Aerogel powder and its supercritical drying preparation method, support device and drying equipment

By employing a staged processing technique involving cold pressurization and slow preheating, combined with a dedicated support device and drying equipment, the problem of skeleton damage during supercritical drying of powder aerogels was solved, achieving stable preparation and high-performance protection of aerogel powders.

CN123102252APending Publication Date: 2026-11-17GONG YI VAN RES INNOVATION COMPOSITE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611544463.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the supercritical drying process, the skeleton of powder aerogel is susceptible to thermal shock and thermal stress damage, and existing equipment is difficult to meet the preparation requirements of powder materials.

Method used

A staged processing technology combining cold pressurization and displacement with slow preheating is adopted. Supercritical liquid CO2 is used to replace organic solvents under normal or low pressure. The integrity of the gel skeleton is protected by slow heating and pressurization. Combined with a dedicated carrier device and drying equipment, the uniform distribution of CO2 fluid and temperature stability are ensured.

Benefits of technology

It effectively protects the integrity of the aerogel powder's skeletal structure, avoids damage from thermal shock and capillary forces, and ensures the stability of the drying process and the material's properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102252A_ABST
    Figure CN123102252A_ABST
Patent Text Reader

Abstract

This application relates to the field of aerogel composite materials technology, and particularly to an aerogel powder and its supercritical drying preparation method, supporting device, and drying equipment, comprising the following steps: placing a wet gel in a dry sealed environment; continuously introducing liquid CO2 at a supercritical pressure P1 into the dry sealed environment until the wet gel is completely immersed in the liquid CO2; wherein, before introducing the liquid CO2, the dry sealed environment is at or below atmospheric pressure; introducing CO2 at a supercritical temperature T1 and a supercritical pressure P1 into the dry sealed environment until both temperature T2 and pressure P2 in the dry sealed environment reach a supercritical state; and then circulating and drying the dry sealed environment to obtain the aerogel powder. This application employs a staged processing technology of first cold-state pressurization and displacement followed by slow switching and preheating, which protects the structural integrity of the gel skeleton.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of aerogel composite materials technology, and in particular to an aerogel powder and its supercritical drying preparation method, support device and drying equipment. Background Technology

[0002] Aerogels are a class of high-performance materials with nanoporous network structures. A key step in their preparation is removing the solvent from the wet gel while maintaining the integrity of the framework structure. Supercritical drying technology is a crucial process for achieving this. In existing technologies, supercritical drying is typically carried out by controlling temperature and pressure in stages. For example, a liquid drying medium is used for cold cycling to displace the organic solvent in the wet gel, followed by heating to a supercritical state for thermal cycling drying.

[0003] While the above method reduces thermal stress to some extent, it still has the following drawbacks: the pressure of the liquid drying medium used in the cold cycling stage is only slightly higher than the liquefaction pressure (exceeding it by 0.5~1.0 MPa), the wet gel is not under sufficient high-pressure protection, and a gas-liquid interface may still form during solvent evaporation, thus damaging the framework; when switching from cold cycling to hot cycling, the synchronous fluctuations in temperature and pressure will still cause thermal shock to the material; in addition, this method is mainly for bulk aerogels and does not involve powder aerogel materials. Because powder aerogels have a larger specific surface area, a more fragile framework, and a shorter thermal conduction path, their sensitivity to thermal shock is much higher than that of bulk materials. Therefore, more stringent requirements are placed on the drying process and support device, and existing drying processes and support devices are difficult to meet the above preparation requirements. Summary of the Invention

[0004] In view of this, this application provides an aerogel powder and a supercritical drying preparation method thereon, a support device and a drying equipment, which can solve at least one of the above-mentioned technical problems.

[0005] In a first aspect, this application provides a method for preparing aerogel powder by supercritical drying, comprising the following steps: placing a wet gel in a dry sealed environment, continuously introducing liquid CO2 at a supercritical pressure P1 into the dry sealed environment until the wet gel is completely immersed in the liquid CO2; wherein, before introducing the liquid CO2, the dry sealed environment is at or below atmospheric pressure; introducing CO2 at a supercritical temperature T1 and a supercritical pressure P1 into the dry sealed environment until both temperature T2 and pressure P2 in the dry sealed environment reach a supercritical state, and then circulating and drying the dry sealed environment to obtain the aerogel powder.

