate concentration is 0.01~0.5 g / L. The forward osmosis draw solution is a saturated magnesium chloride or saturated sodium chloride solution prepared from magnesium chloride or sodium chloride from the brine lake. The forward osmosis desalination water is returned to the nanofiltration separation system as dilution water, with a lithium ion content of 0.005~0.10 g / L and a concentration-to-volume ratio of 2.0:1~4:1. The forward osmosis membrane is one or both of CTA membrane and TFC membrane.
[0051] (3) High-pressure reverse osmosis secondary concentration The primary concentrate obtained in the previous step enters a high-pressure reverse osmosis system for secondary concentration, yielding a secondary concentrated lithium-rich solution and reverse osmosis desalination. The secondary concentrate then proceeds to the next stage, while the reverse osmosis desalination is blended with the nanofiltration lithium-containing solution. Residual lithium is recovered and the desalination is reused via a forward osmosis system. The secondary concentration unit employs a two-stage series configuration, with each stage containing a different number of reverse osmosis membranes. The membrane ratio between different stages ranges from 1:1 to 7:1. After secondary concentration via high-pressure reverse osmosis, the lithium ion content in the reverse osmosis concentrate (secondary concentrated lithium-rich solution) is 5–10 g / L; the lithium ion content in the reverse osmosis desalination is 0.005–0.10 g / L; the concentration volume ratio (secondary concentrated lithium-rich solution / primary concentrate) is 0.5:1–6:1; the operating pressure in the secondary concentration unit is 1.0–10.0 MPa; and the reverse osmosis membrane is one or both of Dow BW or SW membranes.
[0052] (4) Preparation of alkaline solution by electrolysis The secondary concentrate obtained in the previous step is electrolyzed to maintain an alkaline environment. The electrolysis system is either an ion-exchange membrane electrolysis system or a bipolar membrane electrolysis system. Under certain voltage conditions, the electrolysis system maintains an alkaline environment by obtaining hydroxide ions, while simultaneously enriching lithium ions. This alkaline environment is defined as a pH value between 10 and 14. After enrichment, the Li ions in the solution... + The ion content is 10~20g / L.
[0053] (5) Carbon dioxide capture and co-production of battery-grade lithium carbonate A certain flow rate of carbon dioxide gas is introduced into the above-mentioned lithium enrichment solution, and a co-precipitation reaction is carried out under specific pH, ultrasonic, dispersant, and temperature conditions. Battery-grade lithium carbonate product is obtained through nucleation, aging, filtration, washing, and drying. The carbon dioxide is flue gas emitted from the combustion of natural gas boilers or coal-fired boilers in salt lake enterprises, with a flow rate of 0.5-10 L / min. The carbon dioxide is introduced into the alkaline lithium-rich solution via an aeration device; the reaction pH is controlled between 10 and 14; the ultrasonic frequency is 10-50 kHz, and the ultrasonic power is 100-1000 W; the dispersant includes polyethylene glycol and / or ethanol dispersants; the stirring rate is 50-200 rpm; the reaction temperature is 80-110℃; the reaction time is 40-90 min, including a feeding time (carbon dioxide introduction time) of 20-50 min and an aging time of 20-40 min. After the reaction, the product is filtered, washed, and dried to obtain battery-grade lithium carbonate product. The prepared lithium carbonate has a main content ≥99.5%, Cl... - ≤40ppm, Na + ≤150 ppm, Mg 2+ ≤90 ppm, Ca 2 + ≤50 ppm, particle size less than 8μm.
[0054] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides detailed implementation methods and specific operation processes. However, the protection scope of the present invention is not limited to the following embodiments.
[0055] Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.
