A production process for a high-efficiency carbon dioxide capture device

By employing a chemical-physical synergistic encapsulation process involving the classification of aminated mesoporous silica nanoparticles and the microencapsulation of thermally initiated crosslinking agents, the interfacial bonding strength and batch stability issues of carbon dioxide separation membrane modules under high-pressure conditions were resolved, enabling the industrial production of highly efficient and stable carbon dioxide capture devices.

CN123102171APending Publication Date: 2026-11-17HOPE GREEN CARBON (SHENZHEN) ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611186362.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing carbon dioxide separation membrane modules have insufficient bonding strength at the encapsulation interface, are prone to delamination under high pressure conditions, and have poor batch stability, making it difficult to meet the quality stability requirements of industrial continuous production.

Method used

A chemical-physical synergistic encapsulation process is adopted, which combines graded aminated mesoporous silica nanoparticles with microencapsulated thermally initiated crosslinking agents. By graded the nanoparticle surface grafting degree and matching differentiated thermo-pressing parameters, combined with a moisture-wicking separator design and an impedance sensing system, a chemically bonded enhanced encapsulation is formed.

Benefits of technology

It significantly improved the interfacial bonding strength between the membrane and the flow channel baffle, ensuring batch consistency of products and long-term operational stability under high humidity conditions, and realizing efficient and stable industrial production of carbon dioxide capture devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102171A_ABST
    Figure CN123102171A_ABST
Patent Text Reader

Abstract

This application relates to the field of carbon capture technology, specifically disclosing a manufacturing process for a high-efficiency carbon dioxide capture device. The core raw materials used in this process include aminated mesoporous silica nanoparticles, microencapsulated thermally initiated crosslinking agents, and polyether block amides. The microencapsulated crosslinking agent exhibits temperature-responsive release characteristics at 115-125°C. The preparation method includes graded grafting degree of aminated mesoporous silica, preparation of composite membrane precursors, processing of moisture-conducting microstructure separators with wettability gradients, chemical-physical synergistic hot-press encapsulation, system integration and impedance sensing system implantation, and graded accelerated aging and digital twin closed-loop calibration. Devices prepared using this process can be used for carbon dioxide capture from industrial flue gas in coal-fired power plants, steel mills, cement plants, etc., significantly improving the interfacial bonding strength of membrane modules, solving the membrane layer delamination problem under high-pressure conditions, improving batch stability, enhancing adaptability to high-humidity conditions, and achieving continuous optimization throughout the entire lifecycle of the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of carbon capture technology, and more specifically, to a manufacturing process for a high-efficiency carbon dioxide capture device. Background Technology

[0002] Driven by the "dual carbon" goals, carbon dioxide capture, utilization, and storage technologies have become one of the core directions for industrial emission reduction. Membrane separation, with its advantages of low energy consumption, simple equipment structure, and no secondary pollution, has gained widespread attention in small- to medium-scale flue gas capture scenarios. As the core unit of a membrane separation device, the quality of the membrane module's encapsulation directly determines the device's operational stability and lifespan, making it a crucial link in realizing the large-scale industrial application of membrane separation technology.

[0003] Existing carbon dioxide separation membrane modules generally employ a physical thermo-pressing encapsulation process, relying on high temperature and pressure to mechanically bond the membrane material to the flow channel separator. This encapsulation method has limited interfacial bonding strength. Under high-pressure operating conditions in industrial flue gas, delamination easily occurs between the membrane and the separator, leading to gas short-circuiting and a rapid decline in capture efficiency. Furthermore, the surface chemical properties of functional fillers such as aminated mesoporous silica exhibit natural batch-to-batch fluctuations. When using uniform thermo-pressing parameters for production, the encapsulation quality varies significantly between different batches, making it difficult to meet the quality stability requirements of continuous industrial production. Summary of the Invention

[0004] To address the issues of insufficient bonding strength at the encapsulation interface of existing carbon dioxide separation membrane modules, easy delamination under high-pressure conditions, and poor batch stability, this application provides a manufacturing process for a high-efficiency carbon dioxide capture device.

[0005] A manufacturing process for a high-efficiency carbon dioxide capture device includes the following steps: S1. Substrate shell pretreatment: preparation of the outer shell of the equipment and the composite film support layer; S2. Nanoparticle classification: The surface grafting degree of aminated mesoporous silica nanoparticles is detected, and they are classified according to the grafting degree range and the classification information is recorded. S3. Preparation of composite membrane precursor: A casting solution containing aminated mesoporous silica nanoparticles graded by S2 and a microencapsulated thermally initiated crosslinking agent was prepared. The film was formed on a polysulfone support layer by phase inversion method and dried at a temperature below the decomposition threshold of the crosslinking agent to obtain the composite membrane precursor. S4. Moisture-guiding baffle processing: Two-level microstructures are processed on the surface of the polytetrafluoroethylene flow channel baffle and regional selective modification is carried out to form a moisture-guiding microstructure with wettability gradient. S5, Chemical-Physical Co-encapsulation: The composite film obtained in S3 and the flow channel partition obtained in S4 are alternately stacked to form a film stack. The hot-pressing parameters are matched according to the hierarchical information of S2 for hot-pressing encapsulation. When the hot-pressing temperature reaches the decomposition threshold of the crosslinking agent, in-situ crosslinking and interfacial grafting reactions are triggered to form chemically bonded enhanced encapsulation. S6. System Integration and Assembly: Integrate the membrane module encapsulated by S5 with the pretreatment unit and compressor unit onto the frame, connect the pipelines and check for leaks; S7. Impedance sensing system implantation: Electrode arrays are integrated at both ends of the membrane stack and connected to the impedance analysis module to form a dynamic impedance spectrum health sensing system. S8. Aging Test Closed-Loop Calibration: Perform benchmark performance tests and graded accelerated aging tests on the integrated device, transmit the test data back to the digital twin system, correct the performance degradation model, and provide feedback to optimize production parameters.

[0006] By adopting the above technical solutions, a complete production system has been constructed, from raw material graded control to full life cycle iterative optimization. The system deeply integrates material chemical property regulation, flow channel fluid dynamics design, precise thermochemical reaction control and intelligent sensing calibration. Each process link forms a synergistic mechanism that supports each other, fundamentally solving the technical problems of existing membrane separation and capture devices, such as weak interfacial bonding, poor batch stability, insufficient adaptability to high humidity conditions, and short lifespan, and realizing the efficient and stable industrial production of carbon dioxide capture devices.

[0007] Preferably, in step S2, the surface grafting degree of the aminated mesoporous silica nanoparticles ranges from 1.2 to 1.8 mmol / g, wherein a grafting degree of 1.2 to 1.5 mmol / g is the first level, corresponding to a hot-pressing temperature of 115 to 122℃ and a pressure of 0.5 to 0.6 MPa; and a grafting degree of 1.5 to 1.8 mmol / g is the second level, corresponding to a hot-pressing temperature of 122 to 130℃ and a pressure of 0.6 to 0.7 MPa.