[0006] Compared to existing technologies, the supercritical drying method for preparing aerogel powder provided in this application employs a staged processing technology combining cold pressurization and displacement with slow preheating. First, supercritical liquid CO2 is introduced into a dry, enclosed environment at atmospheric or below atmospheric pressure. Initially, the liquid CO2 vaporizes due to pressure changes. This vaporized, low-temperature CO2 increases the pressure within the dry, enclosed environment while simultaneously addressing the issue of high-temperature CO2 impacting the gel skeleton, thus protecting the structural integrity of the gel skeleton. As the pressure within the dry, enclosed environment continues to increase, the vaporized CO2 reverts to liquid CO2. 2. The wet gel is completely immersed in liquid CO2 to displace the air and residual organic solvent in the pores of the wet gel. Then, with the introduction of CO2 at supercritical temperature and supercritical pressure, the dry and sealed environment is slowly heated and pressurized. This avoids thermal shock to the gel skeleton caused by pressure fluctuations and rapid temperature rise in the dry and sealed environment. Moreover, the liquid CO2 in the dry and sealed environment is directly transformed into a supercritical fluid through in-situ heating at supercritical temperature. There is no vaporization phase change in this stage, which avoids the generation of gas-liquid interface during the phase change process and fundamentally protects the structural integrity of the gel skeleton.

[0007] In some embodiments, P1 is 10 MPa-15 MPa. Liquid CO2 has a supercritical pressure within this range and good miscibility with organic solvents, allowing the organic solvents to be displaced without damaging the gel skeleton.

[0008] In some embodiments, after CO2 at a supercritical temperature T1 and a supercritical pressure P1 is introduced into the dry and sealed environment, the heating rate within the dry and sealed environment is 0.5℃ / min to 1℃ / min. This heating rate within the dry and sealed environment, within the above range, avoids thermal shock to the gel skeleton caused by rapid heating, thus protecting the structural integrity of the gel skeleton.

[0009] In some embodiments, T1 > 31.1°C. When the supercritical temperature T1 of the introduced CO2 is within the above range, the heating process in the dry and sealed environment can be slowly and precisely controlled, so that the liquid CO2 in the dry and sealed environment can be directly transformed into a supercritical fluid through in-situ heating of CO2 at the supercritical temperature. There is no vaporization phase change throughout the process, avoiding the generation of gas-liquid interface during the phase change process, eliminating capillary force damage, and fundamentally protecting the structural integrity of the gel skeleton.

[0010] In some embodiments, after the temperature and pressure in the drying and sealed environment both reach the supercritical state, T2 > 31.1℃ and P2 > 7.4 MPa. The temperature and pressure within the drying and sealed environment are within the above ranges, ensuring stable operation of the cyclic drying process within a stable supercritical window, avoiding the generation of a gas-liquid interface during the phase transition process, and protecting the structural integrity of the gel skeleton during the cyclic drying process.

[0011] In some embodiments, the purity of the liquid CO2 is ≥99%. The purity of the liquid CO2 used to displace air and residual organic solutions is within the above range, ensuring that the entire cold pressurization and displacement process falls within the homogeneous supercritical fluid range with zero surface tension. This allows for continuous extraction and displacement of the organic solvent without secondary wetting, thereby completely preserving the gel skeleton.

[0012] Secondly, this application provides an aerogel powder, which is prepared by the supercritical drying preparation method of the aerogel powder described in any one of the first aspects.

[0013] Thirdly, this application provides a support device for implementing the supercritical drying preparation method of aerogel powder according to any one of the first aspects, comprising a frame, a breathable hood covering the frame, a plurality of stacked trays placed inside the frame, and an airflow distribution plate arranged at the bottom of the trays; the breathable hood is provided with breathable holes, and the pore size of the breathable holes is smaller than the particle size of the aerogel powder; the bottom wall and side wall of the tray are provided with through holes, and the pore size of the through holes is smaller than the particle size of the aerogel powder; the airflow distribution plate is configured to uniformly distribute the introduced CO2.

