A porous graphene oxide composite nanofiltration membrane with an adhesive layer, its preparation method and application
By setting a polymer adhesive layer between the base membrane and the porous graphene oxide separation layer and crosslinking the porous graphene oxide separation layer, the problems of low flux and insufficient binding force of graphene oxide nanofiltration membranes are solved, achieving high flux and excellent salt/dye separation performance.
Patent Information
- Application Number
- CN202611196007.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-07
- Publication Date
- 2026-11-17
AI Technical Summary
Existing graphene oxide nanofiltration membranes have low flux and insufficient bonding between the graphene oxide membrane and the base membrane, making it easy for the membrane to detach in a wet state, making it difficult to achieve both high flux and dye rejection rate at the same time.
A polymer adhesive layer is set between the base film and the porous graphene oxide separation layer, and the porous graphene oxide separation layer is cross-linked with a cross-linking agent. Combined with pore-forming treatment of graphene oxide to form a porous structure, the bonding force between graphene oxide layers and between the base film is improved.
The structure stability and flux of the porous graphene oxide composite nanofiltration membrane were significantly improved, while the dye rejection rate was maintained or slightly increased, achieving high flux and excellent salt/dye separation performance.
Smart Images

Figure CN123102172A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a porous graphene oxide composite nanofiltration membrane with an adhesive layer, its preparation method and application, belonging to the field of nanofiltration membrane technology. Background Technology
[0002] The processing, weaving, and dyeing of cotton textile products are highly complex, with each process adding and generating different pollutants. In particular, the wastewater discharged from the dyeing stage contains large amounts of salts (typically including one or more of NaCl, Na2CO3, and Na2SO4), undyed dyes, and their hydrolysis products. This dyeing wastewater is high in salinity and color, making it difficult to treat biologically. Traditional methods treat this wastewater by mixing it with wastewater from other production stages, diluting the salinity and color, and then subjecting it to advanced treatment through physicochemical, biological, or combined physicochemical-biological methods before discharging it to meet standards. Even after meeting discharge standards, the wastewater still requires advanced oxidation or activated carbon adsorption for complete decolorization to meet reuse requirements. However, these steps inevitably lead to secondary environmental pollution.
[0003] Furthermore, the dyes used in the dyeing process of cotton textile products are reactive dyes, which are typically composed of dye matrix, reactive groups, linking groups, and leaving groups. The production of reactive dyes involves coupling and diazo reactions, during which a large amount of acid is added to adjust the pH, ultimately neutralizing to form salts. In addition, many reaction intermediates are of low purity and contain a large amount of salt. Therefore, the final synthesized dye contains a large amount of salt, unreacted intermediates, and reaction byproducts. Traditional cotton textile dyeing processes add electrolytes, so impurities such as salt in the dye do not significantly affect the dyeing process. However, with increasing environmental awareness, digital printing and non-aqueous dyeing of cotton textile products are gradually developing. Unlike traditional dyeing processes, digital printing uses reactive dyes to formulate printing inks, which have strict requirements on the salt content of the dyes; otherwise, it will cause inkjet nozzle clogging. Non-aqueous dyeing also has very high requirements on the salt content of the dyes; otherwise, it will lead to severe internal and external color differences. Therefore, it is necessary to desalt and purify reactive dyes to prepare high-purity salt-free dyes.
[0004] Loose nanofiltration is a membrane separation technology with pore sizes between ultrafiltration and nanofiltration. While ensuring high retention of organic dyes, it allows most inorganic salts to permeate, thus achieving efficient separation of organic dyes / salt water in dyeing and printing wastewater. It can also be applied to dye desalination and purification, possessing high economic value and research significance. However, most commercial nanofiltration membranes are organic membranes. Due to the inherent properties of polymer network structures, organic membranes have relatively wide pore sizes, poor selectivity, and poor fouling resistance. When treating high-salinity, high-color wastewater or desalinizing and purifying dyes, if a high dye retention rate is required, the organic membrane needs a smaller pore size. In this case, it also retains a certain amount of salt. Due to the osmotic pressure of this retained salt, the membrane flux is very low, making it difficult to simultaneously achieve high flux and dye retention rates.
[0005] Graphene oxide is a derivative of graphene and a single-layer, two-dimensional sheet-like carbon material. Recent studies have shown that water molecules can flow rapidly on the surface of graphene oxide, resulting in excellent separation performance. The surface of graphene oxide is rich in oxygen-containing functional groups such as hydroxyl, carboxyl, epoxy, and carbonyl groups, exhibiting good hydrophilicity. Therefore, it is easily dispersed in water to form a uniform dispersion, making it easy to prepare graphene oxide films.
[0006] Currently, graphene oxide nanofiltration membranes can be prepared using methods such as vacuum filtration, dip coating, spraying, layer-by-layer self-assembly, and coating, exhibiting excellent salt / dye separation performance. CN110523297A discloses a graphene oxide composite nanofiltration membrane and its preparation method. This preparation method includes the following steps: uniformly coating a graphene oxide dispersion onto one side of a base membrane using a coating rod, followed by drying and partial reduction under ultraviolet light irradiation to obtain the graphene oxide composite nanofiltration membrane. CN116020286A discloses a graphene oxide composite nanofiltration membrane, its preparation method, and its application. A mixture containing graphene oxide-like materials, polymer nanomaterials, and a crosslinking agent is coated onto the surface of a base membrane, and a crosslinking reaction is carried out to obtain the graphene oxide composite nanofiltration membrane.
[0007] While the two patents mentioned above provide preliminary solutions for the mass production of graphene oxide nanofiltration membranes, and CN116020286A achieves chemical cross-linking between graphene oxide layers by embedding polymer nanomaterials into the graphene oxide sheets using a cross-linking agent, thus improving the structural and chemical stability of the membrane, CN116020286A also preferentially uses positively charged modified nylon microfiltration membranes as the base membrane, utilizing the electrostatic attraction between the positive charge on its surface and the negatively charged graphene oxide to enhance the bonding force between the graphene oxide membrane and the base membrane. However, these patents do not perform pore-forming treatment on the graphene oxide. Although the flux of the graphene oxide membrane is improved compared to traditional organic membranes, it is still at a relatively low level, resulting in high membrane operating costs. Further significant improvements in the flux of graphene oxide membranes are still needed.
[0008] Therefore, developing a high-flux graphene oxide composite nanofiltration membrane that is simple to prepare, easy to mass-produce, has a stable interlayer structure of graphene oxide, excellent bonding between the graphene oxide membrane and the base membrane, and excellent salt / dye separation performance has become one of the urgent problems to be solved in this field. Summary of the Invention
[0009] To address the aforementioned technical problems, the present invention aims to provide a porous graphene oxide composite nanofiltration membrane with an adhesive layer, its preparation method, and its applications. The porous graphene oxide composite nanofiltration membrane of the present invention exhibits stable structure, excellent separation performance, and high flux.
[0010] To achieve the above objectives, a first aspect of the present invention provides a porous graphene oxide composite nanofiltration membrane with an adhesive layer, comprising a base membrane, a polymer adhesive layer, and a porous graphene oxide separation layer stacked sequentially; the porous graphene oxide separation layer contains porous graphene oxide, and the porous graphene oxide separation layer is formed on the surface of the polymer adhesive layer by crosslinking through a first crosslinking agent; the porous graphene oxide is obtained by creating pores in the graphene oxide using a pore-forming agent, the pore-forming agent comprising a main pore-forming agent and selectively including an auxiliary agent, wherein the main pore-forming agent is hydrogen peroxide.
[0011] A second aspect of the present invention provides a method for preparing the above-mentioned porous graphene oxide composite nanofiltration membrane with an adhesive layer, comprising the following steps: (1) A solution containing a polymer or a monomer that can be polymerized to form a polymer is applied to the base film, and after curing, a polymer adhesive layer is formed; (2) A mixture containing porous graphene oxide and a crosslinking agent is coated onto the surface of the polymer adhesive layer and crosslinking reaction is carried out to form a porous graphene oxide separation layer, thereby obtaining the porous graphene oxide composite nanofiltration membrane with the adhesive layer.
[0012] The third aspect of the present invention provides the application of the above-mentioned porous graphene oxide composite nanofiltration membrane with an adhesive layer in the treatment of high-salt wastewater containing dyes and / or the desalination and purification of salt-containing dyes.
[0013] The present invention has at least the following beneficial effects: This invention utilizes a polymer adhesive layer between the base membrane and the porous graphene oxide separation layer. The excellent fluidity of the polymer solution ensures uniform adhesion to the base membrane surface, significantly enhancing the bonding force between the porous graphene oxide separation layer and the base membrane, effectively preventing localized or complete detachment of the porous graphene oxide separation layer under wet conditions. Simultaneously, crosslinking the porous graphene oxide separation layer with a crosslinking agent enhances the interlayer bonding force, suppresses the water solubility effect of the porous graphene oxide separation layer, and improves the structural and chemical stability of the membrane. Furthermore, this invention creates nanoporous graphene oxide by creating pores in the graphene oxide, allowing water molecules to pass through while hindering the passage of large molecules such as dyes. This significantly increases the membrane flux while only slightly reducing the dye rejection rate. Moreover, the combined use of pore creation and enhanced crosslinking improves both flux and rejection rate and stability. The synergistic effect of these two methods allows for a significant increase in flux while maintaining or even slightly improving the dye rejection rate, further enhancing the stability of the GO membrane. Therefore, this invention develops a graphene oxide composite nanofiltration membrane that is simple to prepare, easy to mass-produce, has a stable interlayer structure of porous graphene oxide, excellent bonding between the porous graphene oxide membrane and the base membrane, high throughput, and excellent salt / dye separation performance. It can be applied to the treatment of high-salt dye wastewater containing dyes, desalination and purification of salt-containing dyes, and other fields. Attached Figure Description
[0014] Figure 1 The surface electron microscope image of the porous graphene oxide composite nanofiltration membrane prepared in Example 8.
[0015] Figure 2 This is a cross-sectional electron microscope image of the porous graphene oxide composite nanofiltration membrane of Example 8.
[0016] Figure 3 The images show the B0.1 and D0.3 membranes after testing.
[0017] Figure 4 The images show the actual composite membrane from Test Example 2 and the membrane after it has been peeled off with tape.
[0018] Figure 5 For the nylon-based membrane / porous GO membrane, nylon-based membrane / crosslinked porous GO membrane, and nylon-based membrane / PVA-N in Test Example 2. + A photograph of the polymer adhesive layer / crosslinked porous GO membrane after peeling.