[0008] By adopting the above technical solution, the nanoparticles are graded and controlled according to the difference in the number of amino active sites on their surface, and different hot pressing process parameters are matched to ensure that different batches of nanoparticles can complete the interface grafting reaction during the hot pressing process. This avoids the situation where batches with high grafting degree react excessively, causing the film material to become brittle, or batches with low grafting degree react insufficiently and fail to form stable chemical bonds. This effectively reduces the performance difference between different batches of products and improves the quality stability of large-scale industrial production.

[0009] Preferably, in step S3, the microencapsulation thermal initiation crosslinking agent uses dicumyl peroxide as the core material and polyamide as the wall material, with a thermal decomposition threshold temperature of 115-125℃, and the addition amount is 1-3% of the total mass of the solute in the casting solution; the addition amount of aminated mesoporous silica nanoparticles is 10-15% of the total mass of the solute in the casting solution.

[0010] By employing the above technical solution, the temperature response characteristics of polyamide wall materials are utilized to achieve controlled release of the crosslinking agent, ensuring its stability during the casting solution preparation and drying stages, and releasing the active ingredient only when the threshold temperature is reached during the hot-pressing stage. Aminated mesoporous silica serves both as a carbon dioxide adsorption site to enhance separation performance and as an active site for interfacial grafting reactions to strengthen encapsulation. A reasonable addition range avoids nanoparticle aggregation that could disrupt membrane pore uniformity, while also preventing excessive crosslinking of the polyether block amide matrix due to excessive crosslinking agent.

[0011] Preferably, in step S3, the casting solution is prepared by dissolving polyether block amide in N,N-dimethylformamide to form a polymer solution and then adding the corresponding components. The phase inversion method uses a water and ethanol mixed solution with a volume ratio of (2.8-3.2):1 as the coagulation bath, and the drying temperature is 55-65℃ and the drying time is 20-28h.

[0012] By employing the above technical solution, a uniform and stable casting solution is prepared using the excellent solubility of N,N-dimethylformamide in polyether block amides. Water is used as a non-solvent, and ethanol as a weak non-solvent. By adjusting the ratio of the two, the phase transformation rate is controlled, resulting in a membrane pore structure with a uniform pore size distribution. Simultaneously, the drying temperature is controlled below the decomposition threshold of the crosslinking agent to prevent premature release of the crosslinking agent and subsequent pore blockage, thus ensuring the gas permeation flux and separation selectivity of the composite membrane.

[0013] Preferably, in step S4, the two-stage microstructure includes a primary main channel and a secondary capillary channel. The primary main channel has a width of 180-220 μm and a depth of 45-55 μm. The secondary capillary channel has an angle of 55-65° with the main channel, a width of 8-12 μm, and a depth of 18-22 μm. The regional selective modification involves forming hydrophilic strips at the bottom of the capillary channel while maintaining hydrophobic properties in the main channel region.

[0014] By adopting the above technical solution, the primary main channel achieves uniform distribution of flue gas on the membrane surface, reducing gas flow resistance. The capillary action of the secondary capillary channels collects the condensate that has permeated through the membrane. The hydrophobicity of the main channel region prevents condensate from spreading in the gas flow area, while the hydrophilicity of the bottom of the capillary channels enhances the adsorption and collection capacity of condensate, driving the condensate to flow directionally along the channels and discharge it, thus preventing condensate from accumulating between the membrane and the separator to form a water film.

[0015] Preferably, in step S5, the heat preservation and pressure holding time for hot pressing is 25-35 minutes, and the interfacial bonding strength of the encapsulated membrane module is not less than 8 MPa.

[0016] By employing the above technical solution, sufficient time is ensured during the hot-pressing process for the crosslinking agent to fully decompose and diffuse to the interface region between the membrane and the flow channel separator. Simultaneously, this triggers crosslinking between polyether block amide molecular chains and grafting reactions between the molecular chains and the amino groups on the surface of aminated mesoporous silica. Sufficient interfacial bonding strength ensures that the membrane module does not delaminate during long-term operation under high-pressure conditions, preventing gas short-circuiting and thus avoiding a decrease in capture efficiency.

[0017] Preferably, in step S6, the pretreatment unit includes a cyclone dust collector and an activated carbon adsorption device; leak detection is performed using helium gas, and the leakage rate is controlled to be less than 1×10⁻⁶. -6 mbar・L / s.

[0018] By adopting the above technical solution, the cyclone dust collector first removes larger dust particles from the flue gas to prevent them from scratching the membrane surface, while activated carbon adsorption further removes trace amounts of acidic gases such as sulfur dioxide, preventing acidic substances from corroding the membrane material and encapsulation interface. High-sensitivity helium leak detection technology is used to test the system's sealing performance, ensuring no gas leakage during high-pressure operation, thus improving operational safety and collection efficiency.

[0019] Preferably, in step S7, the electrode array forms a parallel plate capacitive sensing structure, and the electrode surface is coated with a polytetrafluoroethylene protective layer; the frequency range of the swept AC signal applied by the impedance analysis module is 1Hz-1MHz, which is used for online measurement of the full-band AC impedance spectrum of the membrane stack.

[0020] By employing the above technical solution, the changes in the dielectric properties of the membrane module are sensed using a parallel plate capacitor structure. After the membrane material undergoes chemical erosion or physical compaction, its dielectric constant and conductivity will change accordingly. Impedance signals at different frequency bands can correspond to the state changes of the membrane body, interface, and flow channel, respectively. The polytetrafluoroethylene protective layer can isolate acidic flue gas from direct contact with the electrodes, avoiding electrode corrosion failure and realizing non-invasive online monitoring of the membrane module's health status.

[0021] Preferably, in step S8, the graded accelerated aging test includes an acidic mode, an abrasion mode, and a hot-cold-humidity cycle mode in sequence. The acidic mode uses simulated flue gas containing SO2, the abrasion mode uses simulated flue gas containing dust, and the hot-cold-humidity cycle mode is carried out under alternating temperature and humidity conditions.

[0022] By adopting the above technical solutions, the main failure factors in different industrial application scenarios are simulated respectively. The acid mode corresponds to the high sulfur flue gas environment such as steel plants, the wear mode corresponds to the high dust environment such as cement plants, and the cold, hot and humid cycle mode corresponds to the load fluctuation and seasonal climate change of power plants. The potential defects in materials, structures and packaging systems are systematically exposed, unqualified products are screened out before leaving the factory, and comprehensive experimental data are provided for establishing an accurate performance degradation model.

[0023] Preferably, in step S8, the digital twin system receives benchmark performance test data, accelerated aging test data, and actual device operation data, automatically corrects the fluid distribution model, membrane performance degradation model, and interface bonding strength prediction model, and feeds back the optimized hot-pressing packaging parameters and material grading standards to the production end.

[0024] By adopting the above technical solutions and integrating multi-source measured data to continuously refine the digital twin model, the model's prediction accuracy is constantly improved. The operational data from each batch of products is used to optimize the production parameters of subsequent batches, forming a closed-loop process for production testing, operation, and optimization throughout the entire lifecycle. This allows the production process to continuously adapt to the needs of different raw material characteristics and application scenarios, thereby continuously improving product performance and reliability.