[0014] Compared to existing technologies, the carrier device provided in this application has a breathable hood that can buffer the impact of CO2 fluid and prevent the gel skeleton from being damaged during process switching of wet gel. At the same time, the design of the airflow distribution plate and tray can ensure the uniformity of the flow rate and temperature of CO2 fluid in the dry and closed environment, avoid the thermal shock caused by pressure fluctuations and rapid temperature rise in the dry and closed environment, and further protect the structural integrity of the gel skeleton.

[0015] In some embodiments, the supporting device further includes a fiber mesh laid on the bottom wall of the tray, wherein the mesh aperture is 1 / 3 to 1 / 2 of the minimum particle size of the aerogel powder. The relationship between the mesh aperture and the particle size of the aerogel powder is within the aforementioned range, allowing the fiber mesh to physically intercept the aerogel powder while allowing organic solvents to pass through, thus preventing the gel skeleton from collapsing due to defects.

[0016] Fourthly, this application provides a drying device, which includes a drying kettle, a liquid CO2 source, a booster pump, a preheater, a bypass pipeline, a control unit, and a carrying device as described in any one of the third aspects; wherein, the preheater is connected to the booster pump and the drying kettle, the inlet end of the preheater is provided with an inlet valve, the bypass pipeline bypasses the preheater and connects the booster pump and the drying kettle, the bypass pipeline is provided with a bypass valve, and the control unit is configured to control the opening and closing of the inlet valve and the bypass valve. Attached Figure Description

[0017] Figure 1 This is a process flow diagram of the aerogel powder and its supercritical drying preparation method according to this application.

[0018] Figure 2 A schematic diagram of the framework provided for this application.

[0019] Figure 3 This is a schematic diagram of the structure of the tray and gas distribution plate provided in this application.

[0020] Figure 4 Assembly drawing of the pallet and frame provided in this application.

[0021] Figure 5 This is a SEM comparison image of the aerogel powders obtained in Example 1 and Comparative Example 1 of this application.

[0022] Figure 6 This is the pressure-temperature-time curve for preparing aerogel powder in a dry, enclosed environment according to this application.

[0023] Attached image labels: 1. Frame; 2. Tray; 21. Through hole; 3. Airflow distribution plate. Detailed Implementation

[0024] The technical solutions of the embodiments of this application will be described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments.

[0025] In a first aspect, this application provides a supercritical drying method for preparing aerogel powder, referring to... Figure 1 It includes the following steps: Step S1: Place the wet gel in a dry and sealed environment, and continuously introduce liquid CO2 at a supercritical pressure P1 into the dry and sealed environment until the wet gel is completely immersed in the liquid CO2; wherein, before introducing the liquid CO2, the dry and sealed environment is at or below atmospheric pressure.

[0026] In some embodiments, P1 is 10 MPa-15 MPa. Optionally, P1 can be 10 MPa, 11 MPa, 12 MPa, 13 MPa, 14 MPa, and 15 MPa, or other values ​​or ranges within that range. In traditional atmospheric pressure drying processes, the organic solvent within the pores of the wet gel generates capillary pressure during vaporization. This strong contractile force easily leads to irreversible collapse and severe volume shrinkage of the gel's nanoscale porous framework. The supercritical pressure of the liquid CO2 in this application is within the aforementioned range, forming a supercritical fluid with good miscibility with organic solvents. This allows the organic solvent to be displaced without damaging the gel framework. Simultaneously, the supercritical fluid is in a gas-liquid inseparable state with zero surface tension, eliminating the capillary force between the liquid phase and the gel framework during drying. This maximizes the preservation of the original three-dimensional nano-network structure of the wet gel, effectively preventing the collapse of the pore structure and material shrinkage.

[0027] Step S2: CO2 at supercritical temperature T1 and supercritical pressure P1 is introduced into the drying and sealed environment until both temperature T2 and pressure P2 in the drying and sealed environment reach the supercritical state. Then, the drying and sealed environment is circulated and dried to obtain aerogel powder.