[0019] Figure 6 This is a schematic diagram of the desalting and purification system for salt-containing dyes according to a specific embodiment of the present invention.
[0020] Figure 7 The images show the actual salt-containing dye, the dye solution after three rounds of concentration-dilution, and the low-salt dye solution after six rounds of concentration-dilution in Example 16.
[0021] Reference numerals: 1-Clear water tank; 2-Dye solution tank; 3-First membrane element; 4-Permeate tank; 5-Second membrane element; 6-Secondary permeate tank; 7-Feed line; 8-First permeate line; 9-Concentrate line; 10-Clear water flushing line; 11-Secondary feed line; 12-Secondary permeate line; 13-Secondary concentrate line; 14-First inlet valve; 15-First product water valve; 16-Cleaning valve; 17-First concentrate valve; 18-First booster pump; 19-Second booster pump; 20-Second inlet valve; 21-Second product water valve; 22-Second concentrate valve. Detailed Implementation
[0022] To provide a clearer understanding of the technical features, objectives, and beneficial effects of the present invention, the present invention will now be described in detail below, but this should not be construed as limiting the scope of the invention.
[0023] It should be noted that, unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.
[0024] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.
[0025] It should be understood that the terms “comprising,” “including,” and / or “containing” as used herein specify the presence of the stated features, integers, steps, components, or combinations thereof, but do not exclude the presence or addition of one or more other features, integers, steps, components, or combinations thereof.
[0026] The endpoints and any values of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of the various ranges, the endpoint values of the various ranges and individual point values, and individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this invention.
[0027] In the description of this invention, it should be noted that the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.
[0028] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installed", "equipped", "sleeved / connected", "connected", etc., should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium; it can be a connection within two components. For those skilled in the art, the specific meaning of the above terms in this invention can be understood according to the specific circumstances.
[0029] According to a specific embodiment of the first aspect of the present invention, the present invention provides a porous graphene oxide composite nanofiltration membrane with an adhesive layer, comprising a base membrane, a polymer adhesive layer, and a porous graphene oxide separation layer stacked sequentially; the porous graphene oxide separation layer contains porous graphene oxide, and the porous graphene oxide separation layer is formed on the surface of the polymer adhesive layer by crosslinking through a first crosslinking agent; the porous graphene oxide is obtained by creating pores in the graphene oxide using a pore-forming agent, the pore-forming agent comprising a main pore-forming agent and selectively comprising an auxiliary agent, wherein the main pore-forming agent is hydrogen peroxide.
[0030] Graphene oxide is mainly divided into sp 2 Graphene regions and sp 3 Graphene oxide regions. Graphene oxide films formed by the stacking or self-assembly of graphene oxide layers have a narrow interlayer spacing, which can effectively trap dyes while allowing most salts to pass through, offering unique advantages in the separation of salts and dyes. However, the interlayer bonding force of graphene oxide mainly relies on sp... 2 The π-π conjugation effect in the region means that the bonding force between the graphene oxide film and the base film mainly relies on the hydrogen bonds and van der Waals forces between the graphene oxide and the base film at the phase contact. When the film is in a dry state, the interlayer bonding force of the graphene oxide is good, and there is also a certain bonding force between the graphene oxide and the base film. The better the hydrophilicity of the base film, the better the bonding force between the base film and the graphene oxide film. For example, the bonding force between the graphene oxide film and the nylon base film is good, but the bonding force with the PVDF base film is poor.
[0031] However, due to the water-soluble effect of graphene oxide, when the graphene oxide film comes into contact with water, the carboxyl and hydroxyl groups on the graphene oxide will undergo hydration with the water, causing the interlayer expansion. 2The π-π conjugation effect in the region weakens or even disappears, resulting in weaker interlayer bonding in the graphene oxide film. Furthermore, the van der Waals forces of the hydrophilic groups between the graphene oxide film and the base film are significantly reduced, further weakening the bonding between them. Therefore, under the influence of water flow or external forces, the graphene oxide film is prone to localized damage, and may even detach directly from the base film. In practical applications, it has also been observed that in the early stages of membrane element fabrication or testing, the graphene oxide film may partially detach from the base film, leading to a lower dye rejection rate for the membrane element compared to the membrane sheet.
[0032] This invention utilizes chemical etching to create pores in graphene oxide sheets, expanding defects into 0.5-2 nm nanopores to obtain porous graphene oxide. Water molecules can pass through, while large molecules such as dyes cannot, thus significantly increasing the throughput of graphene oxide while only slightly reducing dye rejection. Furthermore, this invention incorporates a polymer adhesive layer between the base film and the porous graphene oxide separation layer, along with cross-linking the porous graphene oxide. This significantly enhances the bonding force between the porous graphene oxide separation layer and the base film, as well as the interlayer structural stability of the porous graphene oxide, effectively suppressing localized or complete detachment of the porous graphene oxide separation layer under wet conditions.
[0033] Specifically, the polymer solution used in the polymer adhesive layer has good fluidity, enabling it to adhere uniformly to the surface of the base film and firmly bond with it through van der Waals forces and physical intercalation. Simultaneously, the numerous hydrophilic groups (such as hydroxyl, carboxyl, and amino groups) on the polymer can interact with the hydrophilic groups on the porous graphene oxide through van der Waals forces and hydrogen bonds; amino groups can also form covalent amide bonds with the carboxyl groups on the porous graphene oxide; furthermore, quaternary ammonium salt-modified polymers can be selected, whose quaternary ammonium groups (positively charged) bond with the carboxyl groups (negatively charged) of the porous graphene oxide through ionic bonds, thereby firmly fixing the porous graphene oxide separation layer onto the base film and significantly improving the adhesion between the porous GO membrane and the base film.
[0034] Furthermore, ionic or chemical crosslinking of porous graphene oxide can enhance the interlayer bonding force, suppress the water solubility effect of the porous graphene oxide film, and improve its structural and chemical stability. While increasing the degree of crosslinking alone can improve the rejection rate, it will significantly reduce the flux. However, this invention combines pore-forming and crosslinking—pore-forming significantly increases the intrinsic flux of graphene oxide, providing a flux margin to withstand higher crosslinking agent dosages, while moderate crosslinking compensates for the decrease in rejection rate caused by pore-forming and further enhances the interlayer bonding force. The result of the synergistic effect of these two methods is that while maintaining or even slightly increasing the dye rejection rate, a 2-6 times increase in flux is achieved, along with superior membrane stability.
[0035] In some embodiments, the pore-forming agent includes one or more of a strong oxidizing agent, an inorganic base, an organic base, and a ferrous salt. Preferably, the strong oxidizing agent includes one or more of sodium hypochlorite, ozone, and potassium permanganate. Preferably, the inorganic base includes NaOH and / or ammonia. Preferably, the organic base includes C6-C12 tertiary amine compounds. More preferably, the organic base includes one or more of triethylamine, tripropylamine, and tributylamine. Preferably, the ferrous salt includes ferrous sulfate and / or ferrous chloride.
[0036] In some embodiments, during the process of preparing porous graphene oxide by creating pores in graphene oxide with a pore-forming agent, the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, preferably (3-20):1.
[0037] In some embodiments, the sheet size of the graphene oxide is 0.5-100 μm, preferably 3-10 μm.
[0038] In some embodiments, the pore-forming agent is hydrogen peroxide, or a combination of sodium hypochlorite and hydrogen peroxide, or a combination of hydrogen peroxide and a ferrous salt, or a combination of hydrogen peroxide and ammonia, or a combination of hydrogen peroxide and an organic base. Preferably, the pore-forming agent is a combination of sodium hypochlorite and hydrogen peroxide, or a combination of hydrogen peroxide and a ferrous salt, or a combination of hydrogen peroxide and ammonia, or a combination of hydrogen peroxide and an organic base.
[0039] In some embodiments, when the pore-forming agent is hydrogen peroxide, the porous graphene oxide is prepared by forming pores in graphene oxide using the pore-forming agent. This includes reacting a mixed solution of graphene oxide and hydrogen peroxide at 45-60°C for 6-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, to obtain the porous graphene oxide. Preferably, the mass ratio of hydrogen peroxide to graphene oxide is (3-20):1. Preferably, the content of graphene oxide in the mixed solution of graphene oxide and hydrogen peroxide is 0.25-10 mg / mL, more preferably 1-4 mg / mL. When hydrogen peroxide is used alone to etch graphene oxide for pore formation, because hydrogen peroxide has a relatively mild oxidizing property, it can usually only etch existing defects on the graphene oxide sheets to form pores, and it is difficult to etch more defects by its own oxidizing property, thus the pore-forming effect is limited. Meanwhile, this reaction generally needs to be carried out at a relatively high temperature (the reaction is extremely slow at around 25°C at room temperature), but excessively high temperatures may cause graphene oxide to be reduced and its dispersibility to deteriorate. Therefore, using hydrogen peroxide alone as a pore-forming agent is not a preferred solution of this invention.
[0040] In some embodiments, when the pore-forming agent is a combination of sodium hypochlorite and hydrogen peroxide, the porous graphene oxide is prepared by creating pores in the graphene oxide using the pore-forming agent. This process includes: first, reacting a mixed solution of graphene oxide and sodium hypochlorite at 5-25°C for 12-30 hours, with the mass ratio of sodium hypochlorite to graphene oxide being 1:100-1:10, to obtain pretreated graphene oxide; then, reacting the mixed solution of the pretreated graphene oxide and hydrogen peroxide at 45-60°C for 12-48 hours, with the mass ratio of hydrogen peroxide to the pretreated graphene oxide being (1-100):1, to obtain the porous graphene oxide. Preferably, the mass ratio of hydrogen peroxide to the pretreated graphene oxide is (3-20):1. Preferably, the graphene oxide content in the mixed solution of graphene oxide and sodium hypochlorite is 0.25-10 mg / mL, more preferably 1-4 mg / mL. Hydrogen peroxide's oxidizing properties are not particularly strong; it can typically only etch existing defects into pores on graphene oxide sheets, and it is difficult to etch out more defects using its own oxidizing properties. This invention preferably uses a small amount of sodium hypochlorite, which has stronger oxidizing properties, to etch out more defects on the graphene oxide sheets at a lower temperature beforehand, and then uses mild hydrogen peroxide to etch out more pores, thereby increasing the pore density and etching efficiency.
