A rare earth metal modified FAU-type molecular sieve adsorbent, its preparation method and application

Rare earth metal modified FAU molecular sieves were prepared by in-situ introduction of rare earth metal ions through submolten salt activation, which solved the problem of insufficient selective adsorption capacity of FAU molecular sieves for CO2/N2 and achieved efficient and low-cost CO2/N2 separation.

CN123102299APending Publication Date: 2026-11-17FUZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611555454.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing FAU-type molecular sieves have insufficient selective adsorption capacity for CO2/N2, and traditional modification methods are complex and costly, making it difficult to meet the needs of industrial applications.

Method used

Rare earth metal ions were introduced in situ using a submolten salt activation method. Rare earth metal modified FAU molecular sieves were prepared by stably dispersing rare earth metal cations in a highly alkaline medium. The unique 4f electronic structure and high charge density of these sieves were used to form a local electrostatic field, thereby achieving efficient separation of CO2 and N2.

Benefits of technology

The prepared rare earth metal modified FAU molecular sieve has high CO2 adsorption capacity and excellent CO2/N2 adsorption selectivity. The synthesis steps are simple and the cost is low, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102299A_ABST
    Figure CN123102299A_ABST
Patent Text Reader

Abstract

This invention discloses a rare-earth metal-modified FAU-type molecular sieve adsorbent, its preparation method, and its application. An activated precursor is obtained by mixing and reacting an aluminum source, a silicon source, sodium hydroxide, a rare-earth metal salt, and water. This precursor is then pulverized and mixed with an alkali source, seed crystals, supplementary silicon source, and water. After aging and hydrothermal crystallization, the product is centrifuged, washed, dried, and calcined to obtain the M-FAU molecular sieve adsorbent, where M represents a rare-earth metal. This invention utilizes the stable dispersion of rare-earth metal cations in a sub-molten salt, highly alkaline medium, matching its hydrolysis behavior with the depolymerization-condensation process of silicon-aluminum species, thus achieving in-situ encapsulation of the rare-earth metal within a zeolite cage. The 4f electron structure and high charge density of the rare-earth metal create a strong local electrostatic field within the cage, resulting in polarized adsorption of CO2 molecules and weakening N2 adsorption. The M-FAU molecular sieve adsorbent exhibits high adsorption capacity for CO2 and excellent CO2 / N2 adsorption selectivity, making it widely applicable for the adsorption and separation of CO2 / N2 mixed gases and showing promising industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of zeolite molecular sieve adsorption and separation, specifically relating to a rare earth metal modified FAU type molecular sieve adsorbent, its preparation method, and its application. Background Technology

[0002] With the acceleration of global industrialization, the massive combustion of fossil fuels has led to a continuous increase in greenhouse gas emissions, primarily carbon dioxide, resulting in increasingly severe global warming. Carbon capture, utilization, and storage (CCUS) technology is considered one of the key technological pathways to achieving carbon neutrality. Among numerous carbon capture technologies, adsorption methods have attracted much attention due to their advantages such as simple processes, low energy consumption, and flexible operation. However, the concentration of carbon dioxide in industrial flue gas is typically low (approximately 10–15%) and often coexists with gases such as nitrogen. Therefore, developing adsorbents with high adsorption capacity and high selectivity for CO2 is crucial for achieving efficient carbon capture.

[0003] FAU-type molecular sieves (Faujasite, also known as octahedral zeolite) are a class of aluminosilicate zeolites with a three-dimensional twelve-membered ring pore structure. Their framework consists of sodalite cages (β-cages) interconnected by double six-membered rings, forming supercages (α-cages) with a pore size of approximately 0.74 nm. Based on the silica-to-alumina ratio of the framework and the types of exchangeable cations, FAU-type molecular sieves mainly include X-type molecular sieves (with a low SiO2 / Al2O3 molar ratio, approximately 2–3) and Y-type molecular sieves (with a high SiO2 / Al2O3 molar ratio, generally greater than 3). Among them, NaX molecular sieves (industrially known as 13X molecular sieves) have advantages such as large specific surface area, well-developed microporous structure, and high cation exchange capacity. The cations within their pores can serve as adsorption active sites, selectively adsorbing polar molecules such as CO2 through electrostatic interactions, thus finding wide application in the field of gas adsorption and separation.