[0028] In some embodiments, after CO2 at a supercritical temperature T1 and a supercritical pressure P1 is introduced into a dry, sealed environment, the heating rate within the dry, sealed environment is 0.5℃ / min to 1℃ / min. Optionally, the heating rate can be 0.5℃ / min, 0.6℃ / min, 0.7℃ / min, 0.8℃ / min, 0.9℃ / min, and 1℃ / min, or other values ​​or ranges within that range. After CO2 at a supercritical temperature T1 and a supercritical pressure P1 is introduced into the dry, sealed environment, the CO2 can heat the temperature within the dry, sealed environment in situ. The heating rate within the dry, sealed environment is within the above-mentioned range, avoiding thermal shock to the gel skeleton caused by rapid heating and protecting the structural integrity of the gel skeleton.

[0029] In some embodiments, T1 > 31.1℃. Optionally, T1 can be 32℃, 35.1℃, 40.1℃, 45.1℃, and 50.1℃, or other values ​​or ranges within this range. When the supercritical temperature of the introduced CO2 is within the above range, the heating process within the dry, sealed environment can be slowly and precisely controlled. This allows the liquid CO2 within the dry, sealed environment to directly transform into a supercritical fluid through in-situ heating at the supercritical temperature, without any vaporization phase change. This avoids the formation of a gas-liquid interface during the phase change process, eliminates capillary force damage, and fundamentally protects the structural integrity of the gel skeleton. Further, T1 can be 35℃-55℃.

[0030] In some embodiments, after the temperature and pressure in the dry, enclosed environment reach a supercritical state, T2 > 31.1℃ and P2 > 7.4 MPa. Optionally, T1 can be 33.1℃, 35.1℃, 40.1℃, 45.1℃, and 50.1℃, etc., and P1 can be 7.5 MPa, 9 MPa, 11 MPa, 13 MPa, and 15 MPa, etc., or other values ​​or ranges within the range. When the temperature and pressure in the dry, enclosed environment are within the above ranges, the cyclic drying process can be ensured to operate stably within a stable supercritical window, avoiding the generation of a gas-liquid interface during the phase change process and protecting the structural integrity of the gel skeleton during the cyclic drying process.

[0031] In some embodiments, the purity of the liquid CO2 is ≥99%. Optionally, the purity of the liquid CO2 can be 99%, 99.2%, 99.3%, 99.4%, 99.5%, 99.6%, and 99.7%, or other values ​​or ranges within that range. The purity of the liquid CO2 used to displace air and residual organic solutions is within the above range, ensuring that the entire cold pressurization and displacement process falls within the homogeneous supercritical fluid range with zero surface tension. This allows for continuous extraction and displacement of the organic solvent without secondary wetting, thereby completely preserving the gel skeleton.

[0032] Compared to existing technologies, the supercritical drying method for preparing aerogel powder provided in this application employs a staged processing technology combining cold pressurization and displacement with slow preheating. First, supercritical liquid CO2 is introduced into a dry, sealed environment at atmospheric or below atmospheric pressure. Initially, the liquid CO2 vaporizes due to pressure changes. This vaporized, low-temperature CO2 increases the pressure within the sealed environment while simultaneously addressing the issue of high-temperature CO2 impacting the gel skeleton, thus protecting the structural integrity of the gel skeleton. As the pressure within the sealed environment continues to increase, the vaporized CO2 reverts to liquid CO2. The wet gel is completely immersed in liquid CO2 to displace the air and residual organic solvent in the pores of the wet gel. Then, with the introduction of CO2 at supercritical temperature and pressure, the dry and sealed environment is slowly heated and pressurized. This avoids thermal shock to the gel skeleton caused by pressure fluctuations and rapid temperature rise in the dry and sealed environment. Moreover, the liquid CO2 in the dry and sealed environment is directly transformed into a supercritical fluid through in-situ heating of CO2 at supercritical temperature. There is no vaporization phase change in this stage, which avoids the formation of gas-liquid interface during the phase change process and fundamentally protects the structural integrity of the gel skeleton.