[0041] In some embodiments, when the pore-forming agent is a combination of hydrogen peroxide and ferrous salt, the porous graphene oxide is prepared by creating pores in the graphene oxide using the pore-forming agent. This includes reacting a mixed solution of graphene oxide, hydrogen peroxide, and ferrous salt at 25-45°C for 12-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the mass ratio of ferrous salt to graphene oxide is 1:100-1:10, thereby obtaining the porous graphene oxide. Preferably, the mass ratio of hydrogen peroxide to graphene oxide is (3-20):1. Preferably, the graphene oxide content in the mixed solution of graphene oxide, hydrogen peroxide, and ferrous salt is 0.25-10 mg / mL, more preferably 1-4 mg / mL. The present invention preferably uses Fe... 2+ When used in conjunction with hydrogen peroxide, the Fenton reaction generates more potent hydroxyl radicals (·OH), which can etch more pores at lower temperatures, significantly improving pore-forming efficiency. Furthermore, the Fe generated by the Fenton reaction... 3+ Hydrolysis forms iron colloids (such as Fe(OH)3). These iron colloids interact with the graphene oxide sheets, increasing the effective particle size of the graphene oxide. This makes the graphene oxide easier to separate by centrifugal sedimentation, facilitating subsequent removal of residual H2O2 and Fe by centrifugal washing. 2+ and newly generated Fe 3+ .
[0042] In some embodiments, when the pore-forming agent is a combination of hydrogen peroxide and ammonia, the porous graphene oxide is prepared by forming pores in the graphene oxide using the pore-forming agent. This includes reacting a mixed solution of graphene oxide, hydrogen peroxide, and ammonia at 25-45°C for 12-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the ammonia is used to adjust the pH of the mixed solution to 9-12.5, thereby obtaining the porous graphene oxide. Preferably, the mass ratio of hydrogen peroxide to graphene oxide is (3-20):1. Preferably, the graphene oxide content in the mixed solution of graphene oxide, hydrogen peroxide, and ammonia is 0.25-10 mg / mL, more preferably 1-4 mg / mL. The present invention preferably uses a combination of hydrogen peroxide and ammonia. Under alkaline conditions (the pH is adjusted to 9-12.5 by ammonia), hydrogen peroxide undergoes alkaline catalytic decomposition, which generates reactive oxygen species with stronger oxidizing power. These reactive oxygen species have a significantly stronger oxidizing ability than hydrogen peroxide itself, and can etch more pores at lower temperatures, thereby improving pore-forming efficiency.
[0043] In some embodiments, when the pore-forming agent is a combination of hydrogen peroxide and an organic base, the porous graphene oxide is prepared by forming pores in the graphene oxide using the pore-forming agent. This includes reacting a mixed solution of graphene oxide, hydrogen peroxide, and an organic base at 25-60°C for 2-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the mass ratio of the organic base to hydrogen peroxide is 1:2-1:20, thereby obtaining the porous graphene oxide. Preferably, the mass ratio of hydrogen peroxide to graphene oxide is (3-20):1. Preferably, the mass ratio of the organic base to hydrogen peroxide is 1:5-1:10. Preferably, the organic base includes a C6-C12 tertiary amine compound. More preferably, the organic base includes one or more of triethylamine, tripropylamine, and tributylamine. Preferably, the graphene oxide content in the mixed solution of graphene oxide, hydrogen peroxide, and organic base is 0.25-10 mg / mL, more preferably 1-4 mg / mL. This invention preferably uses a combination of hydrogen peroxide and an organic base, where the organic base promotes the alkaline-catalyzed decomposition of hydrogen peroxide to generate hydrogen peroxide anions (HO2). - More reactive oxygen species, such as hydroxyl radicals (·OH), can be used to etch more pores at lower temperatures, improving pore-forming efficiency. Meanwhile, compared to ammonia, organic bases have higher boiling points and are less prone to volatilization during the reaction, maintaining a more stable alkaline environment. Further optimized C6-C12 tertiary amine compounds lack NH bonds, are less susceptible to consumption by hydrogen peroxide, and are more stable in the reaction system.
[0044] Existing technologies include methods for preparing porous graphene oxide by etching graphene oxide with alkaline solutions or oxidizing agents. However, alkaline heat treatment, while etching nanopores, can also reduce graphene oxide, leading to decreased dispersibility and even solution aggregation. In contrast, this invention uses hydrogen peroxide as the primary pore-forming agent, which etches nanopores without reducing the dispersibility of graphene oxide. After etching, residual hydrogen peroxide can be removed by multiple rounds of centrifugation. However, it should be noted that the etching process reduces the size of graphene oxide sheets, making centrifugal separation difficult. Furthermore, since the reaction rate between hydrogen peroxide and graphene oxide is slow at room temperature or low temperatures, when using an oxidation-resistant first crosslinking agent, residual hydrogen peroxide can be left unremoved after etching, and subsequent crosslinking steps can be performed directly, thus simplifying the process. Alternatively, manganese dioxide can be added to catalyze the decomposition of hydrogen peroxide, followed by centrifugation at low speed (500-2000 rpm) to obtain porous graphene oxide from the supernatant. Alternatively, porous graphene oxide can be centrifuged at high speed (10,000-15,000 rpm) and hydrogen peroxide can be removed by multiple rounds of centrifugation-washing dispersion.
[0045] This invention uses hydrogen peroxide as the primary pore-forming agent, and preferably supplements it with the aforementioned NaClO, ammonia, and Fe. 2+ Chemical etching of graphene oxide using additives such as organic bases can enhance pore-forming effects and create nanoscale pores. Among these, the combination of hydrogen peroxide and C6-C12 tertiary amine compounds is the most preferred pore-forming agent combination. Compared to NaClO, tertiary amine compounds regulate the decomposition rate of hydrogen peroxide through a base catalytic mechanism, resulting in a gentler etching process that is beneficial for forming nanopores with uniform pore size. NaClO, on the other hand, has strong oxidizing properties, which may lead to over-oxidation of graphene oxide sheets or even structural damage; the combination of Fe... 2+ In comparison, tertiary amine compounds do not contain metal ions, resulting in a cleaner reaction system that eliminates the need for subsequent iron removal steps and avoids the uncontrollable pore size problem caused by the excessively rapid generation rate of hydroxyl radicals in the Fenton reaction. Compared to ammonia, tertiary amine compounds have higher boiling points and are less volatile. They also do not contain NH bonds and are not consumed by hydrogen peroxide, thus maintaining a more stable alkaline environment throughout the reaction process. This leads to the production of porous graphene oxide with a more uniform pore size distribution and higher pore density.
[0046] In some embodiments, the porous graphene oxide exhibits a bimodal pore size distribution, comprising micropores and macropores. The average pore size of the micropores is 0.5-2 nm, and the average pore size of the macropores is 2-50 nm (preferably 10-50 nm). The micropores account for more than 75% of the total number of pores (preferably more than 80%, more preferably more than 85%, and even more preferably more than 90%). The micropores are nanofiltration functional pores, allowing water molecules and inorganic salt ions to pass through while retaining dye molecules. The macropores are mainly defects at the edges of graphene oxide sheets or interlayer pores. The porous graphene oxide of the present invention, dominated by micropores, exhibits high salt / dye separation performance.
[0047] In some embodiments, the first crosslinking agent comprises an ionic crosslinking agent and / or a first chemical crosslinking agent. Preferably, the ionic crosslinking agent comprises Ca... 2+ Mg 2+ and Fe 3+ One or more of the following. More preferably, the ionic crosslinking agent is Fe. 3+ Preferably, the first chemical crosslinking agent includes one or more of carboxyl crosslinking agents, hydroxyl crosslinking agents, and multifunctional crosslinking agents. More preferably, the carboxyl crosslinking agent includes one or more of polyamines, multifunctional aziridines, and polycarbodiimides; the hydroxyl crosslinking agent includes one or more of polyaldehydes, isocyanates, and borax; and the multifunctional crosslinking agent includes polyphenols and / or siloxanes. Specifically, the first chemical crosslinking agent includes one or more of tannic acid, glutaraldehyde, borax, polyethyleneimine, 3-aminopropyltriethoxysilane, and (3-glycidylpropoxy)trimethoxysilane. It is understood that the carboxyl crosslinking agent refers to a crosslinking agent that mainly reacts with carboxyl groups (-COOH), the hydroxyl crosslinking agent refers to a crosslinking agent that mainly reacts with hydroxyl groups (-OH), and the multifunctional crosslinking agent refers to a crosslinking agent that contains two or more functional groups that can participate in the crosslinking reaction and can achieve crosslinking through covalent bonds and / or non-covalent bond interactions (such as hydrogen bonds, hydrophobic interactions, coordination bonds, etc.).
[0048] In some embodiments, the first crosslinking agent accounts for 1-50% of the mass of the porous graphene oxide, preferably 3-30%.
[0049] In some embodiments, the porous graphene oxide separation layer further contains polymeric nanomaterials. Preferably, the polymeric nanomaterials include one or more of the following: cellulose nanofibers, cellulose nanocrystals, chitin nanofibers, chitin nanocrystals, chitosan nanofibers, chitosan nanocrystals, lignin nanofibers, and lignin nanocrystals. Preferably, the mass ratio of the polymeric nanomaterials to the porous graphene oxide is (0.5-5):1.
[0050] In some embodiments, the thickness of the porous graphene oxide separation layer is 10-500 nm, preferably 20-100 nm.
[0051] In some embodiments, the polymer adhesive layer is formed by applying a solution containing a polymer or monomers that can polymerize to the base film and then curing it.
[0052] In some embodiments, the polymer includes one or more of the following: polyvinyl alcohol (PVA), polyacrylic acid (PAA), chitosan (CS), carbomer, guar gum, polyethyleneimine (PEI), polydiallyldimethylammonium chloride (PDDA), positively charged polyvinyl alcohol, positively charged polyacrylic acid, positively charged chitosan, positively charged carbomer, and positively charged guar gum. Preferably, the polymer is one or more of the following: PVA, a combination of PVA and PAA, quaternary ammonium salt modified positively charged PVA, and chitosan.
[0053] In some embodiments, the polymerizable monomers include dopamine, or a mixture of soybean oil, malic acid, and tannic acid.
[0054] In some embodiments, the mass content of the polymer or the total mass content of the monomer in the solution containing the polymer or monomers that can polymerize to form a polymer is 0.1-5%, preferably 0.25-2%.
[0055] The polymer adhesive layer of the present invention is formed by coating the base film surface or immersing the base film in a solution containing polymers or monomers that can polymerize to form polymers and then curing it. It can firmly bond the base film and the porous graphene oxide separation layer together.