[0004] However, the selective adsorption capacity of unmodified FAU-type molecular sieves for CO2 / N2 still falls short of industrial application requirements. Modifying zeolites with metal cations to regulate their pore structure and surface polarity is an important method to improve zeolite adsorption and separation performance. FAU molecular sieves modified with alkali metal and alkaline earth metal ions have been extensively studied in the field of gas adsorption and separation. In recent years, rare earth metals, due to their unique 4f electron structure and high charge density, have shown good application potential in modifying zeolite adsorbents. Introducing rare earth metal ions into the zeolite framework can enhance the local electric field within the molecular sieve cage, improving the adsorption capacity for polar molecules (such as CO2). However, traditional ion exchange methods suffer from problems such as complex exchange processes, low exchange efficiency, and the potential for damage to the zeolite framework due to frequent hydrothermal exchanges. Metal particles introduced by traditional impregnation methods are limited by the pore size of the zeolite micropores, making it difficult for them to enter the zeolite cage. Most active sites are located on the outer surface of the zeolite, making them prone to aggregation or even detachment, affecting adsorption performance and service life.

[0005] In-situ introduction of metals during zeolite synthesis is one effective way to solve the above problems. Related literature reports methods that use organic ligands or template agents to encapsulate metals in situ within zeolites during synthesis. However, the use of organic template agents and complexing agents leads to high production costs, complex synthesis processes, and the generation of harmful gases during calcination to remove template agents, which is detrimental to the promotion of green industrialization. The submolten salt activation method, as a highly efficient inorganic synthesis technique, utilizes a high-concentration alkaline medium at moderate temperatures (100–300 °C) to depolymerize highly reactive monomeric or oligomeric silicon-aluminum species in solid raw materials, providing a new approach for low-cost, green synthesis of molecular sieves.

[0006] Chinese patent application CN117861613A discloses a zeolite-based adsorbent material for acetylene / ethylene separation, its preparation method, and its application. This invention introduces transition metals during sub-molten salt activation to prepare M@LSX zeolite, using natural minerals and involving transition metals (Ni, Cu, Zn). The application is for acetylene / ethylene separation. Currently, there are no reports on the preparation of FAU-type molecular sieves by introducing rare earth metals during sub-molten salt activation for CO2 / N2 separation. Summary of the Invention

[0007] The purpose of this invention is to provide a rare earth metal modified FAU type molecular sieve adsorbent, its preparation method, and its application.

[0008] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted:

[0009] A method for preparing a rare earth metal modified FAU-type molecular sieve adsorbent includes the following steps:

[0010] 1) Mix aluminum source, silicon source, sodium hydroxide, rare earth metal salt and water, stir evenly to obtain a mixture, place the mixture in an oven, and react at 100~350℃ for 48~60 hours to obtain an activated precursor containing rare earth metal;

[0011] 2) The rare earth metal-containing activated precursor is crushed to obtain activated precursor powder. Then the activated precursor powder is mixed with alkali source, seed crystal, supplementary silicon source and water, and aged at room temperature for 10-16 hours to obtain initial gel.

[0012] 3) The initial gel was transferred into a stainless steel reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 80~160℃ for 22~48 hours to obtain a solid product;

[0013] 4) The above solid product is centrifuged, washed, dried and calcined to obtain M-FAU molecular sieve adsorbent, wherein M is a rare earth metal.

[0014] In step 1), the mass ratio of the aluminum source, silicon source, sodium hydroxide, rare earth metal salt and water is 1:(0.4-0.6):(0.8-1.4):(0.1-0.3):(3-5).

[0015] In step (1), the rare earth metal salt is a nitrate, chloride or acetate of at least one of the following metals: lanthanum, cerium, praseodymium, neodymium, samarium and yttrium.

[0016] In step 2), the mass ratio of the activated precursor powder, alkali source, seed crystal, supplementary silicon source and water is (5-15):1:(0.05-0.12):(0.3-0.5):(20-30).

[0017] In step 1), the silicon source is at least one of solid silica gel, silica sol, water glass, and tetraethyl orthosilicate, and the aluminum source is at least one of sodium aluminate, aluminum sol, and boehmite.

[0018] In step 2), the alkali source is sodium hydroxide, the seed crystal is NaX molecular sieve, and the supplementary silicon source is at least one of silica sol, water glass, and tetraethyl orthosilicate.

[0019] In step 4), the calcination temperature is 250–650°C and the calcination time is 2–8 h.

[0020] This invention introduces metals during the submolten salt activation process without the need for adding organic templates and complexing agents, achieving in-situ synthesis of metals to prepare rare earth metal-modified FAU molecular sieves, which can be applied to the adsorption and separation of CO2 / N2 mixed gases.