[0033] Secondly, this application provides an aerogel powder, which is prepared by the supercritical drying preparation method of any one of the first aspects of the aerogel powder, and the aerogel powder has good gel skeleton structure integrity.

[0034] Thirdly, please refer to Figures 2-4This application provides a support device for implementing the supercritical drying preparation method of aerogel powder according to any one of the first aspects.

[0035] Fourthly, refer to Figure 1 This application also provides a drying device, which includes a drying kettle, a liquid CO2 source, a booster pump, a preheater, a bypass pipeline, a control unit, and a carrying device according to any of the third aspects. The preheater is connected to the booster pump and the drying kettle. The inlet end of the preheater is provided with an inlet valve and a pressure equalization valve. The bypass pipeline bypasses the preheater and connects to the booster pump and the drying kettle. A bypass valve is provided on the bypass pipeline. The control unit is configured to control the opening and closing of the inlet valve and the bypass valve. The liquid CO2 source, booster pump, bypass valve, bypass pipeline, and drying kettle form a fluid path for the cold pressurization and displacement stage; the liquid CO2 source, booster pump, inlet valve and pressure equalization valve, preheater, and drying kettle form a fluid path for the slow switching preheating stage. The pressure equalization valve can balance the pressure between the preheater and the drying kettle.

[0036] The liquid CO2 source is used to store and supply dry liquid CO2 to the drying vessel. The drying vessel is equipped with a cavity, and the CO2 output from the liquid CO2 source enters the cavity of the drying vessel.

[0037] The support device is housed in a dry, enclosed environment provided by the cavity, and includes a frame 1, a breathable hood (not shown) covering the frame 1, multiple stacked trays 2 installed inside the frame 1, and an airflow distribution plate 3 arranged at the bottom of each tray 2. The tray 2 is used to lay the wet gel. Multiple trays are stacked and placed inside the frame 1. The vent hood has vent holes (not shown in the figure), and the pore size of the vent holes is smaller than the particle size of the aerogel powder, so that CO2 in the cavity can enter the frame 1, but the aerogel in the frame 1 cannot diffuse out of the frame 1. The bottom wall and side wall of the tray 2 are provided with through holes 21, and the pore size of the through holes 21 is smaller than the particle size of the aerogel powder, to prevent the aerogel powder from leaking out of the tray. The airflow equalization plate 3 installed at the bottom of the tray 2 has regularly arranged holes. When CO2 entering the drying kettle passes through the dense and uniformly distributed holes on the airflow equalization plate 3, the flow rate in the high-speed area is weakened due to the greater local resistance loss of the holes, while the low-speed area is relatively easier to pass through. This creates a redistribution of pressure and velocity behind the plate, so that the originally biased or uneven CO2 airflow tends to be uniform after passing through the airflow equalization plate 3, and finally the CO2 airflow enters the tray 2 evenly. Compared to existing technologies, the carrier device provided in this application uses a breathable hood to buffer the impact of CO2 fluid, preventing damage to the gel skeleton during process switching of the wet gel. Simultaneously, the design of the airflow distribution plate 3 and the tray 2 ensures the uniformity of the CO2 fluid flow rate and temperature within the dry, enclosed environment, preventing thermal shock caused by pressure fluctuations and rapid temperature increases, further protecting the structural integrity of the gel skeleton. In some embodiments, the carrier device also includes a fiber mesh (not shown), laid on the bottom wall of the tray 2. The mesh pore size is 1 / 3 to 1 / 2 of the minimum particle size of the aerogel powder. The relationship between the mesh pore size and the particle size of the aerogel powder is within the aforementioned range, allowing the fiber mesh to physically intercept the aerogel powder while allowing organic solvents to pass through, preventing the gel skeleton from collapsing due to defects.

[0038] The booster pump connects the outlet of the liquid CO2 source and the inlet of the drying vessel, and can be used to pressurize the liquid CO2 to the required supercritical pressure before introducing it into the drying vessel.

[0039] The preheater and bypass pipeline work together. After CO2 flows through the preheater and is heated to the supercritical temperature, it enters the drying kettle through the bypass pipeline.