[0056] Example 1 The lithium carbonate mother liquor used in this embodiment is from the lithium extraction mother liquor of a salt lake in Qinghai Province. The mother liquor contains Li... + The concentration is 3 g / L, CO3 2- The concentration was 25 g / L. After dilution, 5 L of the lithium precipitation mother liquor was pretreated via ultrafiltration, resulting in a lithium ion concentration of 0.5 g / L and a CO3 concentration of... 2- The concentration was 5 g / L. After pretreatment, the solution entered a nanofiltration system equipped with DK membranes for the separation of divalent ions such as carbonate from lithium, obtaining a nanofiltration lithium-containing dilute solution and a nanofiltration low-lithium carbonate-containing concentrated solution. The operating pressure was 0.5 MPa, and the nanofiltration membrane ratio between different stages was 1:1. The lithium ion content in the lithium-containing dilute solution was 1.5 g / L, and the carbonate concentration was reduced to below 0.08 g / L. The lithium-containing dilute solution entered a forward osmosis primary concentration system. The forward osmosis draw solution was a saturated solution of sodium chloride prepared from a salt lake. The lithium-containing dilute solution was concentrated to 2 g / L via CTA membrane forward osmosis to obtain a primary concentrate. The carbonate concentration in the primary concentrate was 0.01 g / L, and the lithium concentration in the dilute solution was controlled at 0.005 g / L. The volume ratio of dilute solution to primary concentrate was 2:1. The primary concentrate enters the high-pressure reverse osmosis system for secondary concentration, resulting in a lithium ion content of 5 g / L in the secondary concentrate; the lithium ion content in the secondary desalination is 0.10 g / L. The reverse osmosis system uses Dow BW series reverse osmosis membranes, with a 1:1 ratio of primary and secondary membranes. The inlet pressure is controlled at 1 MPa, and the concentration volume ratio (secondary concentrate / primary concentrate) is 2. The obtained high-pressure reverse osmosis desalination is directly mixed with nanofiltration desalination. A secondary concentration lithium-ion membrane electrolysis system raises the solution pH to 10 and concentrates the lithium-ion content to 10 g / L, obtaining an alkaline lithium-rich solution. The alkaline lithium-rich solution is heated to 80°C, and carbon dioxide from the natural gas boiler of the salt lake enterprise is introduced into it at a flow rate of 0.5 L / min through an aeration device for 20 minutes. A precipitation reaction is carried out at a stirring speed of 50 rpm, and during the nucleation stage, a 10 kHz, 100 W ultrasonic wave is activated for 10 minutes. A small amount of polyethylene glycol dispersant is added during the reaction. After the reaction, the solution is filtered, washed, and dried to obtain battery-grade lithium carbonate with a lithium carbonate content of not less than 99.5%. - ≤40ppm, Na+ ≤150 ppm, Mg 2+ ≤90 ppm, Ca 2+ ≤50 ppm. Battery-grade lithium carbonate particle size: 8 μm.
[0057] Example 2 The lithium carbonate mother liquor used in this embodiment is derived from the raw brine of a carbonate-type salt lake in Tibet. The raw brine contains 0.7 g / L lithium and 30 g / L carbonate ions. After dilution, 5 L of the raw brine solution is pretreated using a ceramic filtration system, resulting in a lithium ion concentration of 0.07 g / L and a CO3 concentration of... 2- The concentration was 3 g / L. After pretreatment, the solution entered a nanofiltration system equipped with a DL membrane for the separation of divalent ions such as carbonate from lithium, obtaining a nanofiltration lithium-containing dilute solution and a nanofiltration low-lithium carbonate-containing concentrated solution. The operating pressure was 5 MPa, and the nanofiltration membrane ratio between different stages was 7:1. The lithium ion content in the lithium-containing dilute solution was 0.5 g / L, and the carbonate concentration was reduced to below 0.06 g / L. The lithium-containing dilute solution entered a forward osmosis primary concentration system. The forward osmosis draw solution was a saturated solution of sodium chloride prepared from a salt lake. The lithium-containing dilute solution was concentrated to 5 g / L via TFC membrane forward osmosis to obtain a primary concentrate. The carbonate concentration in the primary concentrate was 0.5 g / L, and the lithium concentration in the dilute solution was controlled at 0.10 g / L. The volume ratio of dilute solution to primary concentrate was 4:1. The primary concentrate enters the high-pressure reverse osmosis system for secondary concentration, resulting in a lithium ion content of 10 g / L in the secondary concentrate and a lithium ion content of 0.005 g / L in the secondary desalination. The reverse osmosis system uses Dow SW series membranes, with a 7:1 ratio of primary to secondary membranes. The inlet pressure is controlled at 10 MPa, and the concentration volume ratio (secondary concentrate / primary concentrate) is 0.5:1. The obtained high-pressure reverse osmosis desalination is directly mixed with nanofiltration desalination. A secondary concentration ion-exchange membrane electrolysis system raises the solution pH to 14 and concentrates the lithium ion content to 20 g / L, obtaining an alkaline lithium-rich solution. The alkaline lithium-rich solution is heated to 110°C, and carbon dioxide from a coal-fired boiler supplied by a salt lake enterprise is introduced into it at a flow rate of 10 L / min via an aeration device for 50 min. A precipitation reaction is initiated with stirring at 200 rpm, and during the nucleation stage, a 50 kHz, 1000 W ultrasonic wave is activated for 10 min. A small amount of ethanol dispersant is added during the reaction. After the reaction, the solution is filtered, washed, and dried to obtain battery-grade lithium carbonate with a lithium carbonate content of not less than 99.5%. - ≤40ppm, Na + ≤150 ppm, Mg 2+ ≤90 ppm, Ca 2+ ≤50 ppm. Battery-grade lithium carbonate particle size: 6 μm.
