A method for preparing a component-in-situ interfacial polymerization hollow fiber reverse osmosis membrane

By forming a polyamide separation layer in hollow fiber reverse osmosis membranes through in-situ interfacial polymerization of components, the problems of mechanical damage and uneven performance in existing technologies are solved, and the simultaneous improvement of high desalination rate and high water flux is achieved.

CN123102165APending Publication Date: 2026-11-17AROMEM PTE LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611607095.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies make it difficult to simultaneously achieve high water flux and high desalination rate in the preparation of hollow fiber reverse osmosis membranes, and the internal surface polymerization method carries the risk of mechanical damage, affecting the yield and performance consistency.

Method used

Hollow fiber-based membrane fibers were prepared by dry-wet spinning of PES casting solution using an in-situ interfacial polymerization method. The fibers were combined with an aqueous mixture of aminated carbon quantum dots, microporous polymers and m-phenylenediamine, and polyamide separation layer was formed in the hollow fiber-supported membrane module through in-situ diffusion interfacial polymerization to avoid mechanical damage. The network density and free volume were improved through hydrogen bonding and covalent crosslinking.

Benefits of technology

It achieves uniform and controllable desalination layer thickness, avoids mechanical damage during assembly, improves yield and performance consistency, and simultaneously improves desalination rate and water flux.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to the field of water treatment technology, and in particular to a method for preparing a hollow fiber reverse osmosis membrane using in-situ interfacial polymerization. The method includes the following steps: S1: Preparation of a hollow fiber supporting membrane module; S2: Preparation of an aqueous phase mixture; S3: Preparation of an oil phase solution; S4: Preparation of a polyamide separation layer: Using the hollow fiber membrane filaments inside the hollow fiber supporting membrane module as a carrier, an aqueous phase mixture and an oil phase solution are introduced, and in-situ diffusion interfacial polymerization is performed to form a polyamide separation layer. The layer is then subjected to constant-temperature thermosetting to obtain the hollow fiber reverse osmosis membrane. The hollow fiber reverse osmosis membrane obtained in this application utilizes in-situ diffusion interfacial polymerization to prepare a polyamide separation layer. The desalination layer thickness is uniform and controllable, and mechanical damage to the desalination layer during assembly is avoided, improving the module yield and performance consistency, while balancing desalination rate and water flux.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of water treatment technology, and in particular to a method for preparing a component-in-situ interfacial polymerization hollow fiber reverse osmosis membrane. Background Technology

[0002] Reverse osmosis is a technology that separates solutes and solvents under pressure using the selective retention of semi-permeable membranes. Since its invention in the 1960s, it has made significant progress. This technology plays a crucial role in seawater desalination, pure water production, and wastewater treatment, greatly alleviating water shortages and water pollution problems. Currently, flat-sheet spiral wound membrane modules have become the mainstream product in the market. However, hollow fiber reverse osmosis membranes, with their advantages of high packing density and the ability to provide a larger effective membrane area within the same volume, show significant application potential in seawater and brackish water desalination.

[0003] In the preparation of hollow fiber reverse osmosis membranes, existing technologies typically employ interfacial polymerization to form a polyamide desalination layer on the surface of a porous supporting membrane. Based on the location of the polyamide layer on the membrane fibers, there are two main routes: external surface polymerization and internal surface polymerization. External surface polymerization is suitable for flat sheet membranes, where the membrane is first formed on the surface of the membrane fibers and then assembled into modules. However, the subsequent assembly process inevitably causes mechanical damage to the desalination layer, resulting in a lower product yield and hindering large-scale, high-efficiency production. Internal surface polymerization, on the other hand, involves first forming modules and then performing interfacial polymerization within the membrane fiber cavity. Its advantage lies in avoiding mechanical damage caused by assembly after membrane formation, reducing the risk of damage to the desalination layer during assembly, and thus protecting the integrity of the desalination layer.