[0040] In practical applications, please refer to Figure 1 The supercritical drying preparation method for the above-mentioned aerogel powder using drying equipment includes two stages.

[0041] Phase 1: Cold pressing and displacement.

[0042] (1) Place the wet gel in the drying kettle, close the inlet valve of the preheater, and open the bypass valve to connect the booster pump to the drying kettle.

[0043] (2) The booster pump pressurizes the dry liquid CO2 delivered by the liquid CO2 source to the supercritical pressure P1 and directly introduces it into the drying kettle in the form of cold high-pressure liquid.

[0044] (3) When cold high-pressure liquid CO2 enters the drying vessel, it vaporizes instantly (because the initial pressure inside the vessel is normal or below normal) to form CO2 gas at a low temperature, which has a small impact on the wet gel. As the time of introduction increases, the pressure increases and CO2 liquefies.

[0045] (4) Continue to introduce CO2 until the wet gel is completely immersed in liquid CO2 and the air and residual organic solvent in the gel skeleton are displaced.

[0046] In the first stage, the CO2 gas supplied by the liquid CO2 source can be dried by a drying filter and then cooled into liquid by a condenser. A flow meter can be installed at the output end of the booster pump to detect the flow rate of liquid CO2 entering the drying vessel.

[0047] Second stage: slow switching and heating drying.

[0048] (1) After confirming that the wet gel in the drying kettle has been completely immersed in liquid CO2, first use the equalizing valve to balance the pressure between the preheater and the drying kettle.

[0049] (2) Close the bypass valve, disconnect the booster pump from the drying kettle, and open the inlet valve of the preheater at the same time.

[0050] (3) CO2 at supercritical pressure P1 is heated to supercritical temperature T1 by the preheater and then enters the drying kettle. The pressure inside the drying kettle remains stable and the temperature rises slowly.

[0051] (4) When the drying vessel reaches the supercritical state (the drying vessel is equipped with a temperature gauge and a pressure gauge, the temperature gauge detects T2>31.1℃, and the pressure gauge detects P2>7.4MPa), the circulation system is turned on for dynamic drying until the organic solvent is completely removed.

[0052] In the second stage, a back pressure regulating valve can be used to reduce the pressure of the supercritical CO2 fluid at the outlet of the drying vessel, so that it is in a pressure range suitable for solvent separation when it enters the separation vessel. Then, the pressure / temperature reduction in the separation vessel allows organic solvents such as ethanol to be separated from CO2. The solvent is recovered through a collection tank, and the CO2 is discharged to a mixer, where it is mixed evenly with the CO2 supplied by the liquid CO2 source and participates in the reaction again.

[0053] The solution of this application will be described below with reference to specific embodiments: Example 1 (1) Prepare tray 2. Lay fiber mesh (6-20 mesh) on the bottom wall of tray 2. Fill 14 trays 2 with the inside of frame 1 by stacking them on top of each other. Place 650kg of wet gel (95% organic solvent content) evenly in multiple trays 2. The amount of wet gel is 1 / 3 of the height of tray 2. The wet gel in each layer of tray 2 does not contact each other. The diameter of tray 2 is 800mm and the height of each layer is 120mm. The height of frame 1 is 1800mm and the diameter is 960mm. Then place the entire supporting device in the drying kettle, seal the kettle, and check the airtightness.

[0054] (2) The booster pump pressurizes the liquid CO2 supplied by the liquid CO2 source to a supercritical pressure of 13MPa. The above CO2 fluid is directly introduced into the drying kettle in a cold, high-pressure liquid state. The flow continues until the wet gel is completely immersed in the liquid CO2, displacing the air and residual organic solvent in the gel skeleton.

[0055] (3) The pressure of the preheater and the drying kettle is balanced for 60 seconds by the equalizing valve. The bypass valve is closed, the connection between the booster pump and the drying kettle is cut off, and the inlet valve of the preheater is opened at the same time. The supercritical pressure CO2 delivered by the liquid CO2 source flows through the preheater and is heated to the supercritical temperature of 55°C before entering the drying kettle.