[0025] In summary, this application has the following beneficial effects: 1. Because this application adopts a process of graded grafting degree of aminated mesoporous silica and pre-matching of hot pressing parameters, combined with the mechanism of in-situ triggering of microencapsulation thermal initiation crosslinking agent during the hot pressing stage, it realizes chemical-physical synergistic encapsulation of membrane and flow channel partition, significantly improves the interfacial bonding strength, solves the industry pain point of membrane layer delamination under high pressure conditions, and ensures batch consistency of products.

[0026] 2. In this application, a moisture-conducting baffle design with a two-stage microstructure and wettability gradient is preferred. The condensate that has permeated through the membrane is actively and directionally discharged by capillary force, which avoids the condensate from accumulating at the interface to form a water film, effectively reducing mass transfer resistance and improving the long-term operational stability of the device under high humidity flue gas conditions.

[0027] 3. The method of this application integrates electrode arrays at both ends of the membrane module and connects them with impedance analysis modules to form a dynamic impedance spectrum health sensing system. This system can non-invasively monitor the microscopic state changes of the membrane module online, realize early warning of performance degradation, and provide a reliable basis for the operation and control of the device.

[0028] 4. The method of this application conducts graded accelerated aging tests and combines them with a digital twin system to transmit benchmark test, aging test and actual operation data back to correct relevant models, and feeds back the optimized parameters to the production end, forming a closed loop throughout the entire life cycle, and continuously improving manufacturing accuracy and product adaptability. Attached Figure Description

[0029] Figure 1 This is a production process flow diagram of a high-efficiency carbon dioxide capture device provided in this application. Detailed Implementation

[0030] The present application will be further described in detail below with reference to embodiments and comparative examples. Unless otherwise specified, the experimental methods used below are conventional methods. Unless otherwise specified, the materials, reagents, methods and instruments used are all conventional materials, reagents, methods and instruments in the art, which can be obtained by those skilled in the art through commercial channels or prepared according to literature methods.

[0031] Technical Concept: Membrane separation is a crucial technology in the current carbon dioxide capture field, but its industrial application is still limited by insufficient reliability of membrane module encapsulation and poor batch-to-batch consistency. Existing technologies generally employ physical thermo-pressing encapsulation, relying solely on high temperature and pressure to achieve mechanical bonding between the membrane and the flow channel separator. This results in limited interfacial adhesion, and under high-pressure operating conditions in industrial flue gas, membrane and separator delamination easily occurs, leading to gas short-circuiting and rapid decline in capture efficiency. Simultaneously, the surface amino grafting degree of functional fillers such as aminated mesoporous silica exhibits natural batch-to-batch fluctuations. Current processes using uniform thermo-pressing parameters cannot adapt to the reaction requirements of different grafting degrees, easily resulting in some batches with insufficient reaction or excessive cross-linking, leading to significant differences in product performance.

[0032] This technical solution addresses the aforementioned issues by first employing a microencapsulated thermally initiated crosslinking agent. Leveraging its temperature-responsive characteristics, the active ingredient is released in situ at the threshold temperature during the hot-pressing stage. This initiates crosslinking of the polyether block amide molecular chains and a grafting reaction with the amino groups on the surface of the aminated mesoporous silica, upgrading the simple physical bonding to a chemically-physical synergistic encapsulation enhanced by chemical bonding. Simultaneously, the grafting degree of the aminated mesoporous silica is pre-classified through detection. Different hot-pressing temperatures and pressure parameters are matched according to different grafting degrees to ensure that each batch of raw materials completes a sufficient interfacial reaction, fundamentally improving encapsulation quality and product batch stability.

[0033] Example 1: This example provides a production process for a high-efficiency carbon dioxide capture device, including the following steps: S1. Substrate shell pretreatment: preparation of the outer shell of the equipment and the composite film support layer; The outer shell of the device is made of 316L stainless steel, which is sandblasted to Sa2.5 grade and then pickled and passivated to remove the surface oxide layer and oil stains. The composite membrane support layer is made of polysulfone material, which is formed by casting method and has a thickness of 120μm. After forming, it is washed with deionized water 3 times and vacuum dried at 60℃ for 12h for later use.

[0034] S2. Nanoparticle classification: The surface grafting degree of aminated mesoporous silica nanoparticles is detected, and they are classified according to the grafting degree range and the classification information is recorded. Among them, the surface grafting degree of the aminated mesoporous silica nanoparticles was 1.35 mmol / g, which belongs to the first level, corresponding to a hot-pressing temperature of 118.5℃ and a pressure of 0.55 MPa. The grafting degree was determined by elemental analysis, and the grading information was entered into the production batch management system after the test was completed.

[0035] S3. Preparation of composite membrane precursor: A casting solution containing S2-graded aminated mesoporous silica nanoparticles and a microencapsulation thermal initiating crosslinking agent was prepared. A film was formed on a polysulfone support layer using a phase inversion method and dried at a temperature below the decomposition threshold of the crosslinking agent to obtain the composite membrane precursor. The microencapsulation thermal initiation crosslinking agent uses dicumyl peroxide as the core material and polyamide as the wall material, with a thermal decomposition threshold temperature of 120℃ and an addition amount of 2% of the total mass of the solute in the casting solution; the addition amount of aminated mesoporous silica nanoparticles is 12.5% ​​of the total mass of the solute in the casting solution; the casting solution is prepared by dissolving polyether block amide in N,N-dimethylformamide to form a polymer solution and then adding the corresponding components, with a polymer solution mass fraction of 10%, a stirring rate of 400 r / min, and a stirring time of 4 h; the phase inversion method uses a water and ethanol mixed solution with a volume ratio of 3:1 as the coagulation bath, and the coagulation bath temperature is 25℃; the drying temperature is 60℃, the drying time is 24 h, and the vacuum degree is maintained at -0.09 MPa during the drying process; the ultrasonic dispersion power is 300 W, and the dispersion time is 2 h.

[0036] S4. Moisture-guiding baffle processing: Two-level microstructures are processed on the surface of the polytetrafluoroethylene flow channel baffle and regional selective modification is carried out to form a moisture-guiding microstructure with wettability gradient. The two-stage microstructure includes a primary main channel and a secondary capillary channel. The primary main channel has a width of 200 μm and a depth of 50 μm, while the secondary capillary channel has a width of 10 μm and a depth of 20 μm, with an angle of 60° to the main channel. Regional selective modification involves forming hydrophilic strips at the bottom of the capillary channel while maintaining hydrophobic properties in the main channel region. The microstructure is fabricated using laser etching with a laser power of 15 W and a scanning rate of 500 mm / s. Regional modification is achieved using mask plasma treatment with a processing power of 75 W and a processing time of 30 s.