[0004] While the internal surface polymerization route can mitigate mechanical damage to some extent, addressing only this single issue is insufficient to meet actual production needs. Furthermore, existing technologies have failed to effectively balance flux and desalination rate, making it difficult to simultaneously achieve high water flux and high desalination rate. This fails to meet the requirements of large-scale production for high-performance reverse osmosis membranes, severely hindering the commercialization of hollow fiber reverse osmosis membranes. Summary of the Invention

[0005] In order to effectively improve the separation performance of hollow fiber reverse osmosis membranes, this application provides a method for preparing a component-based in-situ interfacial polymerization hollow fiber reverse osmosis membrane.

[0006] The method for preparing an in-situ interfacial polymerization hollow fiber reverse osmosis membrane provided in this application adopts the following technical solution: A method for preparing an in-situ interfacial polymerized hollow fiber reverse osmosis membrane includes the following steps: S1: Preparation of hollow fiber supported base membrane module: Hollow fiber base membrane filaments are obtained by dry and wet spinning of PES casting solution, sorting, bundling, single-end epoxy potting and sealing, and assembly of central water collection pipe and module shell to obtain hollow fiber supported base membrane module. S2: Preparation of aqueous phase mixture: Add 0.1-0.5 parts of aminated carbon quantum dots to 70-82 parts of water and disperse by ultrasonication; then add 0.5-1 parts of microporous polymer, 3-5 parts of m-phenylenediamine, and 2-2.5 parts of camphor sulfonic acid and stir. Adjust the pH to 8.5-9.5 with triethylamine to obtain the aqueous phase mixture. S3: Preparation of oil phase solution: Dissolve acyl chloride monomers in an oil phase solvent to obtain an oil phase solution; S4: Preparation of polyamide separation layer: Using hollow fiber base membrane filaments inside the hollow fiber support base membrane assembly as a carrier, an aqueous phase mixture and an oil phase solution are introduced, and polyamide separation layer is formed by in-situ diffusion interface polymerization. After constant temperature thermal curing treatment, hollow fiber reverse osmosis membrane is obtained.

[0007] This application first prepares hollow fiber-based membrane filaments by wet-dry spinning of PES casting solution, fabricating modules. Using the base membrane filaments as a carrier, a polyamide separation layer is prepared by in-situ diffusion interfacial polymerization, followed by isothermal thermosetting to form a reverse osmosis membrane. The desalination layer thickness is uniform and controllable, avoiding excessive crosslinking that leads to flux loss and mitigating mechanical damage to the desalination layer during assembly. This improves module yield and performance consistency, while balancing desalination rate and water flux. In the aqueous phase mixture, aminated carbon quantum dots, microporous polymers, and m-phenylenediamine work together. During in-situ diffusion interfacial polymerization, m-phenylenediamine reacts with acyl chloride to construct a polyamide basic network. The amino groups on the surface of the aminated carbon quantum dots covalently crosslink with acyl chloride to form additional nanoscale crosslinking nodes, enhancing network density and improving desalination rate. Simultaneously, the rigid twisted structure of the microporous polymer is embedded within the network, maintaining high free volume. Through hydrogen bonding, it maintains interaction with the polyamide chains, thereby maintaining high flux and ultimately achieving improved water flux and desalination rate.

[0008] Preferably, the in-situ diffusion interfacial polymerization includes: introducing an aqueous phase mixture into the inner cavity of the hollow fiber base membrane filament through a central water collection pipe at a constant temperature and pressure, allowing it to be soaked and filled before allowing it to diffuse, and then introducing an oil phase solution into the shell side of the module to cause interfacial polymerization and obtain a polyamide separation layer.

[0009] More preferably, the hollow fiber-based membrane filament is circulated and impregnated with an aqueous mixture for 15-25 minutes, allowed to stand and diffuse for 10-15 minutes, and then subjected to interfacial polymerization for 60-90 seconds.