[0058] Example 3 The lithium carbonate mother liquor used in this embodiment is from the lithium extraction mother liquor of a salt lake in Qinghai Province. The mother liquor contains Li... + The concentration is 1 g / L, CO3 2- The concentration was 15 g / L. After dilution, 5 L of the lithium precipitation mother liquor was passed through a polyceramic membrane pretreatment system, where the lithium ion concentration was 0.06 g / L and CO3 concentration was [not specified]. 2- Concentration 1 g / L.
[0059] After pretreatment, the solution enters a nanofiltration system equipped with an NF membrane for the separation of divalent ions such as carbonate from lithium, yielding a nanofiltration solution containing lithium and a nanofiltration concentrate containing low lithium and carbonate. The operating pressure is 3 MPa, and the nanofiltration membrane ratio between different stages is 2:1. The lithium ion content in the lithium-containing dilute solution is 1.0 g / L, and the carbonate concentration is reduced to below 0.09 g / L. The lithium-containing dilute solution then enters a forward osmosis primary concentration system. The forward osmosis draw solution is a saturated solution of sodium chloride prepared from a brine lake. The lithium-containing dilute solution is concentrated to 3 g / L via CTA membrane forward osmosis to obtain a primary concentrate. The primary concentrate contains 0.05 g / L carbonate, and the lithium concentration in the dilute solution is controlled at 0.01 g / L. The volume ratio of dilute solution to primary concentrate is 3:1. The primary concentrate enters the high-pressure reverse osmosis system for secondary concentration, resulting in a lithium ion content of 8 g / L in the secondary concentrate and a lithium ion content of 0.05 g / L in the secondary desalination. The reverse osmosis system uses Dow BW series reverse osmosis membranes, with a 4:1 ratio of primary to secondary membranes. The inlet pressure is controlled at 5 MPa, and the concentration volume ratio (secondary concentrate / primary concentrate) is 6:1. The obtained high-pressure reverse osmosis desalination is directly mixed with nanofiltration desalination. A secondary concentration ion-exchange membrane electrolysis system raises the solution pH to 12 and concentrates the lithium ion content to 15 g / L, obtaining an alkaline lithium-rich solution. The alkaline lithium-rich solution is heated to 100°C, and carbon dioxide from the natural gas boiler of the salt lake enterprise is introduced into it at a flow rate of 5 L / min via an aeration device for 30 minutes. A precipitation reaction is initiated at 100 rpm, and during the nucleation stage, a 20 kHz, 500 W ultrasonic wave is activated for 20 minutes. A small amount of polyethylene glycol dispersant is added during the reaction. After the reaction, the solution is filtered, washed, and dried to obtain battery-grade lithium carbonate with a lithium carbonate content of not less than 99.5%. - ≤40ppm, Na + ≤150 ppm, Mg 2+ ≤90 ppm, Ca 2+ ≤50 ppm. Battery-grade lithium carbonate particle size: 5 μm.