[0056] In some embodiments, the solution containing a polymer or a monomer capable of polymerizing into a polymer further contains a second crosslinking agent, which includes a second chemical crosslinking agent. Preferably, the second chemical crosslinking agent includes one or more of carboxyl crosslinking agents, hydroxyl crosslinking agents, and amino crosslinking agents. More preferably, the second chemical crosslinking agent includes one or more of polyaldehydes, borax, and polyfunctional aziridines.
[0057] In some embodiments, the second crosslinking agent accounts for 1-30% of the mass of the polymer or the monomer that can polymerize to form the polymer, preferably 3-10%.
[0058] The present invention preferably employs a chemical crosslinking agent in a solution containing polymers or monomers that can polymerize to form polymers. This agent can react with the hydroxyl, carboxyl, or amino groups on the polymer, causing the water-soluble polymer adhesive layer to crosslink and form a crosslinked network, thereby improving its structural stability and water resistance. Furthermore, the crosslinked network can enhance the physical interlocking between the polymer adhesive layer and the base film, further improving the overall structural stability of the composite film.
[0059] In some embodiments, the solvent in the solution containing the polymer or monomer that can polymerize to form a polymer is water or a mixture of water and an organic solvent. Preferably, the organic solvent is an alcohol solvent. More preferably, the organic solvent is ethanol and / or isopropanol. The addition of an alcohol solvent can adjust the surface tension of the polymer or monomer solution, resulting in appropriate affinity between the solution and the base film. This facilitates uniform coating of the solution onto base films of different materials without excessive penetration into the interior of the base film.
[0060] In some embodiments, the thickness of the polymer adhesive layer is 1-1000 nm, preferably 5-50 nm.
[0061] In some embodiments, the porous graphene oxide composite nanofiltration membrane with an adhesive layer further includes a polymer protective layer located on the side of the porous graphene oxide separation layer away from the polymer adhesive layer. Preferably, the polymer protective layer is made of one or more of the following: neutral polyvinyl alcohol (PVA), polyethylene oxide (PEO), negatively charged sodium polyacrylate (PAA), sodium alginate (SA), carboxyl-modified polyvinyl alcohol, positively charged polyethyleneimine (PEI), polydiallyldimethylammonium chloride (PDDA), chitosan (CS), and quaternary ammonium salt-modified positively charged polyvinyl alcohol. Preferably, the thickness of the polymer protective layer is 10-300 nm.
[0062] For certain specialized applications (such as those requiring frequent physicochemical cleaning or where complete prevention of graphene oxide shedding is necessary), this invention allows for the coating of a polymer protective layer onto the surface of the porous graphene oxide separation layer. Its primary function is to further protect the porous graphene oxide separation layer from external damage, while also altering its charge properties to adjust separation performance, such as rejection rate. This polymer protective layer is rich in hydroxyl, carboxyl, amino, or quaternary ammonium groups, which can tightly bind to the porous graphene oxide through van der Waals forces, hydrogen bonds, covalent bonds, and ionic bonds, providing further protection and increasing antifouling properties. Furthermore, by applying polymer protective layers with different charges, the charge properties of the composite nanofiltration membrane can be altered, thereby adjusting the separation performance of the porous graphene oxide separation layer as needed.
[0063] In some embodiments, the base membrane is an ultrafiltration membrane or a microfiltration membrane. Preferably, the average pore size of the base membrane is 0.01-5 μm, more preferably 0.05-0.5 μm.
[0064] In some embodiments, the base film is made of one or more of the following materials: nylon (such as PA6 or PA66), polyethersulfone (PES), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), cellulose acetate (CA), and polypropylene (PP). Preferably, the base film is made of one or more of the following materials: nylon 6, polyethersulfone, and polyvinylidene fluoride.
[0065] In some embodiments, the thickness of the base film is 50-200 μm.
[0066] In some embodiments, the porous graphene oxide composite nanofiltration membrane with an adhesive layer has a molecular weight cutoff of 1,000-5,000 Daltons, a rejection rate of ≥95% for reactive dyes, and a rejection rate of <12% for inorganic salts (i.e., desalination rate).
[0067] According to a specific embodiment of the second aspect of the present invention, the present invention provides a method for preparing the above-mentioned porous graphene oxide composite nanofiltration membrane with an adhesive layer, which includes the following steps: (1) A solution containing a polymer or a monomer that can be polymerized to form a polymer is applied to the base film, and after curing, a polymer adhesive layer is formed; (2) A mixture containing porous graphene oxide and a crosslinking agent is coated onto the surface of the polymer adhesive layer and crosslinking reaction is carried out to form a porous graphene oxide separation layer, thereby obtaining the porous graphene oxide composite nanofiltration membrane with the adhesive layer.
[0068] In some embodiments, in step (1), the solution containing a polymer or a monomer that can polymerize to form a polymer is applied to the base film by one or more of the following methods: spraying, blade coating, bar coating, slot coating, microgravure coating, and immersion, preferably bar coating and / or immersion.
[0069] In some embodiments, in step (1), the solution containing a polymer or a monomer that can polymerize to form a polymer is applied to the base film to form a polymer adhesive layer wet film, the thickness of which is 1-10 μm.
[0070] In some embodiments, in step (1), the curing temperature is 20-100°C and the time is 1 minute to 48 hours.
[0071] In some embodiments, in step (2), the mixture containing porous graphene oxide and crosslinking agent further contains polymeric nanomaterials.
[0072] In some embodiments, in step (2), the content of porous graphene oxide in the mixture containing porous graphene oxide and crosslinking agent is 1-10 mg / mL, preferably 2-5 mg / mL.
[0073] In some embodiments, in step (2), the method of coating the mixture containing porous graphene oxide and crosslinking agent onto the surface of the polymer adhesive layer includes one or more of the following: blade coating, wire bar coating, slot coating, and microgravure coating.
[0074] In some embodiments, in step (2), a mixture containing porous graphene oxide and a crosslinking agent is coated onto the surface of the polymer adhesive layer to form a porous graphene oxide separation layer wet film, wherein the thickness of the porous graphene oxide separation layer wet film is 5-100 μm, preferably 10-25 μm.
[0075] In some embodiments, in step (2), the crosslinking reaction is carried out at a temperature of 20-100°C for a time of 5 minutes to 48 hours.
[0076] In some embodiments, the preparation method further includes step (3): coating a polymer-containing solution onto the surface of the porous graphene oxide separation layer, and drying it to form a polymer protective layer.
[0077] The porous graphene oxide composite nanofiltration membrane with an adhesive layer of the present invention has a simple preparation process and is easy to mass-produce. Furthermore, the porous graphene oxide composite nanofiltration membrane of the present invention has a stable structure, good bonding force between the porous graphene oxide separation layer and the base membrane, stable performance, and excellent inorganic salt / dye separation performance. It can be applied to the treatment of high-salt wastewater containing dyes, desalination and purification of salt-containing dyes, and purification of municipal water.
[0078] According to a specific embodiment of the third aspect of the present invention, the present invention provides the application of the above-described porous graphene oxide composite nanofiltration membrane with an adhesive layer in the treatment of high-salt wastewater containing dyes and / or the desalination and purification of salt-containing dyes.
[0079] In some embodiments, the salt concentration in the dye-containing high-salt wastewater is above 20 g / L, and the dye concentration is 0.1-5 g / L. Preferably, the salt includes one or more of NaCl, Na2SO4, and Na2CO3.
[0080] In some embodiments, the porous graphene oxide composite nanofiltration membrane with an adhesive layer has a flux of 4-20 L / (m³) for treating the high-salt wastewater containing dyes. 2(·h·Bar), dye retention rate is 95%-99.9%, desalination rate is <12%.
[0081] In some embodiments, the salt-containing dye contains dye, by-products, unreacted intermediates, and salt, the total concentration of the dye, by-products, unreacted intermediates, and salt being 100 g / L or more, and the by-products, unreacted intermediates, and salt accounting for 20-50% (by mass) of the total solid content of the salt-containing dye.
[0082] The technical solutions of the present invention are specifically illustrated below through embodiments, but the present invention is not limited to these embodiments. Of course, various modifications can be made within the scope of the key points of the present invention.
[0083] Test method: Pore size characterization of porous graphene oxide: The pore size distribution of porous graphene oxide was determined by nitrogen adsorption-desorption (BET). The pore morphology on the surface of porous graphene oxide sheets was observed by atomic force microscopy (AFM). The pore size of each pore in the AFM images was measured and counted to obtain the pore size distribution in terms of the number of pores. Based on this, the proportion of small pores (0.5-2 nm) to the total number of pores was calculated.
[0084] Molecular weight cutoff (MWCO) test: A 1 g / L solution of polyethylene glycol (PEG) standard with different molecular weights was prepared as the feed solution, and the cutoff rate was tested at 25℃ and 1 Bar. The PEG molecular weight corresponding to a cutoff rate of 90% is the molecular weight cutoff of the membrane.
[0085] Preparation Example 1
[0086] A mixed aqueous solution containing 2.5 mg / mL GO (with sheet size of 3-10 μm; the same GO was used in the following preparation examples) and 50 mg / mL H2O2 was prepared and reacted with continuous stirring at 60 °C for 6 h to obtain porous graphene oxide. After the reaction, residual H2O2 was removed by centrifugation and washing 3-4 times, and the solution was refrigerated for later use.
[0087] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 1.3 nm, and the average pore size of the macropores is 45 nm. In terms of the number of pores, the micropores account for 78% of the total number of pores.
[0088] Preparation Example 2
[0089] A mixed aqueous solution containing 4 mg / mL GO and 0.25 mg / mL NaClO was prepared and reacted with continuous stirring at room temperature for 24 h to obtain porous graphene oxide. Subsequently, H2O2 (12.5 mg / mL) was added to the solution, and the reaction was carried out at 60℃ for 30 h to prepare porous graphene oxide. After the reaction, residual NaClO and H2O2 were removed by 3-4 rounds of centrifugation washing, and the solution was sealed and stored at room temperature for later use.
[0090] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 1.4 nm, and the average pore size of the macropores is 40 nm. In terms of the number of pores, the micropores account for 88% of the total number of pores.
[0091] Preparation Example 3
[0092] A 3 mg / mL GO aqueous solution was prepared, followed by the addition of H2O2 (30 mg / mL) and FeSO4 (0.08 mg / mL). The mixture was stirred continuously at 45 °C for 15 h to obtain porous graphene oxide. After the reaction, residual H2O2 and iron ions were removed by centrifugation and washing 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0093] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 1.5 nm, and the average pore size of the macropores is 35 nm. In terms of the number of pores, the micropores account for 92% of the total number of pores.