[0021] This invention employs the above technical solution, where aluminum source, silicon source, sodium hydroxide, rare earth metal salt, and water are stirred evenly, followed by high-temperature depolymerization via sub-molten salt activation. This depolymerizes the high-polymerized silicon-aluminum species in the solid raw material into highly reactive monopolymerized or oligomeric silicon-aluminum species. Simultaneously, rare earth metal ions are uniformly dispersed in situ during activation. The resulting rare earth metal-containing activated precursor provides all the aluminum source and part of the silicon source for subsequent zeolite synthesis. An initial gel is prepared by adding an alkali source, seed crystals, a supplementary silicon source, and water. The gel is then hydrothermally crystallized, centrifuged, washed, dried, and calcined to obtain M-FAU molecular sieve adsorbent, where M represents a rare earth metal. The obtained adsorbent exhibits high adsorption capacity for CO2 and excellent CO2 / N2 adsorption selectivity, and can be used for the adsorption and separation of CO2 / N2 mixed gases.

[0022] Compared to Chinese patent application CN117861613A, which discloses a zeolite-based adsorbent material for acetylene / ethylene separation, its preparation method, and its application, this invention introduces transition metals during sub-molten salt activation to prepare M@LSX zeolite. The metals involved are divalent transition metals (Ni, Cu, Zn), and the application is for acetylene / ethylene separation. In contrast, the rare earth metals involved in this invention are used to prepare molecular sieves for the adsorption and separation of CO2 / N2 mixed gases. The hydrolysis behavior and mechanism of transition metals and rare earth metals in sub-molten salt strongly alkaline media are fundamentally different. Transition metal ions (such as Ni...) 2+ Cu 2+ Zn 2+ Ni is a divalent cation with a relatively small ionic radius. 2+ Approximately 0.69 Å, Cu 2+ Approximately 0.73 Å, Zn 2+ Approximately 0.74 Å), and its hydroxide precipitate has a low pH (Cu). 2+ Zn begins to precipitate at a pH of approximately 5-6. 2+ Ni 2+ Precipitation occurs at pH approximately 6.5–8. In submolten salt media with high concentrations of NaOH, insoluble hydroxides or hydroxyl oxides tend to form prematurely, leading to agglomeration and uneven distribution of metal species, making it difficult to mix uniformly with silicon and aluminum species at the molecular level. Rare earth metal ions (such as La)... 3+ C e3+ Y 3+ It is a trivalent cation with a relatively large ionic radius (La). 3+ Approximately 1.16 Å, Ce 3+ Approximately 1.14 Å, Y 3+Approximately 1.02 Å), its hydroxide precipitates at a relatively high pH (typically above pH 7.5–9). In strongly alkaline media activated by submolten salt, rare earth metal ions do not precipitate as hydroxides, but rather exist stably as soluble hydroxyl complexes and are uniformly dispersed within the aluminosilicate species. This better matches the depolymerization-condensation process of aluminosilicate species in terms of time and rate, thus allowing them to be in-situ encapsulated into zeolite supercages and framework cation sites during subsequent hydrothermal crystallization along with the construction of the aluminosilicate framework. Furthermore, transition metals primarily utilize their unfilled 3d orbitals to undergo feedback π-complexation with unsaturated hydrocarbon molecules containing π bonds (such as acetylene and ethylene), thereby achieving selective adsorption and separation of hydrocarbons such as acetylene / ethylene. Their targets are mainly organic molecules containing unsaturated bonds. Rare earth metals, due to their unique 4f electronic structure, high charge density, and large ionic radius, mainly achieve efficient CO2 / N2 separation in zeolite supercages by forming a strong local electrostatic field that polarizes and electrostatically interacts with CO2 molecules with large quadrupole moments. Their separation mechanism is fundamentally different from the π-complexation mechanism of transition metals.

[0023] The present invention has the following beneficial effects:

[0024] This invention utilizes the stable dispersion of rare earth metal cations in sub-molten salt, highly alkaline media as soluble hydroxyl complexes or colloidal dispersions, matching their hydrolysis behavior with the depolymerization-condensation process of silicon-aluminum species. This effectively solves the problem of mismatched hydrolysis rates between metal and silicon-aluminum species, allowing rare earth metal cations to enter the zeolite cages and stably distribute within the supercages and framework cation sites. Simultaneously, the unique 4f electron structure and high charge density of rare earth metals create a strong local electrostatic field within the molecular sieve cages, resulting in polarized adsorption of CO2 molecules and weakened adsorption of N2. The prepared M-FAU molecular sieve adsorbent exhibits a high adsorption capacity for CO2 while showing lower N2 adsorption compared to unmodified FAU molecular sieves, thus demonstrating superior CO2 / N2 adsorption selectivity. It can be widely applied in the adsorption and separation of CO2 / N2 mixed gases, showing promising industrial application prospects.