[0060] Example 4 The lithium carbonate mother liquor used in this embodiment is derived from the raw brine of a carbonate-type salt lake in Tibet. The raw brine contains 2.0 g / L lithium and 40 g / L carbonate ions. After dilution, 5 L of the raw brine solution is pretreated using a ceramic filtration system, resulting in a lithium ion concentration of 0.25 g / L and a CO3 concentration of... 2- The concentration was 8 g / L. After pretreatment, the solution entered a nanofiltration system equipped with a DL membrane for the separation of divalent ions such as carbonate from lithium, obtaining a nanofiltration lithium-containing dilute aqueous solution and a nanofiltration low-lithium carbonate-containing concentrated solution. The operating pressure was 4 MPa, and the nanofiltration membrane ratio between different stages was 5:1. The lithium ion content in the lithium-containing dilute aqueous solution was 0.8 g / L, and the carbonate concentration was reduced to below 0.05 g / L. The lithium-containing dilute aqueous solution entered a forward osmosis primary concentration system. The forward osmosis draw solution was a saturated solution of sodium chloride prepared from a salt lake. The lithium-containing dilute aqueous solution was concentrated to 4 g / L via TFC membrane forward osmosis to obtain a primary concentrate. The carbonate concentration in the primary concentrate was 0.4 g / L, and the lithium concentration in the dilute solution was controlled at 0.08 g / L. The volume ratio of dilute solution to primary concentrate was 2.5:1. The primary concentrate enters the high-pressure reverse osmosis system for secondary concentration, resulting in a lithium ion content of 7 g / L in the secondary concentrate; the lithium ion content in the secondary desalination is 0.08 g / L. The reverse osmosis system uses Dow SW series reverse osmosis membranes, with a 7:1 ratio of primary to secondary membranes. The inlet pressure is controlled at 7 MPa, and the concentration volume ratio (secondary concentrate / primary concentrate) is 4:1. The obtained high-pressure reverse osmosis desalination is directly mixed with nanofiltration desalination. A secondary concentration ion-exchange membrane electrolysis system raises the solution pH to 12 and concentrates the lithium-ion content to 18 g / L, obtaining an alkaline lithium-rich solution. The alkaline lithium-rich solution is heated to 90°C, and carbon dioxide from a coal-fired boiler supplied by a salt lake enterprise is introduced into it at a flow rate of 7 L / min via an aeration device for 40 minutes. A precipitation reaction is initiated with stirring at 150 rpm, and during the nucleation stage, a 30 kHz, 800 W ultrasonic wave is activated for 30 minutes. A small amount of ethanol dispersant is added during the reaction. After the reaction, the solution is filtered, washed, and dried to obtain battery-grade lithium carbonate with a lithium carbonate content of not less than 99.5%. - ≤40ppm, Na + ≤150 ppm, Mg 2+ ≤90 ppm, Ca 2+ ≤50 ppm. Battery-grade lithium carbonate particle size: 5 μm.
[0061] In addition, the applicant also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.
[0062] It should be understood that the technical solutions of the present invention are not limited to the specific embodiments described above. Any technical modifications made to the technical solutions of the present invention without departing from the spirit and scope of the claims are within the scope of protection of the present invention.
Claims
1. A method for capturing mineralized carbon dioxide and co-producing battery-grade lithium carbonate using carbonate-type brine, characterized in that, include: The carbonate brine is pretreated and then separated by nanofiltration using a membrane separation system to obtain a lithium-containing solution and a carbonate-containing concentrate; wherein the carbonate brine includes carbonate-type salt lake raw brine and / or lithium carbonate precipitation mother liquor; The lithium-rich solution was concentrated using a forward osmosis system to obtain a primary concentrate and forward osmosis desalinated water. The primary concentrate is subjected to secondary concentration treatment using a high-pressure reverse osmosis system to obtain a secondary concentrated lithium-rich solution and reverse osmosis desalinated water. The secondary concentrated lithium-rich solution is subjected to ion-exchange membrane electrolysis or bipolar membrane electrolysis to maintain the solution in an alkaline environment, while lithium ions in the solution are enriched to obtain an alkaline lithium-rich solution. Furthermore, carbon dioxide gas is introduced into the alkaline lithium-rich solution to carry out a co-precipitation reaction for nucleation, aging, filtration, washing, and drying to obtain battery-grade lithium carbonate product.
2. The method according to claim 1, characterized in that, Specifically, it includes: Pretreatment of carbonate brine removes mud, sand and organic impurities to obtain pretreated brine. The pretreated brine is diluted to obtain diluted brine; Furthermore, the diluted brine is introduced into a membrane separation system for the separation of carbonate and lithium to obtain a lithium-containing solution and a carbonate-containing concentrate; wherein the carbonate-containing concentrate is discharged into the salt field for subsequent use.