[0010] In-situ diffusion interfacial polymerization can form a polyamide separation layer in situ on hollow fiber membrane filaments. By utilizing the wetting and diffusion of the aqueous mixture in the inner cavity of the membrane filaments, as well as the subsequent interfacial polymerization with the shell-side oil phase solution, it helps to improve the uniformity and integrity of the separation layer formation and ensure the desalination rate of the membrane. Moreover, this method avoids mechanical damage to the desalination layer during post-membrane assembly.

[0011] Preferably, the in-situ diffusion interfacial polymerization includes: introducing an aqueous phase mixture into the shell side of the component to wet the outer surface of the hollow fiber base membrane filament, and draining the free aqueous phase in the shell side; then introducing an oil phase solution into the inner cavity of the hollow fiber base membrane filament through a central water collection pipe at a constant temperature and pressure, whereby the oil phase diffuses outward and interfacial polymerization occurs to obtain a polyamide separation layer.

[0012] More preferably, the aqueous mixture is impregnated for 20-30 minutes, and the hollow fiber-based membrane filament is circulated with an oil phase solution for 50-80 seconds for interfacial polymerization.

[0013] First, the outer surface of the hollow fiber membrane is wetted with an aqueous phase mixture. After the free aqueous phase is emptied, the oil phase solution diffuses from the inner cavity to the outside to carry out interfacial polymerization. This can avoid mechanical damage to the desalination layer during assembly after film formation. The cross-linking reaction is achieved by utilizing the diffusion rate gradient of the oil phase, which progresses along the thickness direction of the membrane wall. This maximizes the cross-linking density on the extremely thin outer wall surface and improves the water flux.

[0014] Preferably, the microporous polymer is the microporous polymer PIM-1.

[0015] Preferably, in the aqueous mixture, the mass ratio of aminated carbon quantum dots, microporous polymer and m-phenylenediamine is 0.2:0.8:3.

[0016] The combination of aminated carbon quantum dots, microporous polymers, and m-phenylenediamine creates a multi-site hydrogen bond network between the hydroxyl terminals of the microporous polymer molecular chains and the amino groups on the m-phenylenediamine molecules, as well as the amino and hydroxyl groups on the surface of the aminated carbon quantum dots. This network allows for integral deposition on the outer wall of the membrane fibers during shell-side wetting. After the free aqueous phase is evacuated, the hydrogen bond network stably anchors the m-phenylenediamine and aminated carbon quantum dots to the outer wall surface. The abundant amino and hydroxyl groups on the quantum dot surface endow them with excellent water dispersibility and hydrogen bonding ability. Their nanoscale size provides a large number of surface active sites, enabling them to exist stably within the hydrogen bond network and providing a uniform and sufficient reactant loading for subsequent interfacial polymerization. In in-situ diffusion interfacial polymerization, the oil-phase acyl chloride monomer diffuses from the inner lumen of the membrane fibers to the outer wall. Upon reaching the outer wall, it reacts with m-phenylenediamine to construct the polyamide basic network. Simultaneously, the amino groups on the surface of the aminated carbon quantum dots undergo covalent cross-linking reactions with the acyl chloride, chemically embedding themselves into the polyamide network to form additional nanoscale cross-linking nodes, enhancing network density and thus significantly improving the desalination rate. The rigid, twisted, three-dimensional folded structure of the microporous polymer is embedded in situ within the polyamide network during its growth. Its high free volume forms water transport channels within the polyamide layer. Simultaneously, the microporous polymer maintains continuous hydrogen bond interactions with the amide groups and residual amino groups on the polyamide chain through its hydroxyl groups, ensuring that the free volume is maintained during the curing process. This prevents the free volume from collapsing due to chain segment relaxation, thereby ensuring high flux. Ultimately, this results in a significant increase in desalination rate without a significant decrease in water flux.

[0017] Preferably, the oil phase solution comprises 0.5-3 parts of acyl chloride monomer and 80-90 parts of oil phase solvent.

[0018] Preferably, the acyl chloride monomer is pyromellitic tricarboxylate chloride or 2,2',4,4'-biphenyltetracarboxylate chloride in a mass ratio of 3-5:1.