[0037] S5, Chemical-Physical Co-encapsulation: The composite film obtained in S3 and the flow channel partition obtained in S4 are alternately stacked to form a film stack. The hot-pressing parameters are matched according to the hierarchical information of S2 for hot-pressing encapsulation. When the hot-pressing temperature reaches the decomposition threshold of the crosslinking agent, in-situ crosslinking and interfacial grafting reactions are triggered to form chemically bonded enhanced encapsulation. The heat-pressing encapsulation process involves a heat preservation and pressure holding time of 30 minutes, resulting in an interfacial bonding strength of no less than 8 MPa for the encapsulated membrane module. The composite membrane is cut to a size of 400 mm × 600 mm, and machine vision is used to inspect for defects with a precision of 0.1 mm. 2 Unqualified membranes are rejected; each unit membrane stack has 20 layers, and the alignment error between the membrane and the flow channel partition is guaranteed to be no more than 0.5mm during stacking.

[0038] S6. System Integration and Assembly: Integrate the membrane module encapsulated by S5 with the pretreatment unit and compressor unit onto the frame, connect the pipelines and check for leaks; The pretreatment unit includes a cyclone dust collector and an activated carbon adsorption unit; leak detection uses helium gas, and the leakage rate is controlled to be less than 1×10⁻⁶. -6 mbar・L / s; the frame is made of carbon steel with a surface anti-corrosion coating; the compressor unit is a screw compressor unit with a pressure adjustment range of 0.1-2.5MPa; the pipeline uses quick-release flange connection, and the inner wall of the pipeline is pickled and passivated before connection.

[0039] S7. Impedance sensing system implantation: Electrode arrays are integrated at both ends of the membrane stack and connected to the impedance analysis module to form a dynamic impedance spectrum health sensing system. The electrode array forms a parallel plate capacitive sensing structure, and the electrode surface is coated with a polytetrafluoroethylene protective layer with a thickness of 5μm. The frequency range of the swept AC signal applied by the impedance analysis module is 1Hz-1MHz, which is used to measure the AC impedance spectrum of the membrane stack in the entire frequency band online. The electrode array is made of gold-plated copper electrodes and integrated into the flow channel partitions of the units at both ends of the membrane stack. The electrodes and the flow channel partitions are bonded together with conductive adhesive.

[0040] S8. Aging test closed-loop calibration: Perform benchmark performance tests and graded accelerated aging tests on the integrated device, and send the test data back to the digital twin system to correct the performance degradation model and feed back to optimize production parameters. The graded accelerated aging test includes an acidic mode, an abrasion mode, and a hot-cold-wet cycle mode. The acidic mode uses simulated flue gas containing 500 ppm SO2, and the abrasion mode uses simulated flue gas containing 50 mg / m³ SO2. 3The simulated flue gas for dust was tested under alternating hot, cold, and humid conditions at 20-60℃ and 30-90%RH. The baseline performance test used simulated flue gas composed of 15% carbon dioxide, 5% oxygen, and 10% water vapor by volume, with nitrogen as the equilibrium gas, running continuously for 72 hours. The digital twin system received baseline performance test data, accelerated aging test data, and actual device operating data, automatically correcting the fluid distribution model, membrane performance degradation model, and interfacial bonding strength prediction model. The optimized hot-pressing encapsulation parameters and material grading standards were fed back to the production end. Each aging mode ran for 240 hours. After aging, the interfacial bonding strength and corresponding impedance spectrum data of the membrane module were retested. Test data was collected every hour and transmitted to the digital twin system in real time.

[0041] Example 2: This example provides a production process for a high-efficiency carbon dioxide capture device, including the following steps: S1. Substrate shell pretreatment: preparation of the outer shell of the equipment and the composite film support layer; The outer shell of the device is made of corrosion-resistant aluminum alloy. After sandblasting to Sa2.5 grade, it is pickled and passivated to remove the surface oxide layer and oil stains. The composite membrane support layer is made of polysulfone material and is formed by casting method. The thickness is 100μm. After forming, it is washed with deionized water 3 times and vacuum dried at 55℃ for 12h for later use.

[0042] S2. Nanoparticle classification: The surface grafting degree of aminated mesoporous silica nanoparticles is detected, and they are classified according to the grafting degree range and the classification information is recorded. Among them, the surface grafting degree of the aminated mesoporous silica nanoparticles was 1.2 mmol / g, which belongs to the first grade, corresponding to a hot-pressing temperature of 115℃ and a pressure of 0.5MPa. The grafting degree was determined by elemental analysis, and the grading information was entered into the production batch management system after the test was completed.

[0043] S3. Preparation of composite membrane precursor: A casting solution containing aminated mesoporous silica nanoparticles graded by S2 and a microencapsulated thermally initiated crosslinking agent was prepared. The film was formed on a polysulfone support layer by phase inversion method and dried at a temperature below the decomposition threshold of the crosslinking agent to obtain the composite membrane precursor. The microencapsulation thermal initiation crosslinking agent uses dicumyl peroxide as the core material and polyamide as the wall material, with a thermal decomposition threshold temperature of 115℃ and an addition amount of 1% of the total mass of the solute in the casting solution; the addition amount of aminated mesoporous silica nanoparticles is 10% of the total mass of the solute in the casting solution; the casting solution is prepared by dissolving polyether block amide in N,N-dimethylformamide to form a polymer solution and then adding the corresponding components, with a polymer solution mass fraction of 8%, a stirring rate of 300 r / min, and a stirring time of 5 h; the phase inversion method uses a water and ethanol mixed solution with a volume ratio of 2.8:1 as the coagulation bath, with a coagulation bath temperature of 20℃; the drying temperature is 55℃, the drying time is 20 h, and the vacuum degree is maintained at -0.09 MPa during the drying process; the ultrasonic dispersion power is 200 W, and the dispersion time is 2.5 h.

[0044] S4. Moisture-guiding baffle processing: Two-level microstructures are processed on the surface of the polytetrafluoroethylene flow channel baffle and regional selective modification is carried out to form a moisture-guiding microstructure with wettability gradient. The two-stage microstructure includes a primary main channel and a secondary capillary channel. The primary main channel has a width of 180 μm and a depth of 45 μm. The secondary capillary channel is at an angle of 55° to the main channel, with a width of 8 μm and a depth of 18 μm. Regional selective modification involves forming hydrophilic strips at the bottom of the capillary channel while maintaining hydrophobic properties in the main channel region. The microstructure is fabricated using laser etching with a laser power of 10 W and a scanning rate of 400 mm / s. Regional modification is performed using mask plasma treatment with a processing power of 50 W and a processing time of 40 s.

[0045] S5, Chemical-Physical Co-encapsulation: The composite film obtained in S3 and the flow channel partition obtained in S4 are alternately stacked to form a film stack. The hot-pressing parameters are matched according to the hierarchical information of S2 for hot-pressing encapsulation. When the hot-pressing temperature reaches the decomposition threshold of the crosslinking agent, in-situ crosslinking and interfacial grafting reactions are triggered to form chemically bonded enhanced encapsulation. The heat-pressing and pressure-holding time for the encapsulation process is 25 minutes, and the interfacial bonding strength of the encapsulated membrane module is no less than 8 MPa. The composite membrane is cut to a size of 390 mm × 590 mm, and machine vision is used to inspect membrane defects with an accuracy of 0.1 mm. 2 Unqualified membranes are rejected; each unit membrane stack has 18 layers, and the alignment error between the membrane and the flow channel baffle is guaranteed to be no more than 0.5mm during stacking.