[0094] Preparation Example 4
[0095] A 4 mg / mL GO aqueous solution was prepared, followed by the addition of 20 mg / mL H2O2 and the adjustment of the pH to 12 with ammonia. The reaction was carried out with continuous stirring at 40 °C for 30 h to obtain porous graphene oxide. After the reaction, residual H2O2 was removed by centrifugation and washing 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0096] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 1.4 nm, and the average pore size of the macropores is 38 nm. In terms of the number of pores, the micropores account for 90% of the total number of pores.
[0097] Preparation Example 5
[0098] A 4 mg / mL GO aqueous solution was prepared, followed by the addition of H2O2 (20 mg / mL) and triethylamine (2 mg / mL). The mixture was stirred continuously at 50 °C for 4 h to obtain porous graphene oxide. After the reaction, residual H2O2 and triethylamine were removed by centrifugation and washing 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0099] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 1.6 nm, and the average pore size of the macropores is 32 nm. In terms of the number of pores, the micropores account for 94% of the total number of pores.
[0100] Comparative Preparation Example 1
[0101] A 4 mg / mL GO aqueous solution was prepared, and then concentrated sulfuric acid (50 mg / mL based on pure substance) was added to it. After stirring continuously at room temperature for 2 h, porous graphene oxide was obtained. After the reaction, residual concentrated sulfuric acid was removed by centrifugation 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0102] The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 2.5 nm, and the average pore size of the macropores is 30 nm. In terms of the number of pores, the micropores account for 45% of the total number of pores.
[0103] Comparative Preparation Example 2
[0104] A 4 mg / mL GO aqueous solution was prepared, and then NaOH (20 mg / mL) was added to it. After stirring continuously at 80 °C for 4 h, porous graphene oxide was obtained. After the reaction, residual NaOH was removed by centrifugation and washing 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0105] The porous graphene oxide has a wide pore size distribution and does not exhibit a typical bimodal distribution, with an average pore size of 4.8 nm. In terms of the number of pores, pores with a diameter in the range of 0.5-2 nm account for 35% of the total number of pores.
[0106] Comparative preparation example 3
[0107] A 4 mg / mL GO aqueous solution was prepared, and then potassium permanganate (5 mg / mL) was added. After stirring continuously at room temperature for 6 h, porous graphene oxide was obtained. After the reaction, residual potassium permanganate and the generated manganese compounds were removed by centrifugation and washing 3-4 times, and the solution was sealed and stored at room temperature for later use.
[0108] The porous graphene oxide has a wide pore size distribution and does not exhibit a typical bimodal distribution, with an average pore size of 3.2 nm. In terms of the number of pores, pores with a diameter in the range of 0.5-2 nm account for 40% of the total number of pores.
[0109] In the examples and comparative examples below, solutions for forming polymer adhesive layers were prepared according to the components in Table 1, and then wire-coated onto a base film to form a wet polymer adhesive layer. After curing at the temperatures and times specified in Table 1, the polymer adhesive layer was obtained. The polymer selected was quaternary ammonium salt-modified positively charged PVA (PVA-N). + The following solvents are used: chitosan, carbomer, and PAA. Glutaraldehyde (GA), borax, and aziridine crosslinking agents are selected. Furthermore, the content of alcohols and acids in the following solvents is by mass in the solvent.
[0110] Table 1
[0111] Example 1
[0112] Take 100 mL of the 2.5 mg / mL porous graphene oxide solution prepared in Preparation Example 1, and adjust its pH to 10.5 using sodium hydroxide. Then, add 5 mL of 1% (w / w) PEI-600 solution, followed by adding deionized water to dilute the porous graphene oxide concentration to 2 mg / mL. Stir at room temperature for 30 minutes to ensure uniform dispersion of the porous graphene oxide and PEI-600, obtaining a mixed solution. Subsequently, use a coating machine to uniformly coat the mixed solution onto the polymer adhesive layer to form a wet film with a thickness of 25 μm. Then, react at 90℃ for 15 minutes to form a porous graphene oxide separation layer (83 nm thick), obtaining a porous graphene oxide composite nanofiltration membrane.
[0113] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1190 Daltons.
[0114] Example 2
[0115] Take 100 mL of the 4 mg / mL porous graphene oxide solution prepared according to Preparation Example 1, and adjust its pH to 10.5 with ammonia. Then, add 20 mg of aziridine crosslinking agent (CX-100), followed by adding deionized water to dilute the porous graphene oxide concentration to 3 mg / mL. Stir at room temperature for 30 minutes to uniformly disperse the porous graphene oxide and aziridine crosslinking agent, obtaining a mixture. Then, use a coating machine to uniformly coat the mixture onto the polymer adhesive layer to form a wet film with a thickness of 15 μm. Then, react at 70°C for 15 minutes to form a porous graphene oxide separation layer (93 nm thick), obtaining a porous graphene oxide composite nanofiltration membrane.
[0116] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1060 Daltons.
[0117] Example 3
[0118] 100 mL of a 5 mg / mL porous graphene oxide solution prepared according to Preparation Example 1 was taken, and its pH was adjusted to 10.5 using ammonia. Then, 100 mL of a 1% (w / w) cellulose nanofiber solution and 25 mg of aziridine crosslinking agent (CX-100) were added. Subsequently, deionized water was added to dilute the porous graphene oxide concentration to 2 mg / mL. The mixture was stirred at room temperature for 30 minutes to uniformly disperse the porous graphene oxide, cellulose nanofibers, and aziridine crosslinking agent, resulting in a mixed solution. The mixed solution was then uniformly coated onto a polymer adhesive layer to form a wet film with a thickness of 20 μm using a coating machine. The film was then reacted at 70 °C for 15 minutes to form a porous graphene oxide separation layer (94 nm thick), thus obtaining a porous graphene oxide composite nanofiltration membrane.
[0119] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1050 Daltons.
[0120] Example 4
[0121] 100 mL of a 3 mg / mL porous graphene oxide solution prepared according to Preparation Example 1 was taken, and its pH was adjusted to 3.5 using hydrochloric acid. Then, 60 μL of a 50% glutaraldehyde solution (graphene oxide:glutaraldehyde = 10:1) was added. Subsequently, deionized water was added to dilute the porous graphene oxide concentration to 2 mg / mL. The mixture was stirred overnight at room temperature to allow the porous graphene oxide and glutaraldehyde to be evenly dispersed and pre-crosslinked, resulting in a mixed solution. The mixed solution was then uniformly coated onto a polymer adhesive layer to form a 25 μm thick wet film using a coating machine. The film was then reacted at 70°C for 15 minutes to form a porous graphene oxide separation layer (89 nm thick), thus obtaining a porous graphene oxide composite nanofiltration membrane.
[0122] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1080 Daltons.
[0123] Example 5
[0124] 100 mL of a 3 mg / mL porous graphene oxide solution prepared according to Preparation Example 1 was taken, and its pH was adjusted to 3.5 using acetic acid. Then, 100 mL of a 1% (w / w) cellulose nanofiber solution and 60 μL of a 50% (w / w) glutaraldehyde solution (graphene oxide:glutaraldehyde = 10:1) were added. Subsequently, deionized water was added to dilute the porous graphene oxide concentration to 2 mg / mL. The mixture was stirred overnight at room temperature to allow the porous graphene oxide, cellulose nanofibers, and glutaraldehyde to be evenly dispersed and pre-crosslinked, resulting in a mixed solution. The mixed solution was then uniformly coated onto a polymer adhesive layer to form a 25 μm thick wet film using a coating machine. The film was then reacted at 70°C for 15 minutes to form a porous graphene oxide separation layer (93 nm thick), thus obtaining a porous graphene oxide composite nanofiltration membrane.
[0125] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1000 Daltons.
[0126] Example 6
[0127] 100 mL of the 2.5 mg / mL porous graphene oxide solution prepared in Preparation Example 1 was taken, and 0.15 mL of a 20 mg / mL tannic acid (TA) aqueous solution and 0.15 mL of a 20 mg / mL 3-aminopropyltriethoxysilane (APTES) ethanol solution were added sequentially. Deionized water was then added to dilute the porous graphene oxide concentration to 2 mg / mL, and the pH was adjusted to 10 using triethylamine. The mixture was stirred at room temperature for 30 h to allow the porous graphene oxide, TA, and APTES to be uniformly dispersed and pre-crosslinked, resulting in a mixed solution. Subsequently, a coating machine was used to uniformly coat the mixed solution onto a polymer adhesive layer to form a wet film with a thickness of 25 μm. The film was then reacted at 70 °C for 15 minutes to form a porous graphene oxide separation layer (108 nm thick), thus obtaining a porous graphene oxide composite nanofiltration membrane.
[0128] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1050 Daltons.
[0129] Example 7
[0130] 100 mL of the 2.5 mg / mL porous graphene oxide solution prepared in Preparation Example 1 was taken, and its pH was adjusted to 10.5 using sodium hydroxide. Then, 5 mL of a 1% (3-glycidylpropoxy)trimethoxysilane (GLMYO) solution was added, followed by the addition of deionized water to dilute the porous graphene oxide concentration to 2 mg / mL. The mixture was stirred at room temperature for 30 minutes to ensure uniform dispersion of the porous graphene oxide and GLMYO, resulting in a mixed solution. The mixture was then uniformly coated onto a polymer adhesive layer using a coating machine to form a 25 μm thick wet film. The film was then reacted at 90 °C for 30 minutes to form a porous graphene oxide separation layer (98 nm thick), thus obtaining a porous graphene oxide composite nanofiltration membrane.
[0131] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1100 Daltons.
[0132] Example 8
[0133] Take 100 mL of a 4 mg / mL porous graphene oxide solution prepared according to Preparation Example 1, and 20 mg of isocyanate crosslinking agent (IPDI). Then, add deionized water to dilute the porous graphene oxide concentration to 2 mg / mL. Stir at room temperature for 30 minutes to uniformly disperse the porous graphene oxide and isocyanate crosslinking agent, obtaining a mixture. Then, use a coating machine to uniformly coat the mixture onto the polymer adhesive layer to form a wet film with a thickness of 20 μm. Then, react at 70°C for 15 minutes to form a porous graphene oxide separation layer (with a thickness of 89 nm), obtaining a porous graphene oxide composite nanofiltration membrane.