[0019] The presence of acyl chloride monomers in the oil phase solution facilitates the construction of a suitable cross-linked structure during interfacial polymerization, achieving a balance between membrane desalination rate and water flux, thus contributing to the acquisition of a high-performance polyamide separation layer. Trimethylbenzene chloride contains three acyl chloride groups, which can react with m-phenylenediamine to form a basic cross-linked aromatic polyamide backbone; 2,2',4,4'-biphenyltetracarboxylic chloride contains four acyl chloride groups and a rigid biphenyl structure, providing tetrafunctional cross-linking, significantly increasing the polyamide cross-linking density, and the biphenyl structure enhances the structural stability of the separation layer. Constructing a suitable gradient cross-linked network with the aqueous phase network of this application results in a dense polyamide layer surface to intercept salt ions, while the bulk phase maintains adequate chain segment mobility to preserve water transport efficiency, thus contributing to improved desalination rate and water flux of the reverse osmosis membrane.

[0020] Preferably, the oil phase solvent includes one or more of n-hexane, cyclohexane, ethylcyclohexane, n-heptane, and Isopar G isoalkanes.

[0021] In summary, this application includes at least one of the following beneficial technical effects: 1. Hollow fiber-based membrane filaments are prepared by wet-dry spinning of PES casting solution, and then fabricated into modules. Using the base membrane filaments as a carrier, a polyamide separation layer is prepared by in-situ diffusion interfacial polymerization, followed by isothermal thermosetting to form a reverse osmosis membrane. The desalination layer thickness is uniform and controllable, avoiding excessive cross-linking that leads to flux loss, and mitigating mechanical damage to the desalination layer during assembly. This improves the module yield and performance consistency, while balancing desalination rate and water flux.

[0022] 2. The aminated carbon quantum dots, microporous polymers and m-phenylenediamine in the aqueous mixture work together. During interfacial polymerization, the carbon quantum dots covalently crosslink with the acyl chloride to form additional crosslinking nodes to improve the desalination rate. The microporous polymers, with their rigid twisted structure, form additional water channels in the polyamide layer and maintain free volume to ensure high throughput. Together, they achieve a simultaneous increase in throughput and desalination rate.

[0023] 3. This application differs from existing single-filament bilateral diffusion and module single-sided polymerization technologies by using a complete, sealed industrial-grade base membrane module without a separation layer as the reaction carrier to construct a module-level bidirectional controllable fluid diffusion system. By interchanging the positions of the inner cavity and shell sides, two directional transmembrane diffusion paths of MPD monomers are realized. It is compatible with the integrated production of two types of reverse osmosis membrane elements, namely high desalination and high flux, on the same set of equipment, thus solving the problems of membrane damage, uneven performance, reagent waste, and limited production capacity. Detailed Implementation

[0024] Unless otherwise specified, all raw materials used in this application are from commercially available brands or obtained through conventional preparation processes. Specifically: Aminated carbon quantum dots: Xi'an Ruixi Biotechnology Co., Ltd.; Microporous polymer PIM-1: Beijing Huawi Ruike Chemical Technology Co., Ltd. Example 1