[0046] S6. System Integration and Assembly: Integrate the membrane module encapsulated by S5 with the pretreatment unit and compressor unit onto the frame, connect the pipelines and check for leaks; The pretreatment unit includes a cyclone dust collector and an activated carbon adsorption unit; leak detection uses helium gas, and the leakage rate is controlled to be less than 1×10⁻⁶. -6mbar・L / s; the frame is made of carbon steel with a surface anti-corrosion coating; the compressor unit is a screw compressor unit with a pressure adjustment range of 0.1-2.5MPa; the pipeline uses quick-release flange connection, and the inner wall of the pipeline is pickled and passivated before connection.

[0047] S7. Impedance sensing system implantation: Electrode arrays are integrated at both ends of the membrane stack and connected to the impedance analysis module to form a dynamic impedance spectrum health sensing system. The electrode array forms a parallel plate capacitive sensing structure, and the electrode surface is coated with a polytetrafluoroethylene protective layer with a thickness of 3μm. The frequency range of the swept AC signal applied by the impedance analysis module is 1Hz-1MHz, which is used to measure the AC impedance spectrum of the membrane stack in the entire frequency band online. The electrode array is made of platinum electrodes and integrated on the flow channel partitions of the units at the beginning and end of the membrane stack. The electrodes and the flow channel partitions are bonded together with conductive adhesive.

[0048] S8. Aging test closed-loop calibration: Perform benchmark performance tests and graded accelerated aging tests on the integrated device, and send the test data back to the digital twin system to correct the performance degradation model and feed back to optimize production parameters. The graded accelerated aging test includes, in sequence, an acidic mode, an abrasion mode, and a hot-cold-wet cycle mode. The acidic mode uses simulated flue gas containing 450 ppm SO2, and the abrasion mode uses simulated flue gas containing 45 mg / m³ SO2. 3 The simulated flue gas containing dust was tested under alternating hot, cold, and humid conditions of 20-60℃ and 30-90%RH. The baseline performance test used simulated flue gas composed of 14% carbon dioxide, 4% oxygen, and 9% water vapor by volume, with nitrogen as the equilibrium gas, running continuously for 70 hours. The digital twin system received baseline performance test data, accelerated aging test data, and actual device operating data, automatically correcting the fluid distribution model, membrane performance degradation model, and interfacial bonding strength prediction model. The optimized hot-pressing encapsulation parameters and material grading standards were fed back to the production end. Each aging mode ran for 230 hours. After aging, the interfacial bonding strength and corresponding impedance spectrum data of the membrane module were retested. Test data was collected every hour and transmitted to the digital twin system in real time.

[0049] Example 3: This example provides a production process for a high-efficiency carbon dioxide capture device, including the following steps: S1. Substrate shell pretreatment: preparation of the outer shell of the equipment and the composite film support layer; The outer shell of the device is made of 316L stainless steel, which is sandblasted to Sa2.5 grade and then pickled and passivated to remove the surface oxide layer and oil stains. The composite membrane support layer is made of polysulfone material, which is formed by casting method and has a thickness of 150μm. After forming, it is washed with deionized water 3 times and vacuum dried at 65℃ for 12h for later use.

[0050] S2. Nanoparticle classification: The surface grafting degree of aminated mesoporous silica nanoparticles is detected, and they are classified according to the grafting degree range and the classification information is recorded. Among them, the surface grafting degree of the aminated mesoporous silica nanoparticles was 1.8 mmol / g, which belongs to the second level, corresponding to a hot-pressing temperature of 130℃ and a pressure of 0.7MPa. The grafting degree was determined by elemental analysis, and the grading information was entered into the production batch management system after the test was completed.

[0051] S3. Preparation of composite membrane precursor: A casting solution containing aminated mesoporous silica nanoparticles graded by S2 and a microencapsulated thermally initiated crosslinking agent was prepared. The film was formed on a polysulfone support layer by phase inversion method and dried at a temperature below the decomposition threshold of the crosslinking agent to obtain the composite membrane precursor. The microencapsulation thermal initiation crosslinking agent uses dicumyl peroxide as the core material and polyamide as the wall material, with a thermal decomposition threshold temperature of 125℃ and an addition amount of 3% of the total mass of the solute in the casting solution; the addition amount of aminated mesoporous silica nanoparticles is 15% of the total mass of the solute in the casting solution; the casting solution is prepared by dissolving polyether block amide in N,N-dimethylformamide to form a polymer solution and then adding the corresponding components, with a polymer solution mass fraction of 12%, a stirring rate of 500 r / min, and a stirring time of 3 h; the phase inversion method uses a water and ethanol mixed solution with a volume ratio of 3.2:1 as the coagulation bath, with a coagulation bath temperature of 30℃; the drying temperature is 65℃, the drying time is 28 h, and the vacuum degree is maintained at -0.09 MPa during the drying process; the ultrasonic dispersion power is 400 W, and the dispersion time is 1.5 h.

[0052] S4. Moisture-guiding baffle processing: Two-level microstructures are processed on the surface of the polytetrafluoroethylene flow channel baffle and regional selective modification is carried out to form a moisture-guiding microstructure with wettability gradient. The two-stage microstructure includes a primary main channel and a secondary capillary channel. The primary main channel has a width of 220 μm and a depth of 55 μm. The secondary capillary channel is at an angle of 65° to the main channel, with a width of 12 μm and a depth of 22 μm. Regional selective modification involves forming hydrophilic strips at the bottom of the capillary channel while maintaining hydrophobic properties in the main channel region. The microstructure is fabricated using laser etching with a laser power of 20 W and a scanning rate of 600 mm / s. Regional modification is performed using mask plasma treatment with a processing power of 100 W and a processing time of 20 s.

[0053] S5, Chemical-Physical Co-encapsulation: The composite film obtained in S3 and the flow channel partition obtained in S4 are alternately stacked to form a film stack. The hot-pressing parameters are matched according to the hierarchical information of S2 for hot-pressing encapsulation. When the hot-pressing temperature reaches the decomposition threshold of the crosslinking agent, in-situ crosslinking and interfacial grafting reactions are triggered to form chemically bonded enhanced encapsulation. The heat-pressing and pressure-holding time for the encapsulation process is 35 minutes, and the interfacial bonding strength of the encapsulated membrane module is no less than 8 MPa. The composite membrane is cut to a size of 410 mm × 610 mm, and machine vision is used to inspect membrane defects with an accuracy of 0.1 mm. 2 Unqualified membranes are rejected; each unit membrane stack has 22 layers, and the alignment error between the membrane and the flow channel partition is guaranteed to be no more than 0.5mm during stacking.

[0054] S6. System Integration and Assembly: Integrate the membrane module encapsulated by S5 with the pretreatment unit and compressor unit onto the frame, connect the pipelines and check for leaks; The pretreatment unit includes a cyclone dust collector and an activated carbon adsorption unit; leak detection uses helium gas, and the leakage rate is controlled to be less than 1×10⁻⁶. -6 mbar・L / s; the frame is made of carbon steel with a surface anti-corrosion coating; the compressor unit is a screw compressor unit with a pressure adjustment range of 0.1-2.5MPa; the pipeline uses quick-release flange connection, and the inner wall of the pipeline is pickled and passivated before connection.