[0134] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1080 Daltons.
[0135] The surface electron microscope image of the porous graphene oxide composite nanofiltration membrane prepared in this embodiment is shown below. Figure 1 As shown. A cross-sectional electron microscope image of the porous graphene oxide composite nanofiltration membrane in this embodiment is shown below. Figure 2 As shown.
[0136] Example 9
[0137] The preparation method of the porous graphene oxide separation layer in this embodiment is basically the same as that in Example 8, except that the porous graphene oxide solution was prepared in Example 2, and the rest is the same as in Example 8.
[0138] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this embodiment has a thickness of 95 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this embodiment is 1250 Daltons.
[0139] Example 10
[0140] The preparation method of the porous graphene oxide separation layer in this embodiment is basically the same as that in Example 8, except that the porous graphene oxide solution was prepared in Example 3, and the rest are the same as in Example 8.
[0141] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this embodiment has a thickness of 86 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this embodiment is 1470 Daltons.
[0142] Example 11
[0143] The preparation method of the porous graphene oxide separation layer in this embodiment is basically the same as that in Example 8. The difference is that the porous graphene oxide solution was prepared in Example 4, and the rest is the same as in Example 8.
[0144] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this embodiment has a thickness of 79 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this embodiment is 1500 Daltons.
[0145] Example 12
[0146] The preparation method of the porous graphene oxide separation layer in this embodiment is basically the same as that in Example 8, except that the porous graphene oxide solution was prepared in Example 5, and the rest are the same as in Example 8.
[0147] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this embodiment has a thickness of 78 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this embodiment is 1580 Daltons.
[0148] Example 13
[0149] A PVA aqueous solution with a mass content of 0.5% was prepared in advance. A porous graphene oxide separation layer was prepared according to the method of Example 12. The PVA aqueous solution was coated on the surface of the porous graphene oxide separation layer, with a wet film thickness of 10 μm. Then, it was dried at 70°C for 5 min to form a PVA protective layer with a thickness of 15 nm.
[0150] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1300 Daltons.
[0151] Example 14
[0152] A PDDA aqueous solution with a mass content of 1% was prepared in advance. A porous graphene oxide separation layer was prepared according to the method of Example 12. The PDDA aqueous solution was coated on the surface of the porous graphene oxide separation layer, with a wet film thickness of 4 μm. Then, it was dried at 70°C for 5 min to form a PDDA protective layer with a thickness of 10 nm.
[0153] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1500 Daltons.
[0154] Example 15
[0155] A 1% sodium alginate (SA) aqueous solution was prepared in advance. A porous graphene oxide separation layer was prepared according to the method in Example 12. The SA aqueous solution was coated on the surface of the porous graphene oxide separation layer, with a wet film thickness of 4 μm. Then, it was immersed in a 500 ppm calcium chloride solution for 5 min to perform ionic crosslinking of sodium alginate. Finally, it was dried at 70°C for 5 min to form an SA protective layer with a thickness of 10 nm.
[0156] The porous graphene oxide composite nanofiltration membrane in this embodiment has a molecular weight cutoff of 1500 Daltons.
[0157] Comparative Example 1
[0158] This comparative example is basically the same as Example 8, except that the porous graphene oxide solution was prepared in Comparative Preparation Example 1, and the rest is the same as Example 8.
[0159] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this comparative example has a thickness of 115 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this comparative example is 1000 Daltons.
[0160] Comparative Example 2
[0161] This comparative example is basically the same as Example 8, except that the porous graphene oxide solution was prepared in Comparative Preparation Example 2, and the rest is the same as Example 8.
[0162] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this comparative example has a thickness of 105 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this comparative example is 1000 Daltons.
[0163] Comparative Example 3
[0164] This comparative example is basically the same as Example 8, except that the porous graphene oxide solution was prepared in Comparative Preparation Example 3, and the rest is the same as Example 8.
[0165] The porous graphene oxide separation layer in the porous graphene oxide composite nanofiltration membrane of this comparative example has a thickness of 107 nm, and the molecular weight cutoff of the porous graphene oxide composite nanofiltration membrane of this comparative example is 1000 Daltons.
[0166] Comparative Example 4
[0167] This comparative example is basically the same as Example 8, except that a graphene oxide solution (in which the GO is the same as in Preparation Example 1) is used instead of a porous graphene oxide solution. All other aspects are the same as in Example 8.
[0168] The graphene oxide membrane in this comparative example has a thickness of 170 nm and a molecular weight cutoff of 900 Daltons.
[0169] Test Example 1
[0170] (1) Flux test: The composite nanofiltration membrane is loaded into a dead-end filter or a cross-flow filter. At 25°C and 4 Bar pressure, a mixed solution of 70 g / L Na2SO4 and 2 g / L reactive dye (such as BlueR) is used as the feed liquid. After pre-pressurization for 30 minutes, the permeate is collected, and the flux is calculated according to the following formula: J = V / (A×t×P), where J is the flux (L / (m 2 ·h·Bar), V is the permeate volume (L), A is the effective membrane area (m²), t is the test time (h), and P is the operating pressure (Bar).
[0171] (2) Dye Retention Rate Test: The absorbance of the dye in the feed solution and the permeate was measured using a UV-Vis spectrophotometer (at the maximum absorption wavelength of the dye). The dye retention rate was calculated using the following formula: R = (1 - Cp / Cf) × 100%, where R is the retention rate (%), Cp is the dye concentration in the permeate, and Cf is the dye concentration in the feed solution.
[0172] (3) Desalination rate test: The conductivity of the feed liquid and the permeate is measured by a conductivity meter, and the desalination rate is calculated according to the following formula: Rs = (1 - κp / κf) × 100%, where Rs is the desalination rate (%), κp is the conductivity of the permeate, and κf is the conductivity of the feed liquid.
[0173] Porous graphene oxide was prepared according to the method of Preparation Example 1, but the reaction temperature and time were adjusted. Then, a porous graphene oxide composite nanofiltration membrane was prepared according to the method of Example 1. The flux and dye rejection rate of the composite nanofiltration membranes formed by the porous graphene oxide prepared under different etching temperatures and times are shown in Table 2.
[0174] Table 2
[0175] Table 2 shows that with increasing etching temperature and etching time, the flux of the composite nanofiltration membrane gradually increases, while the dye rejection initially increases slightly and then gradually decreases. This indicates that hydrogen peroxide can etch nanopores into the graphene oxide surface, significantly improving the flux of the GO membrane. However, excessive etching leads to a significant decrease in dye rejection. Specifically, the etching reaction rate is slow at 25℃, resulting in limited flux improvement (5-8 L / (m²)). 2 While the dye rejection rate remained above 94%, the flux increased significantly over time at 45°C (5-15 L / (m²)). 2 The dye rejection rate remained above 92% within the 6-20 h range, achieving a good balance between flux and rejection rate; at 60℃, the flux increased significantly (reaching a maximum of 22.67 L / (m²)). 2 While the etching rate is relatively fast (·h·Bar), the dye retention rate drops sharply after 6 hours (90.67% at 12 hours and only 45.89% at 30 hours). Considering both throughput and dye retention rate, the preferred etching temperature is 45-60℃ and the etching time is 6-20 hours; a more preferred etching temperature is 45℃ and the etching time is 6-20 hours.
[0176] Porous graphene oxide composite nanofiltration membranes were prepared according to the method in Example 8, but the content of isocyanate crosslinking agent and the porous graphene oxide solution (porous graphene oxide prepared by different methods) were adjusted to obtain different composite nanofiltration membranes. Their flux and dye rejection rates are shown in Table 3.
[0177] Table 3
[0178] As shown in Table 3, GO membranes with added nanofibers exhibit better performance than simply cross-linked GO membranes. Furthermore, the performance of cross-linked porous GO membranes, regardless of whether nanofibers are added or not, is significantly higher than that of uncross-linked GO membranes, with fluxes 2-6 times higher while maintaining comparable dye rejection rates. Moreover, for uncross-linked GO membranes, flux is very low at higher cross-linking agent concentrations. However, for cross-linked GO membranes, high fluxes are still achieved even with cross-linking agent concentrations of 0.3 mg / mL and 1 mg / mL, indicating that the degree of cross-linking in GO membranes can be increased, resulting in better membrane adhesion. For example, the flux in D with a cross-linking agent concentration of 0.3 mg / mL (D0.3) is twice that in B with 0.1 mg / mL (B0.1), while the dye rejection rates remain essentially the same. Furthermore, because the cross-linking agent content in D (0.3 mg / mL) is higher than that in B (0.1 mg / mL), the degree of cross-linking in the D membrane is higher, resulting in better adhesion. Figure 3The images show the B0.1 and D0.3 membranes after testing. The left image shows the B0.1 membrane after testing, where it can be seen that although the GO membrane remains largely intact, slight damage is visible in the rectangular area. The right image shows the D0.3 membrane after testing, where it can be seen that the D0.3 membrane has no visible damage.
[0179] The throughput, dye rejection rate, and desalination rate of the above embodiments and comparative examples are shown in Table 4.
[0180] Table 4
[0181] As shown in Table 4, the composite nanofiltration membranes formed from porous graphene oxide prepared in Examples 2-5 using additives exhibit superior flux and separation performance compared to the composite nanofiltration membrane formed from porous graphene oxide prepared in Example 1 without additives. In particular, Example 5, which used a tertiary amine as an additive, demonstrated even better results.
[0182] Test Example 2
[0183] A polymer adhesive layer combining PVA and PAA was coated on both sides of the nylon base film, followed by the coating of a porous GO membrane. The resulting composite membrane is shown in the images below, as well as images of the membrane after it has been peeled off with adhesive tape. Figure 4 As shown. Figure 4 The left image shows the actual composite membrane. The light-colored areas on both sides are coated with PVA / PAA polymer adhesive layers, while the dark-colored area in the middle has no polymer adhesive layer. Figure 4 The right image shows the actual product after the film has been peeled off with tape, with the rectangular frame indicating the area where the tape was removed. Clearly, the porous GO membrane, which does not contain a polymer adhesive layer and is in direct contact with the base membrane, will be peeled off with the tape, while the porous GO membrane formed on the polymer adhesive layer remains intact. This demonstrates that the polymer adhesive layer of this invention can effectively improve the bonding force between the base membrane and the porous GO membrane.