[0056] (4) Maintaining a stepped heating and pressurization for 70 minutes: This stage is divided into three sub-steps. The first step, 0-15 minutes, involves initial heating: CO2 at supercritical temperature is introduced and heated in situ through the vessel jacket, raising the temperature inside the drying vessel from room temperature (25°C) to 35°C at a constant rate. At this time, the system pressure naturally rises to about 6.0 MPa as the temperature increases. The second step, 15-25 minutes, involves low-temperature holding: CO2 introduction is stopped to maintain the temperature inside the vessel at 35°C for 10 minutes. This step aims to allow the organic solvent inside the wet gel to exchange heat with the external environment to achieve equilibrium and prevent stress cracking of the skeleton due to local temperature differences. The third step, 25-70 minutes, involves raising the pressure inside the vessel to supercritical pressure: CO2 continues to be introduced for in-situ heating, raising the temperature inside the drying vessel from 35°C to the target temperature of 55°C at a uniform rate. At the same time, the pressure inside the vessel reaches the set 13 MPa.

[0057] (3) Supercritical pressure replacement during the 70min-250min stage: When the temperature inside the drying vessel reaches 55℃ and the pressure stabilizes at 13MPa, the system enters the supercritical state. At this time, the pressure and temperature inside the vessel are higher than the critical point. Open the CO2 inlet and outlet valves to maintain constant pressure flow. Utilize the high diffusivity and solubility of supercritical CO2 to continuously replace and carry out organic solvents such as ethanol in the gel micropores.

[0058] (4) Controllable pressure relief for 250-340 minutes: After the replacement is completed, turn off the heating and start the back pressure valve of the drying kettle to slowly depressurize to atmospheric pressure at a rate of 0.2 MPa / min. During this process, keep the temperature inside the kettle not lower than 40°C.

[0059] (5) Cooling and discharging during the 340min-370min stage: After the pressure returns to zero, maintain the cooling water circulation, reduce the temperature inside the reactor to below 30℃, open the reactor lid and take out the finished product to obtain aerogel powder.

[0060] Comparative Example 1 Unlike Example 1, liquid CO2 was pressurized by a booster pump and heated to a supercritical state (temperature 45°C, pressure 12MPa) by a preheater. Then, the high-temperature supercritical CO2 was introduced into a drying kettle to contact the wet gel. The solvent was circulated away in the supercritical state to obtain aerogel powder.

[0061] Test the aerogel powders obtained in Example 1 and Comparative Example 1: (1) Bulk density: graduated cylinder volume method.

[0062] Free-pouring graduated cylinder method (internal control of enterprises, refer to the principles of GB / T1479.1).

[0063] (2) Volume shrinkage rate: caliper method.

[0064] The enterprise's internal control methods refer to the dimensional measurement approach in QB / T 1548-2015. Vernier calipers are used to measure the length, width, and height of the wet gel before and after supercritical drying, and the volume shrinkage rate is calculated. The measuring instruments conform to GB / T 1214.

[0065] (3) Specific surface area: Nitrogen adsorption BET method (low temperature static volumetric method) GB / T 19587 / ISO 9277.

[0066] (4) Thermal conductivity (25℃): Steady-state method of heat flow meter GB / T 10295-2008.

[0067] (5) Particle size: Dry sieve limit test method (single sieve dry sieve) GB / T 6003.2-2024, refer to GB / T1480-2021.

[0068] (6) Product appearance: visual inspection method, JC / T 2518-2019 "Hydrophobic silica aerogel powder" 5.1 Appearance clause, enterprise internal control visual method.

[0069] The test results are shown in Table 1: Table 1 Test Result Analysis: Refer to the test results in Table 1 and Figure 5 It can be seen that, Figure 5 Image (a) is a SEM image of the aerogel powder obtained in Example 1. Figure 5 (b) is an SEM image of the aerogel powder obtained in Comparative Example 1. It can be seen that, compared with Comparative Example 1, the aerogel powder prepared in Example 1 has a smaller particle size, a more distinct and clear morphology, and better particle dispersion. While maintaining a high specific surface area, the data in Table 1 also proves that the aerogel powder obtained in Example 1 has a lower thermal conductivity, effectively suppressing volume shrinkage during the drying process, improving the powder bulk density and appearance uniformity, and its overall performance is significantly better than that of Comparative Example 1.