[0055] S7. Impedance sensing system implantation: Electrode arrays are integrated at both ends of the membrane stack and connected to the impedance analysis module to form a dynamic impedance spectrum health sensing system. The electrode array forms a parallel plate capacitive sensing structure, and the electrode surface is coated with a polytetrafluoroethylene protective layer with a thickness of 7μm. The frequency range of the swept AC signal applied by the impedance analysis module is 1Hz-1MHz, which is used to measure the AC impedance spectrum of the membrane stack in the entire frequency band online. The electrode array is made of gold-plated copper electrodes and integrated on the flow channel partitions of the units at the beginning and end of the membrane stack. The electrodes and the flow channel partitions are bonded together with conductive adhesive.

[0056] S8. Aging test closed-loop calibration: Perform benchmark performance tests and graded accelerated aging tests on the integrated device, and send the test data back to the digital twin system to correct the performance degradation model and feed back to optimize production parameters. The graded accelerated aging test includes an acidic mode, an abrasion mode, and a hot-cold-wet cycle mode. The acidic mode uses simulated flue gas containing 550 ppm SO2, and the abrasion mode uses simulated flue gas containing 55 mg / m³ SO2. 3The simulated flue gas containing dust was tested under alternating hot, cold, and humid conditions at 20-60℃ and 30-90%RH. The baseline performance test used simulated flue gas composed of 16% carbon dioxide, 6% oxygen, and 11% water vapor by volume, with nitrogen as the equilibrium gas, running continuously for 74 hours. The digital twin system received baseline performance test data, accelerated aging test data, and actual device operating data, automatically correcting the fluid distribution model, membrane performance degradation model, and interfacial bonding strength prediction model. The optimized hot-pressing encapsulation parameters and material grading standards were fed back to the production end. Each aging mode ran for 250 hours. After aging, the interfacial bonding strength and corresponding impedance spectrum data of the membrane module were retested. Test data was collected every 30 minutes and transmitted to the digital twin system in real time.

[0057] Comparative Example 1: The only difference between this comparative example and Example 1 is that: in step S3, no microencapsulation thermal initiation crosslinking agent is added to the casting solution, and the amount of aminated mesoporous silica nanoparticles added is still 12.5% ​​of the total mass of the solute in the casting solution. The other raw material ratios, process steps and parameters are exactly the same as those in Example 1.

[0058] Comparative Example 2: The only difference between this comparative example and Example 1 is that in steps S2 and S3, the aminated mesoporous silica nanoparticles are replaced with an equal mass of unaminated mesoporous silica nanoparticles, surface grafting degree testing and grading are not performed, and the hot-pressing packaging parameters are uniformly adopted with a temperature of 118.5℃ and a pressure of 0.55MPa. The remaining raw material ratios, process steps and parameters are exactly the same as those in Example 1.

[0059] Comparative Example 3: The only difference between this comparative example and Example 1 is that in step S5, the hot-pressing encapsulation temperature is adjusted to 100℃, the pressure is 0.55MPa, and the heat and pressure holding time is 30min. The remaining raw material ratios, process steps and parameters are exactly the same as those in Example 1.

[0060] Comparative Example 4: The only difference between this comparative example and Example 1 is that the nanoparticle classification in step S2 is not performed, that is, the surface grafting degree of the aminated mesoporous silica nanoparticles is not detected and classified, and the unclassified nanoparticles are used directly to prepare the casting solution. In step S5, the hot-pressing encapsulation parameters are uniformly adopted with a temperature of 118.5℃ and a pressure of 0.55MPa. The remaining raw material ratios, process steps and parameters are exactly the same as those in Example 1.

[0061] Comparative Example 5: The only difference between this comparative example and Example 1 is that in step S4, the polytetrafluoroethylene flow channel baffle is only processed into the primary main channel, without processing the secondary capillary guide channel, and without performing regional selective modification to form hydrophilic strips. The remaining raw material ratios, process steps and parameters are exactly the same as in Example 1.

[0062] Comparative Example 6: This comparative example replaces the traditional monoethanolamine absorption process, using a 30wt% monoethanolamine aqueous solution as the absorbent. The absorption tower uses stainless steel structured packing, and the desorption tower is regenerated by steam heating. It does not involve steps such as membrane module preparation, moisture-conducting partition processing, chemical and physical co-encapsulation, impedance sensing system implantation, and digital twin closed-loop calibration.

[0063] I. Membrane Module Interface Bonding Strength Test, Test Standard: GB / T7122-2022 "Determination of Tensile Shear Strength of Adhesives (Rigid Material to Rigid Material)". This experiment was conducted in accordance with the above standard. The interface bonding strength of the membrane module samples of Examples 1-3 and Comparative Examples 1-6 was tested. The experimental environment temperature was controlled at 23℃ and the relative humidity was controlled at 50%. Each group of membrane module samples was cut into standard samples with a width of 25mm. A universal testing machine was used to apply tensile force along the interface direction between the membrane and the flow channel baffle at a tensile speed of 5mm / min. The maximum load when the sample peeled off was recorded. The interface bonding strength was calculated by the ratio of the maximum load to the effective contact area of ​​the sample. Each group of samples was tested in parallel 10 times, and the arithmetic mean was taken as the final test result.

[0064] II. Stability Test of Carbon Dioxide Capture Performance under High Humidity Conditions. Test Standard: GB / T30036-2013 "Test Method for Performance of Gas Separation Membrane". This experiment was conducted according to the above standard. Continuous operation tests were performed on the complete capture devices of Examples 1-3 and Comparative Examples 1-6. The experiment used simulated flue gas with a volume fraction of 15% carbon dioxide, 5% oxygen, 10% water vapor, and the remainder nitrogen. The flue gas inlet flow rate was controlled at 5 m³ / s. 3 The system operates at a pressure of 1.5 MPa and a temperature of 50°C for 720 hours. The carbon dioxide capture rate and gas pressure drop data are collected and recorded online every 24 hours. The performance degradation rate is calculated based on the difference between the initial capture rate and the capture rate after 720 hours. The pressure drop variation is also recorded throughout the process. Each unit is tested in parallel three times, and the average value of the stable operating data is taken as the final test result.