[0025] A method for preparing an in-situ interfacial polymerized hollow fiber reverse osmosis membrane includes the following steps: S1: Preparation of hollow fiber supported base membrane module: Polyethersulfone was vacuum dried at 120℃ for 12 h. Polyethersulfone, N-methyl-2-pyrrolidone, polyethylene glycol 400 and water were mixed in a mass ratio of 22:37:37:4 and stirred at 75℃ for 48 h to dissolve. After standing at 75℃ for 12 h to remove bubbles, a casting solution was obtained. The degassed casting solution was fed into the outer ring channel of the annular spinneret at a flow rate of 10 mL / min, and water was fed into the inner ring channel of the spinneret at a flow rate of 4 mL / min. Hollow fiber filaments were extruded and solidified in a water coagulation bath at 25℃. The filaments were soaked in water for 2 days, with the water changed every 10 h. Then, they were soaked in a 50 / 50 wt% glycerol / water solution for 2 days and air-dried at room temperature. The resulting base membrane filaments had an outer diameter of about 0.8 mm and an inner diameter of about 0.5 mm. The filaments were counted one by one according to the design filling amount of 2000 filaments / module. The filaments were neatly arranged into parallel fiber bundles and temporarily fixed at both ends with nylon cable ties. One end of the fiber bundle was vertically inserted into a stainless steel potting mold. Epoxy resin A:B was mixed evenly at a mass ratio of 100:50. After vacuum degassing for 15 minutes, the mixture was injected into the potting mold and cured at 50℃ for 12 hours to form a tube-plate structure. After demolding, the other end of the fiber bundle was potted using the same method. The fiber bundle with potted ends was then installed into the polypropylene module shell (5 cm in diameter, 50 cm in length). A central water collection pipe (with evenly distributed water collection holes on the side wall, communicating with the fiber cavity) and end caps were installed, and the hollow fiber supported the base membrane module. 0.03 MPa nitrogen gas was introduced into the module cavity and held for 5 minutes; then 0.03 MPa nitrogen gas was introduced into the shell side and held for 5 minutes, confirming no crossflow between the cavity and the shell side. S2: Preparation of aqueous phase mixture: Add 0.2 parts of aminated carbon quantum dots to water and ultrasonically disperse for 30 min; add 0.8 parts of microporous polymer and stir for 4 h; add 3 parts of m-phenylenediamine and 2 parts of camphor sulfonic acid and stir; adjust pH to 9 with triethylamine; add water to 100 parts to obtain aqueous phase mixture; S3: Preparation of oil phase solution: Dissolve 0.3 parts of pyromellitic methyl chloride and 0.1 parts of 2,2',4,4'-biphenyltetracarboxylate chloride in 99.5 parts of IsoparG to obtain an oil phase solution; S4: Preparation of the polyamide separation layer: The hollow fiber support base membrane module that passed the leak test in S1 was placed horizontally. The aqueous phase mixture obtained in S2 was introduced into the module from the shell-side inlet, completely filling the shell-side cavity and immersing all membrane fibers. It was circulated and wetted for 20 min (circulation flow rate 0.5 L / min). The free aqueous phase was then drained from the shell-side outlet. The oil phase solution obtained in S3 was introduced into all hollow fiber cavities from the central water collection pipe inlet. It was circulated through the fiber cavities under a nitrogen back pressure of 0.1 bar at a circulation flow rate of 0.3 L / min. It diffused directionally from the inner cavity through the membrane wall micropores to the outer wall, and an interfacial polycondensation reaction occurred for 60 s to obtain the polyamide separation layer. It was then cleaned with n-hexane for 5 min, cleaned with pure water in both directions for 15 min, cured at 65℃ for 30 min, and cooled to obtain the hollow fiber reverse osmosis membrane. Example 2

[0026] The only difference between this embodiment and Example 1 is: S2: Preparation of aqueous phase mixture: 0.8 parts of aminated carbon quantum dots are added to water and ultrasonically dispersed for 30 min; 0.2 parts of microporous polymer are added and stirred for 4 h; 3 parts of m-phenylenediamine and 2 parts of camphor sulfonic acid are added and stirred; the pH is adjusted to 9 with triethylamine; water is added to 100 parts to obtain aqueous phase mixture. Example 3

[0027] The only difference between this embodiment and Example 1 is: S3: Preparation of oil phase solution: Take 0.1 parts of pyromellitic methyl chloride and 0.3 parts of 2,2',4,4'-biphenyltetracarboxylic chloride and dissolve them in 99.5 parts of IsoparG to obtain an oil phase solution. Example 4

[0028] The only difference between this embodiment and Example 1 is: S3: Prepare the oil phase solution: Dissolve 0.4 parts of pyromellitic chloride in 99.5 parts of IsoparG to obtain the oil phase solution. Example 5

[0029] The only difference between this embodiment and Example 1 is: S3: Preparation of oil phase solution: Take 0.4 parts of 2,2',4,4'-biphenyltetracarboxylic chloride and dissolve it in 99.5 parts of IsoparG to obtain an oil phase solution.