3. The method according to claim 2, characterized in that: The lithium ion concentration in the raw brine of the carbonate-type salt lake is 0.7~2.0 g / L, and the carbonate concentration is 30~40 g / L; And / or, the lithium ion concentration in the lithium carbonate precipitation mother liquor is 1~3.0 g / L, and the carbonate concentration is 15~25 g / L; And / or, the pretreatment includes any one of ultrafiltration, ceramic filtration, and polyceramic membrane filtration; And / or, the turbidity of the pretreated brine is less than 3 NTU; And / or, when the carbonate brine is the original brine of a carbonate salt lake, the lithium concentration in the diluted brine is 0.07~0.25 g / L, the carbonate concentration is 3~8 g / L, and the sulfate concentration is 0.7~1.5 g / L; And / or, when the carbonate brine is a lithium carbonate precipitation mother liquor, the lithium concentration in the diluted brine is 0.06~0.5 g / L and the carbonate concentration is 1~5 g / L.
4. The method according to claim 2, characterized in that: The membrane separation system includes a nanofiltration separation unit, which is a multi-stage nanofiltration system. The nanofiltration separation unit adopts a multi-stage, multi-segment series configuration. The nanofiltration membrane used in the membrane separation system is any one or a combination of DK membrane, DL membrane, and NF membrane. And / or, the nanofiltration membrane ratio between different segments of the nanofiltration separation unit in the membrane separation system is in the range of 1:1 to 7:1, preferably 2:1 to 5:1; And / or, the operating pressure of the nanofiltration separation unit in the membrane separation system is 0.5~5.0MPa, preferably 3.0~4.0MPa; And / or, the lithium ion content in the lithium-containing solution is 0.5~1.5 g / L.
5. The method according to claim 1, characterized in that: The lithium ion concentration in the primary concentrate is 2~5.0 g / L, and the carbonate concentration is 0.01~0.5 g / L. And / or, the forward osmosis draw solution used in the forward osmosis system includes a saturated magnesium chloride or saturated sodium chloride solution prepared from magnesium chloride or sodium chloride from a salt lake. And / or, the forward osmosis freshwater is used for dilution of carbonate-type brine; And / or, the lithium ion content in the forward osmosis freshwater is 0.005~0.10 g / L; And / or, the volume ratio of the primary concentrate to forward osmosis desalination water is 2.0:1 to 4:1; And / or, the forward osmosis system uses forward osmosis membranes including CTA membranes and / or TFC membranes.
6. The method according to claim 1, characterized in that: The secondary concentration unit in the high-pressure reverse osmosis system is arranged in two series, each containing a different number of reverse osmosis membranes. The ratio of reverse osmosis membranes between different numbers of sections is 1:1 to 7:
1. The operating pressure in the secondary concentration unit process is 1.0 to 10.0 MPa. And / or, the lithium ion content in the secondary concentrated lithium-rich solution is 5~10 g / L; And / or, the lithium ion content in the reverse osmosis desalination water is 0.005~0.10 g / L; And / or, the concentration volume ratio of the secondary concentrated lithium-rich solution to the primary concentrated solution is 0.5:1 to 6:1; And / or, the reverse osmosis membranes used in the high-pressure reverse osmosis system include Dow BW membranes and / or SW membranes.
7. The method according to claim 1, characterized in that, Specifically, it includes: The secondary concentrated lithium-rich solution is electrolyzed using an electrolysis system to maintain the pH value of the solution between 10 and 14, while lithium ions are enriched in the solution to obtain an alkaline lithium-rich solution. Furthermore, carbon dioxide gas is introduced into the alkaline lithium-rich solution, and a dispersant is added simultaneously. The co-precipitation reaction is carried out under the conditions of pH value of 10-14, ultrasonic frequency of 10-50 kHz, ultrasonic power of 100-1000 W, stirring speed of 50-200 rpm, and reaction temperature of 80-110°C. The resulting products are then aged, filtered, washed, and dried to obtain battery-grade lithium carbonate.
8. The method according to claim 7, characterized in that: The alkaline lithium-rich solution Li + The concentration is 10~20 g / L.
9. The method according to claim 7, characterized in that: The carbon dioxide gas originates from the carbon dioxide flue gas emitted by the combustion of natural gas boilers or coal boilers used for power supply in salt lake enterprises. And / or, the flow rate of the carbon dioxide gas introduced is 0.5~10 L / min; And / or, the carbon dioxide gas is introduced for 20 to 50 minutes; And / or, the carbon dioxide gas is introduced into the alkaline lithium-rich solution via an aeration device; and / or, the dispersant includes polyethylene glycol and / or ethanol dispersant; And / or, the coprecipitation reaction takes 40 to 90 minutes; And / or, the aging time is 20-40 minutes.