[0065] III. Reliability and Lifespan Simulation Testing of the Device Throughout its Life Cycle. Testing standards: GB / T2423.1-2008 "Environmental Testing for Electrical and Electronic Products - Part 2: Test Methods - Test A: Low Temperature", GB / T2423.2-2008 "Environmental Testing for Electrical and Electronic Products - Part 2: Test Methods - Test B: High Temperature", and GB / T2423.3-2016 "Environmental Testing - Part 2: Test Methods - Test Cab: Constant Damp Heat Test". This experiment comprehensively followed the above standards, conducting graded accelerated aging tests on the devices of Examples 1-3 and Comparative Examples 1-6. Three stages were carried out sequentially: acidic flue gas aging, dust scouring aging, and temperature and humidity alternating aging. Each stage lasted 240 hours. In the acidic aging stage, simulated flue gas containing 500 ppm sulfur dioxide was introduced, and in the dust scouring stage, the concentration was 50 mg / m³. 3 For micron-sized dust and flue gas, the temperature is controlled to cycle between 20℃ and 60℃ and the relative humidity to cycle between 30% and 90% during the temperature and humidity alternation stage. The performance changes of the membrane module are recorded throughout the aging process using an impedance spectroscopy monitoring system. The effective lifespan of the device is defined as the operating time when the membrane module's capture rate drops below 80%. At the same time, the occurrence time of faults such as interface failure, performance degradation, and sealing leakage is recorded. Each group of devices is tested once, and the continuous stable operating time and key fault node data are used as the evaluation criteria.

[0066] Table 1: Test results of interfacial bonding strength of membrane modules Sample number Interfacial bonding strength (MPa) Failure Mode Example 1 8.5 Cohesive failure of membrane materials Example 2 8.2 Cohesive failure of membrane materials Example 3 8.3 Cohesive failure of membrane materials Comparative Example 1 3.2 Interface adhesion failure Comparative Example 2 4.6 Mixed destruction Comparative Example 3 3.5 Interface adhesion failure Comparative Example 4 5.8 Mixed destruction Comparative Example 5 8.3 Cohesive failure of membrane materials Comparative Example 6 — not applicable Note: "Cohesive failure of membrane material" refers to the fracture occurring inside the membrane material itself, indicating that the interfacial bonding strength between the membrane and the flow channel partition has exceeded the strength of the membrane material itself, resulting in excellent encapsulation effect; "Interfacial adhesion failure" refers to the fracture occurring at the contact interface between the membrane and the flow channel partition, indicating insufficient bonding force between the two; "Hybrid failure" refers to the simultaneous presence of cohesive failure and interfacial failure on the fracture surface.

[0067] "—" indicates that Comparative Example 6 uses the traditional monoethanolamine absorption process, which does not involve membrane module preparation or the interfacial bonding between the membrane and the flow channel partition, and this test item is not applicable.

[0068] Table 2: Stability Test Results of Carbon Dioxide Capture Performance under High Humidity Conditions Sample number <![CDATA[Initial CO₂ capture rate (%)]]> <![CDATA[CO₂ capture rate after 720 hours (%)]]> Performance degradation rate (%) Pressure drop variation (kPa) Example 1 93.2 91.8 1.5 2.1 Example 2 91.5 89.6 2.1 2.8 Example 3 92.8 91.0 1.9 2.4 Comparative Example 1 92.5 89.2 3.6 3.5 Comparative Example 2 85.3 80.1 6.1 4.8 Comparative Example 3 92.3 88.9 3.7 3.6 Comparative Example 4 91.0 87.5 3.8 3.9 Comparative Example 5 92.8 <![CDATA[72.6 1 ]]> <![CDATA[21.8 1 ]]> <![CDATA[12.6 1 ]]> Comparative Example 6 88.5 84.2 4.9 8.5 Note: Data is superscripted " 1 "This indicates that the capture rate of Comparative Example 5 had dropped to 78.3% and the pressure drop had increased to 11.2 kPa after running for 580 hours. The performance further deteriorated after running for 720 hours. The data for 720 hours is the actual test value."

[0069] Performance degradation rate = (initial CO2 capture rate - CO2 capture rate after 720h) / initial CO2 capture rate × 100%. The lower the degradation rate, the better the long-term operational stability of the unit under high humidity flue gas conditions.

[0070] Table 3: Reliability and Lifetime Simulation Test Results of the Device Throughout Its Life Cycle Sample number Collection rate after acid aging (%) Dust collection rate after aging (%) Collection rate (%) after temperature and humidity alternation Effective lifespan of the device (h) Time to first failure (h) Fault type Example 1 91.2 90.5 89.8 >10000 >10000 No fault Example 2 89.8 88.9 88.0 >10000 >10000 No fault Example 3 90.5 89.6 89.0 >10000 >10000 No fault Comparative Example 1 87.5 85.3 <![CDATA[82.1 2 ]]> <![CDATA[5800 2 ]]> 4200 Interface layering Comparative Example 2 83.2 <![CDATA[79.6 3 ]]> <![CDATA[76.8 3 ]]> <![CDATA[3800 3 ]]> 2100 Performance degradation Comparative Example 3 87.0 85.0 <![CDATA[82.5 2 ]]> <![CDATA[5600 2 ]]> 4100 Interface layering Comparative Example 4 88.1 86.5 84.3 7200 5500 Interface layering Comparative Example 5 88.9 87.2 86.0 7500 — — Comparative Example 6 — — — 4500 1800 Equipment corrosion Note: Data is superscripted " 2 This indicates that the capture rate of the device was close to the 80% threshold at the end of the temperature and humidity alternating aging stage. It is inferred that it will drop below 80% after several hundred hours of continued operation, and the effective life of the device is calculated accordingly.

[0071] Data superscript " 3 "This indicates that the capture rate of the comparison ratio has dropped below 80% during the dust erosion aging stage, and all three levels of aging tests have not been completed. This data is the actual measured value at the end of the dust aging stage."

[0072] ">10000" indicates that after completing 720h graded accelerated aging, the capture rate of Examples 1-3 still remained above 88%. Based on the performance degradation trend extrapolation and combined with impedance spectrum monitoring data, the expected effective life of the device exceeds 10,000 hours. Actual testing is still ongoing.

[0073] "—" indicates that Comparative Example 6 uses the amine absorption method, and its failure modes are equipment corrosion and solvent degradation. This is different from the graded accelerated aging test system for membrane modules, and the data are not directly comparable.

[0074] "Fault-free" means that no faults such as interface delamination, seal leakage, or sudden drop in capture rate occurred during the entire accelerated aging test, and the impedance spectrum monitoring data did not show any abnormal shift.

[0075] As can be seen from Examples 1-3 and Comparative Example 1, and Tables 1 and 3, the microencapsulation thermal initiation crosslinking agent is the core component for achieving chemical-physical co-encapsulation. Its characteristic of being released in situ and participating in the reaction during hot pressing can transform the simple physical bond between the membrane and the flow channel partition into a composite bond enhanced by chemical bonding. Without this component, the interfacial bonding force relies solely on physical pressing, which cannot meet the long-term operation requirements under high pressure conditions, and is prone to membrane layer delamination, thereby shortening the service life of the device.

[0076] As can be seen from Examples 1-3 and Comparative Example 2, and Tables 1-3, amylation modification is the key to the dual role of mesoporous silica. The amino groups on its surface can serve as carbon dioxide adsorption sites to improve the capture efficiency, and can also serve as active sites for interfacial grafting reactions to enhance the encapsulation strength. Unamyled silica cannot participate in interfacial chemical bonding, nor can it provide enough adsorption sites, which will lead to a decrease in capture performance and insufficient interfacial bonding, thus accelerating the degradation of device performance.