[0030] Comparative Example 1 The only difference between Comparative Example 1 and Example 1 is: S2: Preparation of aqueous mixture: 0.2 parts of aminated carbon quantum dots were added to water and ultrasonically dispersed for 30 min; 3.8 parts of m-phenylenediamine and 2 parts of camphor sulfonic acid were added and stirred, the pH was adjusted to 9 with triethylamine, and water was added to 100 parts to obtain aqueous mixture.

[0031] Comparative Example 2 The only difference between Comparative Example 2 and Example 1 is: S2: Preparation of aqueous mixture: 0.8 parts of microporous polymer were added to water and stirred for 4 h; 3.8 parts of m-phenylenediamine and 2 parts of camphor sulfonic acid were added and stirred, the pH was adjusted to 9 with triethylamine, and water was added to 100 parts to obtain aqueous mixture.

[0032] Comparative Example 3 The only difference between Comparative Example 3 and Example 1 is: S2: Preparation of aqueous mixture: 4 parts of m-phenylenediamine were added to water and ultrasonically dispersed for 30 min; 2 parts of camphor sulfonic acid were stirred, the pH was adjusted to 9 with triethylamine, and water was added to 100 parts to obtain aqueous mixture.

[0033] Comparative Example 4 The only difference between Comparative Example 4 and Example 1 is that: the hollow fiber support base membrane module that passed the leak test in S1 was placed horizontally, and the aqueous phase mixture prepared in S2 was introduced into all hollow fiber cavities through the central water collection pipe inlet. It was circulated and impregnated at a constant temperature of 27°C for 20 min (circulation flow rate 0.5 L / min). After the circulation was stopped, it was allowed to stand and diffuse for 12 min, and then the free aqueous phase in the cavity was drained. The oil phase solution prepared in S3 was introduced into the sealed shell side of the module through the shell side inlet. It was polymerized at a constant temperature of 27°C for 75 s to generate a polyamide separation layer. After the reaction was completed, the oil phase was drained, and the cavity was circulated and cleaned with n-hexane for 5 min and the shell side for 2 min. Then it was circulated and cleaned with pure water for 15 min. It was then placed in a constant temperature oven at 65°C for 30 min for heat curing and cooled to obtain a hollow fiber reverse osmosis membrane.

[0034] The separation performance of the hollow fiber reverse osmosis membranes prepared in Examples 1-5 and Comparative Examples 1-4 was tested under the following conditions: test temperature 25℃, pressure 225 psi, and test solution 2000ppm sodium chloride solution. The initial water flux and desalination rate were tested, and the results are shown in Table 1.

[0035] Table 1. Water flux performance test results

[0036] As can be seen from Examples 1-5 and Comparative Examples 1-4 of the present invention, the hollow fiber reverse osmosis membrane obtained in this application uses in-situ diffusion interface polymerization to prepare a polyamide separation layer. The thickness of the desalination layer is uniform and controllable, and mechanical damage to the desalination layer during assembly is avoided, thereby improving the yield and performance consistency of the module, while taking into account both the desalination rate and water flux.

[0037] As can be seen from Examples 1-2 and Comparative Examples 1-4 of this application, the combination of aminated carbon quantum dots, microporous polymers, and m-phenylenediamine in the aqueous phase is key to achieving simultaneous improvement in flux and desalination rate. When using a reverse diffusion mode (water phase shell-side wetting causing MPD adsorption on the outer wall, and oil phase diffusion from the inner cavity to the outer wall), a polyamide layer is formed on an extremely thin outer wall surface. The covalent cross-linking of amino groups and acyl chlorides on the carbon quantum dot surface forms additional cross-linking nodes, densifying the network to improve the desalination rate. The microporous polymer, with its rigid twisted structure, forms additional water channels in the polyamide layer and maintains free volume to ensure high flux. Both work together within the basic network constructed by m-phenylenediamine to obtain a hollow fiber reverse osmosis membrane with a dense separation layer and high flux.