[0070] Reference Figure 6 As can be seen, the temperature curve rises in a "step-like" manner, with a clear plateau at 35℃, and then continues to rise to 55℃; the pressure curve rises synchronously with the temperature, reaching a peak of 13 MPa at 70 minutes, then remaining horizontal, and finally declining in a sloping manner. It is evident that in the preparation process of Example 1, the decoupling of pressurization and heating time allows the aerogel powder to maintain equilibrium in a high-pressure environment without a gas-liquid interface, eliminating capillary force damage and preserving the structural integrity of the gel skeleton.

[0071] Furthermore, those skilled in the art should recognize that the above embodiments are merely illustrative of this application and are not intended to limit this application. Any appropriate changes and variations made to the above embodiments within the essential spirit and scope of this application fall within the scope of this application's disclosure.

Claims

1. A method for preparing aerogel powder by supercritical drying, characterized in that, Includes the following steps: The wet gel is placed in a dry, sealed environment, and liquid CO2 at a supercritical pressure P1 is continuously introduced into the dry, sealed environment until the wet gel is completely immersed in the liquid CO2; wherein, before the liquid CO2 is introduced, the dry, sealed environment is at or below atmospheric pressure; CO2 at a supercritical temperature T1 and a supercritical pressure P1 is introduced into the drying and sealed environment until both the temperature T2 and the pressure P2 in the drying and sealed environment reach a supercritical state. Then, the drying and sealed environment is circulated and dried to obtain the aerogel powder.

2. The method for preparing aerogel powder by supercritical drying according to claim 1, characterized in that, P1 is 10 MPa-15 MPa.

3. The method for preparing aerogel powder by supercritical drying according to claim 1, characterized in that, After CO2 at a supercritical temperature T1 and a supercritical pressure P1 is introduced into the dry and sealed environment, the heating rate within the dry and sealed environment is 0.5℃ / min-1℃ / min.

4. The method for preparing aerogel powder by supercritical drying according to claim 1, characterized in that, T1>31.1℃。 5. The method for preparing aerogel powder by supercritical drying according to claim 1, characterized in that, After the temperature and pressure in the dry and enclosed environment both reach the supercritical state, T2 > 31.1℃ and P2 > 7.4 MPa.

6. The method for preparing aerogel powder by supercritical drying according to claim 1, characterized in that, The purity of the liquid CO2 is ≥99%.

7. An aerogel powder, characterized in that, It is prepared by the supercritical drying method for aerogel powder according to any one of claims 1-6.

8. A supporting device, characterized in that, The support device is used to implement the supercritical drying preparation method of aerogel powder according to any one of claims 1-6, and includes a frame, a breathable hood covering the frame, a plurality of stacked trays installed in the frame, and an airflow distribution plate arranged at the bottom of the trays. The ventilated hood is provided with vent holes, and the pore size of the vent holes is smaller than the particle size of the aerogel powder; the bottom wall and side wall of the tray are provided with through holes, and the pore size of the through holes is smaller than the particle size of the aerogel powder; the airflow distribution plate is configured to distribute the introduced CO2 evenly.

9. The bearing device according to claim 8, characterized in that, The supporting device also includes a fiber mesh, which is laid on the bottom wall of the tray, and the mesh size of the fiber mesh is 1 / 3 to 1 / 2 of the minimum particle size of the aerogel powder.

10. A drying apparatus, characterized in that, The drying equipment includes a drying kettle, a liquid CO2 source, a booster pump, a preheater, a bypass pipe, a control unit, and a support device as described in any one of claims 8-9; wherein, the preheater connects the booster pump and the drying kettle, the inlet end of the preheater is provided with an inlet valve, the bypass pipe bypasses the preheater and connects the booster pump and the drying kettle, the bypass pipe is provided with a bypass valve, and the control unit is configured to control the opening and closing of the inlet valve and the bypass valve.