[0077] Based on Examples 1-3 and Comparative Example 3, and in conjunction with Tables 1 and 3, it can be seen that the precise matching of hot-pressing temperature and the decomposition threshold of the microencapsulation crosslinking agent is a necessary condition for triggering the synergistic encapsulation mechanism. When the hot-pressing temperature is lower than the decomposition threshold, the microcapsule wall material will not rupture, the crosslinking agent cannot be released to participate in the reaction, the membrane and the separator are still physically bonded, the interfacial bonding strength cannot meet the design requirements, and the membrane layer will also face the risk of delamination under high pressure conditions.

[0078] Based on Examples 1-3 and Comparative Example 4, and in conjunction with Tables 1 and 3, it can be seen that the grading of grafting degree of aminated mesoporous silica and the pre-matching of hot-pressing parameters are the core means to ensure batch consistency of products. Nanoparticles with different grafting degrees require different hot-pressing conditions to achieve sufficient cross-linking grafting reaction. When using uniform parameters to process different batches of raw materials, some batches may not react sufficiently, resulting in large fluctuations in interfacial bonding strength and significant differences in performance between batches, which affects the quality stability of industrial production.

[0079] As can be seen from Examples 1-3 and Comparative Example 5, and Table 2, the synergistic design of the two-stage moisture-conducting microstructure and the wettability gradient is the key to solving the performance degradation under high humidity conditions. This structure can actively and directionally discharge the condensate that has permeated through the membrane using capillary force, preventing the condensate from accumulating between the membrane and the separator to form a water film. Without this structure, the condensate will continuously accumulate, increasing the mass transfer resistance, leading to a rapid decrease in the capture rate and a significant increase in the system pressure drop, which seriously affects the long-term operational stability of the device.

[0080] As can be seen from Examples 1-3 and Comparative Example 6, and Tables 2 and 3, the membrane separation process of the present invention has significant comprehensive advantages over the traditional monoethanolamine absorption method. It avoids the equipment corrosion, solvent evaporation and degradation problems commonly found in amine processes, has a more stable operation, lower maintenance costs, and effectively extends the service life of the device, making it more suitable for large-scale industrial carbon capture applications.

[0081] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A production process for a high-efficiency carbon dioxide capture device, characterized in that: Includes the following steps: S1. Substrate shell pretreatment: preparation of the outer shell of the equipment and the composite film support layer; S2. Nanoparticle classification: The surface grafting degree of aminated mesoporous silica nanoparticles is detected, and they are classified according to the grafting degree range and the classification information is recorded. S3. Preparation of composite membrane precursor: A casting solution containing aminated mesoporous silica nanoparticles graded by S2 and a microencapsulated thermally initiated crosslinking agent was prepared. The film was formed on a polysulfone support layer by phase inversion method and dried at a temperature below the decomposition threshold of the crosslinking agent to obtain the composite membrane precursor. S4. Moisture-guiding baffle processing: Two-level microstructures are processed on the surface of the polytetrafluoroethylene flow channel baffle and regional selective modification is carried out to form a moisture-guiding microstructure with wettability gradient. S5, Chemical-Physical Co-encapsulation: The composite film obtained in S3 and the flow channel partition obtained in S4 are alternately stacked to form a film stack. The hot-pressing parameters are matched according to the hierarchical information of S2 for hot-pressing encapsulation. When the hot-pressing temperature reaches the decomposition threshold of the crosslinking agent, in-situ crosslinking and interfacial grafting reactions are triggered to form chemically bonded enhanced encapsulation. S6. System Integration and Assembly: Integrate the membrane module encapsulated by S5 with the pretreatment unit and compressor unit onto the frame, connect the pipelines and check for leaks; S7. Impedance sensing system implantation: Electrode arrays are integrated at both ends of the membrane stack and connected to the impedance analysis module to form a dynamic impedance spectrum health sensing system. S8. Aging Test Closed-Loop Calibration: Perform benchmark performance tests and graded accelerated aging tests on the integrated device, transmit the test data back to the digital twin system, correct the performance degradation model, and provide feedback to optimize production parameters.

2. The production process of the high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S2, the surface grafting degree of the aminated mesoporous silica nanoparticles ranges from 1.2 to 1.8 mmol / g, wherein a grafting degree of 1.2 to 1.5 mmol / g is the first level, corresponding to a hot-pressing temperature of 115 to 122℃ and a pressure of 0.5 to 0.6 MPa; and a grafting degree of 1.5 to 1.8 mmol / g is the second level, corresponding to a hot-pressing temperature of 122 to 130℃ and a pressure of 0.6 to 0.7 MPa.

3. The production process of the high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S3, the microencapsulation thermal initiation crosslinking agent uses dicumyl peroxide as the core material and polyamide as the wall material, with a thermal decomposition threshold temperature of 115-125℃, and the amount added is 1-3% of the total mass of the solute in the casting solution; the amount added of the aminated mesoporous silica nanoparticles is 10-15% of the total mass of the solute in the casting solution.

4. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S3, the casting solution is prepared by dissolving polyether block amide in N,N-dimethylformamide to form a polymer solution and then adding the corresponding components. The phase inversion method uses a water and ethanol mixed solution with a volume ratio of (2.8-3.2):1 as the coagulation bath. The drying temperature is 55-65℃ and the drying time is 20-28h.

5. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S4, the two-stage microstructure includes a primary main channel and a secondary capillary channel. The primary main channel has a width of 180-220 μm and a depth of 45-55 μm. The secondary capillary channel has an angle of 55-65° with the main channel, a width of 8-12 μm, and a depth of 18-22 μm. The regional selective modification involves forming hydrophilic strips at the bottom of the capillary channel while maintaining hydrophobic properties in the main channel region.

6. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S5, the heat preservation and pressure holding time for hot-pressing encapsulation is 25-35 minutes, and the interfacial bonding strength of the encapsulated membrane module is not less than 8 MPa.

7. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S6, the pretreatment unit includes a cyclone dust collector and an activated carbon adsorption device; the leak detection uses helium gas, and the leakage rate is controlled to be less than 1×10⁻⁶. -6 mbar·L / s.

8. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S7, the electrode array forms a parallel plate capacitive sensing structure, and the electrode surface is coated with a polytetrafluoroethylene protective layer; the frequency range of the swept AC signal applied by the impedance analysis module is 1Hz-1MHz, which is used to measure the full-band AC impedance spectrum of the membrane stack online.

9. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S8, the graded accelerated aging test includes an acidic mode, an abrasion mode, and a hot-cold-humidity cycle mode. The acidic mode uses simulated flue gas containing SO2, the abrasion mode uses simulated flue gas containing dust, and the hot-cold-humidity cycle mode is carried out under alternating temperature and humidity conditions.

10. The production process of a high-efficiency carbon dioxide capture device according to claim 1, characterized in that: In step S8, the digital twin system receives benchmark performance test data, accelerated aging test data, and actual device operation data, automatically corrects the fluid distribution model, membrane performance degradation model, and interface bonding strength prediction model, and feeds back the optimized hot-pressing packaging parameters and material grading standards to the production end.