[0038] Comparing Examples 1 and 3-5, it can be seen that pyromellitic tricarboxylic acid first reaches the outer wall to construct a moderately cross-linked basic framework to maintain water transport efficiency; biphenyl tetracarboxylic acid then reaches the outer wall and superimposes tetrafunctional hypercrosslinking to densify the surface layer to intercept salt ions. The two work together to form a gradient network structure with a dense surface layer and moderately cross-linked bulk phase, achieving optimization of high desalination rate and high throughput in the reverse diffusion mode.

[0039] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.

Claims

1. A method for preparing a component-based in-situ interfacial polymerization hollow fiber reverse osmosis membrane, characterized in that, Includes the following steps: S1: Preparation of hollow fiber supported base membrane module: Hollow fiber base membrane filaments are obtained by dry and wet spinning of PES casting solution, sorting, bundling, single-end epoxy potting and sealing, and assembly of central water collection pipe and module shell to obtain hollow fiber supported base membrane module. S2: Preparation of aqueous phase mixture: Add 0.1-0.5 parts of aminated carbon quantum dots to 70-82 parts of water and disperse by ultrasonication; then add 0.5-1 parts of microporous polymer, 3-5 parts of m-phenylenediamine, and 2-2.5 parts of camphor sulfonic acid and stir. Adjust the pH to 8.5-9.5 with triethylamine to obtain the aqueous phase mixture. S3: Preparation of oil phase solution: Dissolve acyl chloride monomers in an oil phase solvent to obtain an oil phase solution; S4: Preparation of polyamide separation layer: Using hollow fiber base membrane filaments inside the hollow fiber support base membrane assembly as a carrier, an aqueous phase mixture and an oil phase solution are introduced, and polyamide separation layer is formed by in-situ diffusion interface polymerization. After constant temperature thermal curing treatment, hollow fiber reverse osmosis membrane is obtained.

2. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 1, characterized in that, The in-situ diffusion interfacial polymerization includes: introducing an aqueous phase mixture into the inner cavity of the hollow fiber base membrane filament through a central water collection pipe at a constant temperature and pressure, allowing it to be soaked and filled before allowing it to diffuse, and then introducing an oil phase solution into the shell side of the component to cause interfacial polymerization and obtain a polyamide separation layer.

3. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 2, characterized in that, The hollow fiber-based membrane filament is circulated and soaked in an aqueous mixture for 15-25 minutes, allowed to stand and diffuse for 10-15 minutes, and then subjected to interfacial polymerization for 60-90 seconds.

4. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 1, characterized in that, The in-situ diffusion interfacial polymerization includes: introducing an aqueous phase mixture into the shell side of the component to wet the outer surface of the hollow fiber base membrane filaments, and draining the free aqueous phase in the shell side; then introducing an oil phase solution into the inner cavity of the hollow fiber base membrane filaments through a central water collection pipe at a constant temperature and pressure, whereby the oil phase diffuses outward and interfacial polymerization occurs to obtain a polyamide separation layer.

5. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 4, characterized in that, The aqueous phase mixture is soaked for 20-30 minutes, and the hollow fiber-based membrane filament inner cavity oil phase solution is circulated and polymerized at the interface for 50-80 seconds.

6. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 1, characterized in that, The oil phase solution comprises 0.5-3 parts of acyl chloride monomer and 80-90 parts of oil phase solvent.

7. The method for preparing a hollow fiber reverse osmosis membrane by in-situ interfacial polymerization according to claim 6, characterized in that, The acyl chloride monomers are pyromellitic tricarboxylic acid chloride and 2,2',4,4'-biphenyltetracarboxylic acid chloride in a mass ratio of 3-5:

1.