[0184] Nylon-based membrane / porous GO membrane, nylon-based membrane / crosslinked porous GO membrane, nylon-based membrane / PVA-N + The actual image after peeling off the polymer adhesive layer / crosslinked porous GO membrane is shown below. Figure 5 As shown. In Figure 5 The membranes in the middle, upper, middle, and lower sections correspond to nylon-based membrane / porous GO membrane, nylon-based membrane / crosslinked porous GO membrane, and nylon-based membrane / PVA-N membrane, respectively. + Polymer adhesive layer / crosslinked porous GO membrane. Figure 5 The left image shows the dry adhesion, indicating that PVA-N is coated. + After the polymer adhesive layer is applied, the dry bonding strength is significantly improved, and the porous GO membrane cannot be removed with tape. Figure 5The right-hand image shows the wet bonding strength, indicating that the wet bonding strength of the cross-linked porous GO membrane is enhanced. External force can only slightly damage the porous GO membrane. (Nylon-based membrane / PVA-N) + The polymer adhesive layer / crosslinked porous GO membrane exhibits the best wet bonding strength, and the porous GO membrane remains intact after being damaged by external force.
[0185] Example 16
[0186] The semi-finished dye solution after dye synthesis contains a large amount of reactive dyes, byproducts, unreacted intermediates, and salts, typically at concentrations exceeding 100 g / L. Impurities such as byproducts, intermediates, and salts may account for 20-50% of the total solid content.
[0187] This embodiment provides a desalting and purification system for salt-containing dyes, such as... Figure 6 As shown, it includes: a water tank 1, a dye solution tank 2, a first membrane element 3, and a permeate tank 4; The dye solution tank 2 is connected to the inlet of the first membrane element 3 via the feed line 7. The permeate outlet of the first membrane element 3 is connected to the permeate tank 4 via the first permeate line 8. The concentrate outlet of the first membrane element 3 is connected to the dye solution tank 2 via the concentrate line 9. The clean water tank 1 is connected to the inlet of the first membrane element 3 via the clean water flushing pipeline 10, and is used to flush the first membrane element 3; The first membrane element 3 includes the porous graphene oxide composite nanofiltration membrane with an adhesive layer of the present invention.
[0188] The desalination and purification system may further include: a second membrane element 5 and a secondary permeate tank 6; the permeate tank 4 is connected to the inlet of the second membrane element 5 through a secondary feed line 11, the permeate outlet of the second membrane element 5 is connected to the secondary permeate tank 6 through a second permeate line 12, and the concentrate outlet of the second membrane element 5 is connected to the permeate tank 4 through a secondary concentrate line 13; the second membrane element 5 includes the porous graphene oxide composite nanofiltration membrane with an adhesive layer of the present invention.
[0189] The dye solution tank 2 is equipped with an upper liquid level indicator and a lower liquid level indicator to monitor the liquid level inside the tank.
[0190] The dye solution tank 2 is also equipped with a stirring device to ensure that the solution in the tank is mixed evenly.
[0191] A liquid level indicator is installed in the permeate tank 4.
[0192] A first inlet valve 14 is installed on the feed line 7, a first product water valve 15 is installed on the first permeate line 8, and a first concentrate valve 17 is installed on the concentrate line 9.
[0193] A cleaning valve 16 is installed on the clean water flushing pipeline 10.
[0194] A first booster pump 18 is installed at the inlet of the first membrane element 3.
[0195] A second booster pump 19 is installed at the inlet of the second membrane element 5.
[0196] A second inlet valve 20 is installed on the secondary feed line 11, a second product water valve 21 is installed on the second permeate line 12, and a second concentrate valve 22 is installed on the secondary concentrate line 13.
[0197] This embodiment also provides a method for desalting and purifying salt-containing dyes, using the above-described system, which includes the following steps: Step 1: Concentrate the dye solution The semi-finished dye solution is pre-filled into dye solution tank 2. When the level of the dye solution reaches the upper level indicator in dye solution tank 2, the filling of dye solution is stopped, and the tank enters standby mode, ready to concentrate and desalinate the dye solution at any time.
[0198] After startup, open the first inlet valve 14 and the first product water valve 15, close the cleaning valve 16, start the first booster pump 18, partially open the first concentrate valve 17 and adjust the inlet pressure to the preset pressure. The dye solution is pumped into the first membrane element 3 by the first booster pump 18, and separated using a porous graphene oxide composite nanofiltration membrane. Because the composite nanofiltration membrane can efficiently retain dye and almost completely remove salt, the permeate contains only a small amount of dye (less than 3% of the original concentration) and salt, which is stored in the permeate tank 4; the concentrate is returned to the dye solution tank 2, and the dye solution is continuously concentrated.
[0199] Due to the osmotic pressure difference across the membrane—the feed end contains a large amount of dye and salt, while the product end contains only a small amount—a significant amount of salt from the feed end permeates through the membrane to the product end to maintain osmotic balance. Therefore, the salt content at the product end is even higher than at the feed end, meaning the salt rejection rate is negative. As the dye solution is concentrated, the salt content of the concentrate decreases. This effect gradually disappears when the salt content in the dye solution is low in the later stages, and the membrane begins to retain some salt. The salt content at the product end is lower than at the feed end, meaning that the later the stage, the more difficult it is to desalinate the dye.
[0200] As the permeate is continuously produced, the liquid level in dye solution tank 2 gradually decreases. When the liquid level drops to the lower liquid level indicator in dye solution tank 2, concentration is stopped, and the process proceeds to the water dilution and membrane rinsing steps.
[0201] Step 2: Diluting with water and rinsing the membrane
[0202] Close the first inlet valve 14 and the first product water valve 15, open the cleaning valve 16, and fully open the first concentrate valve 17. Clean water is flushed onto the membrane surface of the first membrane element 3 by the first booster pump 18 and discharged from the first concentrate valve 17 into the dye solution tank 2. When the solution level in the dye solution tank 2 reaches the upper level indicator, membrane flushing is stopped.
[0203] This process cleans the membrane and restores its flux; on the other hand, it dilutes the concentrated solution again with water, resulting in a dye concentration close to the initial concentration, but a significant decrease in salt content.
[0204] Step 3: Repeat steps 1 and 2 multiple times.
[0205] Repeat steps one (solution concentration) and two (dilution with water and membrane rinsing) multiple times (usually requiring 4-6 rounds), gradually reducing the salt content in the dye solution. Once the conductivity of the solution in dye solution tank 2 reaches the preset level, perform a final round of solution concentration. The concentrated dye concentrate (i.e., the solution in dye solution tank 2) can then be spray-dried to prepare low-salt dye powder.
[0206] Step 4: Selectively, the permeate is concentrated a second time.
[0207] Because a small amount of dye permeates through the membrane, some dye is lost into the permeate tank 4, so the permeate cannot be discharged directly. The permeate in the permeate tank 4 can be concentrated a second time: the second inlet valve 20 and the second product water valve 21 are opened, and the second concentrate valve 22 is partially opened. The permeate is pumped into the second membrane element 5 through the secondary feed line 11 and the second booster pump 19. The secondary permeate (containing salt, unreacted intermediates, and a very small amount of dye) enters the secondary permeate tank 6, and is discharged after being treated to reduce COD. The solution after secondary concentration (i.e., the solution in the permeate tank 4) can be returned to the dye solution tank 2 for further desalination, or directly spray-dried to prepare salt-containing dye powder.
[0208] This embodiment provides the application of a first membrane element 3 and a second membrane element 5 containing the composite nanofiltration membrane of Example 12 in the desalination and purification of salt-containing dyes. It is understood that the membrane elements are formed by rolling up the composite nanofiltration membrane.
[0209] The dye solution used in this embodiment has the following characteristics: dye content 130 g / L, salt content 32% (based on the mass of the dye solution being 100%), and conductivity 27.6 mS / cm (contributed by both salt and dye).
[0210] A total of 10 L of dye solution underwent six rounds of concentration-dilution-rinsing processes. In the first five rounds, approximately 4 L of permeate (referring to the permeate in permeate tank 4) was produced per round, with 4 L of clean water added. The sixth round was the final concentration, producing 5 L of permeate. The solution was then concentrated to 5 L and dried. The conductivity changes at each stage are shown in Table 5 below.
[0211] Table 5
[0212] As can be seen from Table 5, during the first round of concentration, the permeate conductivity (29 mS / cm) was higher than that of the dye solution (26.56 mS / cm), meaning the salt rejection rate was negative, which verified the effect of osmotic pressure difference driving salt permeation through the membrane. As desalination proceeded, this effect gradually disappeared, and from the second round onwards, the permeate conductivity began to be lower than that of the dye solution.
[0213] The initial 10 L dye solution was concentrated to 5 L after six rounds of concentration-dilution, with a conductivity of 3.84 mS / cm (mainly contributed by the dye) and a salt content of 2.53%. After concentration and desalination, the low-salt dye accounted for 58.2% of the original solid content, and the salt content decreased from the initial 32% to 2.53% (by weight). The actual dye loss was only 2.7% (calculated by absorbance), with the remaining approximately 15% of the solid content loss consisting of unreacted intermediates and other byproducts. The desalted low-salt dye can meet the requirements of digital printing and dyeing on non-aqueous media.
[0214] In addition, such as Figure 7 The images shown are actual photos of a salt-containing dye (salt content 32%), a dye solution after three rounds of concentration-dilution (salt content 4.78%), and a low-salt dye solution after six rounds of concentration-dilution (salt content 2.53%).
[0215] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A porous graphene oxide composite nanofiltration membrane with an adhesive layer, comprising a base membrane, a polymer adhesive layer, and a porous graphene oxide separation layer stacked sequentially; the porous graphene oxide separation layer contains porous graphene oxide, and the porous graphene oxide separation layer is formed on the surface of the polymer adhesive layer by crosslinking through a first crosslinking agent; the porous graphene oxide is obtained by creating pores in the graphene oxide using a pore-forming agent, the pore-forming agent comprising a main pore-forming agent and selectively comprising an auxiliary agent, wherein the main pore-forming agent is hydrogen peroxide.
2. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, In the pore-forming agent, the auxiliary agent includes one or more of a strong oxidizing agent, an inorganic base, an organic base, and a ferrous salt; Preferably, the strong oxidant includes one or more of sodium hypochlorite, ozone, and potassium permanganate; Preferably, the inorganic base includes NaOH and / or ammonia. Preferably, the organic base includes C6-C12 tertiary amine compounds; More preferably, the organic base includes one or more of triethylamine, tripropylamine and tributylamine; Preferably, the ferrous salt comprises ferrous sulfate and / or ferrous chloride.
3. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, In the process of preparing porous graphene oxide by creating pores in graphene oxide with a pore-forming agent, the mass ratio of hydrogen peroxide to graphene oxide is (1-100):
1. And / or, the sheet size of the graphene oxide is 0.5-100 μm.
4. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The pore-forming agent is hydrogen peroxide, or a combination of sodium hypochlorite and hydrogen peroxide, or a combination of hydrogen peroxide and ferrous salt, or a combination of hydrogen peroxide and ammonia, or a combination of hydrogen peroxide and organic base.
5. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 4, wherein, When the pore-forming agent is hydrogen peroxide, the porous graphene oxide is prepared by forming pores in graphene oxide using the pore-forming agent. This includes reacting a mixed solution of graphene oxide and hydrogen peroxide at 45-60°C for 6-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, thereby obtaining the porous graphene oxide. And / or, when the pore-forming agent is a combination of sodium hypochlorite and hydrogen peroxide, the porous graphene oxide is prepared by forming pores in the graphene oxide using the pore-forming agent, comprising: first reacting a mixed solution of graphene oxide and sodium hypochlorite at 5-25°C for 12-30 hours, wherein the mass ratio of sodium hypochlorite to graphene oxide is 1:100-1:10, to obtain pretreated graphene oxide; then reacting a mixed solution of the pretreated graphene oxide and hydrogen peroxide at 45-60°C for 12-48 hours, wherein the mass ratio of hydrogen peroxide to the pretreated graphene oxide is (1-100):1, to obtain the porous graphene oxide. And / or, when the pore-forming agent is a combination of hydrogen peroxide and ferrous salt, the porous graphene oxide is prepared by forming pores in graphene oxide using the pore-forming agent, which includes: reacting a mixed solution of graphene oxide, hydrogen peroxide and ferrous salt at 25-45°C for 12-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the mass ratio of ferrous salt to graphene oxide is 1:100-1:10, thereby obtaining the porous graphene oxide. And / or, when the pore-forming agent is a combination of hydrogen peroxide and ammonia, the porous graphene oxide is prepared by forming pores in the graphene oxide using the pore-forming agent, comprising: reacting a mixed solution of graphene oxide, hydrogen peroxide, and ammonia at 25-45°C for 12-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the ammonia is used to adjust the pH of the mixed solution of graphene oxide, hydrogen peroxide, and ammonia to 9-12.5, thereby obtaining the porous graphene oxide; And / or, when the pore-forming agent is a combination of hydrogen peroxide and an organic base, the porous graphene oxide is prepared by forming pores in the graphene oxide using the pore-forming agent, which includes: reacting a mixed solution of graphene oxide, hydrogen peroxide, and an organic base at 25-60°C for 2-48 hours, wherein the mass ratio of hydrogen peroxide to graphene oxide is (1-100):1, and the mass ratio of the organic base to hydrogen peroxide is 1:2-1:20, thereby obtaining the porous graphene oxide.
6. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The porous graphene oxide has a bimodal pore size distribution, including micropores and macropores. The average pore size of the micropores is 0.5-2 nm, and the average pore size of the macropores is 2-50 nm. In terms of the number of pores, the micropores account for more than 75% of the total number of pores.
7. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The first crosslinking agent includes an ionic crosslinking agent and / or a first chemical crosslinking agent; Preferably, the ionic crosslinking agent includes Ca. 2+ Mg 2+ and Fe 3+ One or more of the following; Preferably, the first chemical crosslinking agent includes one or more of carboxyl crosslinking agents, hydroxyl crosslinking agents, and multifunctional crosslinking agents; More preferably, the carboxyl crosslinking agent includes one or more of polyamines, polyfunctional aziridines, and polycarbodiimides; the hydroxyl crosslinking agent includes one or more of polyaldehydes, isocyanates, and borax; and the polyfunctional crosslinking agent includes polyphenols and / or siloxanes.
8. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The first crosslinking agent accounts for 1-50% of the mass of the porous graphene oxide.
9. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The porous graphene oxide separation layer further contains polymer nanomaterials; Preferably, the polymer nanomaterial includes one or more of cellulose nanofibers, cellulose nanocrystals, chitin nanofibers, chitin nanocrystals, chitosan nanofibers, chitosan nanocrystals, lignin nanofibers, and lignin nanocrystals. Preferably, the mass ratio of the polymer nanomaterial to the porous graphene oxide is (0.5-5):
1.
10. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The thickness of the porous graphene oxide separation layer is 10-500 nm.
11. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The polymer adhesive layer is formed by applying a solution containing polymers or monomers that can polymerize to the base film and then curing it.
12. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 11, wherein, The polymer includes one or more of the following: polyvinyl alcohol, polyacrylic acid, chitosan, carbomer, guar gum, polyethyleneimine, polydiallyldimethylammonium chloride, positively charged polyvinyl alcohol, positively charged polyacrylic acid, positively charged chitosan, positively charged carbomer, and positively charged guar gum. And / or, the monomers that can polymerize to form a polymer include dopamine, or a mixture of soybean oil, malic acid and tannic acid; And / or, the mass content of the polymer or the total mass content of the monomer in the solution containing the polymer or monomers that can polymerize to form a polymer is 0.1-5%; And / or, the solution containing a polymer or a monomer that can polymerize to form a polymer further contains a second crosslinking agent, the second crosslinking agent including a second chemical crosslinking agent; And / or, the solvent in the solution containing a polymer or a monomer that can polymerize to form a polymer is water or a mixture of water and an organic solvent, wherein the organic solvent is an alcohol solvent.
13. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 12, wherein, The second chemical crosslinking agent includes one or more of carboxyl crosslinking agents, hydroxyl crosslinking agents, and amino crosslinking agents; And / or, the second chemical crosslinking agent includes one or more of polyaldehydes, borax, and polyfunctional aziridines; And / or, the second crosslinking agent accounts for 1-30% of the mass of the polymer or the monomer that can polymerize to form the polymer.
14. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The thickness of the polymer adhesive layer is 1-1000 nm.
15. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The porous graphene oxide composite nanofiltration membrane with an adhesive layer further includes a polymer protective layer located on the side of the porous graphene oxide separation layer away from the polymer adhesive layer. Preferably, the polymer protective layer is made of one or more of the following: neutral polyvinyl alcohol, polyethylene oxide, negatively charged sodium polyacrylate, sodium alginate, carboxyl-modified polyvinyl alcohol, positively charged polyethyleneimine, polydiallyldimethylammonium chloride, chitosan, and quaternary ammonium salt-modified positively charged polyvinyl alcohol. Preferably, the thickness of the polymer protective layer is 10-300 nm.
16. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The base membrane is an ultrafiltration membrane or a microfiltration membrane; And / or, the average pore size of the base film is 0.01-5 μm; And / or, the base film is made of one or more of nylon, polyethersulfone, polyvinylidene fluoride, polytetrafluoroethylene, cellulose acetate and polypropylene. And / or, the thickness of the base film is 50-200 μm.
17. The porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 1, wherein, The porous graphene oxide composite nanofiltration membrane with an adhesive layer has a molecular weight cutoff of 1000-5000 Daltons, a rejection rate of ≥95% for reactive dyes, and a rejection rate of <12% for inorganic salts.
18. A method for preparing a porous graphene oxide composite nanofiltration membrane with an adhesive layer according to any one of claims 1-17, comprising the following steps: (1) A solution containing a polymer or a monomer that can be polymerized to form a polymer is applied to the base film, and after curing, a polymer adhesive layer is formed; (2) A mixture containing porous graphene oxide and a crosslinking agent is coated onto the surface of the polymer adhesive layer and crosslinking reaction is carried out to form a porous graphene oxide separation layer, thereby obtaining the porous graphene oxide composite nanofiltration membrane with the adhesive layer.
19. The method for preparing a porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 18, wherein, In step (1), the method of applying the solution containing polymers or monomers that can polymerize to form polymers to the base film includes one or more of the following: spraying, blade coating, wire rod coating, slot coating, gravure coating, and immersion. And / or, in step (1), the solution containing a polymer or a monomer that can polymerize to form a polymer is applied to the base film to form a polymer adhesive layer wet film, the thickness of the polymer adhesive layer wet film being 1-10 μm; And / or, in step (1), the curing temperature is 20-100°C and the time is 1 minute to 48 hours.
20. The method for preparing a porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 18, wherein, In step (2), the mixture containing porous graphene oxide and crosslinking agent further contains polymer nanomaterials; And / or, in step (2), the content of porous graphene oxide in the mixture containing porous graphene oxide and crosslinking agent is 1-10 mg / mL; And / or, in step (2), the method of applying the mixture containing porous graphene oxide and crosslinking agent to the surface of the polymer adhesive layer includes one or more of blade coating, wire bar coating, slot coating and microgravure coating; And / or, in step (2), a mixture containing porous graphene oxide and a crosslinking agent is coated onto the surface of the polymer adhesive layer to form a porous graphene oxide separation layer wet film, the thickness of which is 5-100 μm; And / or, in step (2), the crosslinking reaction is carried out at a temperature of 20-100°C for a time of 5 minutes to 48 hours.
21. The method for preparing a porous graphene oxide composite nanofiltration membrane with an adhesive layer according to claim 18, wherein, The preparation method further includes step (3): coating a polymer-containing solution onto the surface of the porous graphene oxide separation layer, and drying it to form a polymer protective layer.
22. The application of the porous graphene oxide composite nanofiltration membrane with an adhesive layer according to any one of claims 1-17 in the treatment of high-salt wastewater containing dyes and / or the desalination and purification of salt-containing dyes.
23. The application according to claim 22, wherein, The salt concentration in the high-salt wastewater containing dye is above 20 g / L, and the dye concentration is 0.1-5 g / L; And / or, the flux of the porous graphene oxide composite nanofiltration membrane with adhesive layer for treating the dye-containing high-salt wastewater is 4-20 L / (m³). 2 (·h·Bar), dye retention rate is 95%-99.9%, desalination rate is <12%; And / or, the salt-containing dye contains dye, by-products, unreacted intermediates and salt, the total concentration of the dye, by-products, unreacted intermediates and salt is above 100 g / L, and the by-products, unreacted intermediates and salt account for 20-50% of the total solid content of the salt-containing dye.
Citation Information
Patent Citations
Graphene oxide composite nanofiltration membrane and preparation method thereof
CN110523297A
Graphene oxide composite nanofiltration membrane as well as preparation method and application thereof
CN116020286A