[0025] The rare-earth metal-modified FAU-type molecular sieve adsorbent of this invention has a simple synthesis procedure, mild operating conditions, and low raw material cost. This invention can achieve efficient CO2 / N2 separation at room temperature and pressure, requires simple operating equipment, and is suitable for industrial application. Attached Figure Description

[0026] Figure 1 This is the XRD pattern of the La-FAU molecular sieve adsorbent obtained in Example 1.

[0027] Figure 2 This is the XRD pattern of the Ce-FAU molecular sieve adsorbent obtained in Example 2.

[0028] Figure 3 This is the XRD pattern of the Y-FAU molecular sieve adsorbent obtained in Example 3.

[0029] Figure 4 This is the XRD pattern of the FAU molecular sieve adsorbent obtained in Comparative Example 1.

[0030] Figure 5 The N2 adsorption-desorption isotherm curve of the La-FAU molecular sieve adsorbent obtained in Example 1 is shown.

[0031] Figure 6 The N2 adsorption-desorption isotherm curve of the Ce-FAU molecular sieve adsorbent obtained in Example 2 is shown.

[0032] Figure 7 The N2 adsorption-desorption isotherm curve of the Y-FAU molecular sieve adsorbent obtained in Example 3 is shown.

[0033] Figure 8 The N2 adsorption-desorption isotherm curve of the FAU molecular sieve adsorbent obtained in Comparative Example 1 is shown.

[0034] Figure 9 This is the dynamic breakthrough curve of La-FAU molecular sieve separating a mixture of CO2 and N2 (CO2 15%, N2 85%) at 25 °C and 1 bar.

[0035] Figure 10 This is the dynamic breakthrough curve of Ce-FAU at 25 °C and 1 bar for separating a mixture of CO2 and N2 (CO2 15%, N2 85%).

[0036] Figure 11 This is the dynamic breakthrough curve of Y-FAU at 25 °C and 1 bar for separating a mixture of CO2 and N2 (CO2 15%, N2 85%).

[0037] Figure 12 This is the dynamic breakthrough curve of FAU at 25 °C and 1 bar for separating a mixture of CO2 and N2 (CO2 15%, N2 85%).

[0038] Figure 13 This is a schematic diagram of the BSD-MAB multi-component adsorption breakthrough curve analyzer. Detailed Implementation

[0039] The present invention will be further illustrated below by way of examples, but the scope of the present invention is not limited to these examples.

[0040] Unless otherwise specified, the raw materials, reagents, and methods used in the embodiments are all conventional raw materials, reagents, and methods in the art.

[0041] NaX molecular sieve seed crystals were purchased from the catalyst factory of Nankai University; lanthanum nitrate hexahydrate and yttrium nitrate hexahydrate were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; cerium nitrate hexahydrate was purchased from Shandong Keyuan Biochemical Co., Ltd.; and deionized water was prepared in-house using a laboratory ultrapure water system. Calculations of dynamic adsorption capacities for CO2 and N2 were performed.

[0042]

[0043] In the formula: q is the dynamic adsorption capacity of CO2, mmol / g; V is the total flow rate of the mixed gas, cm⁻¹ 3 / min; m is the mass of the adsorbent, in g; ρ is the mole fraction of CO2 in the gas mixture; v is the standard gas constant at 25℃ and 1 bar, v = 24.5 cm⁻¹ 3 / mmol; t is the time to CO2 adsorption saturation, min; c is the molar concentration of CO2 during the adsorption process, mol / m³. 3 ; The initial molar concentration of N2 in the gas mixture, in mol / m³ 3 .

[0044] Example 1

[0045] A method for preparing a zeolite-based adsorbent (La-FAU molecular sieve adsorbent) for CO2 / N2 separation includes the following steps:

[0046] 1) Synthesis of activated precursors containing rare earth metals:

[0047] Add 37g of deionized water, 10.8g of sodium aluminate, and 5.4g of silica sol to a polytetrafluoroethylene (PTFE) beaker. Stir for 10 minutes until the sodium aluminate is completely dissolved and the silica sol is uniformly dispersed. Then add 2g of La(NO3)3·6H2O and stir for 110 minutes at room temperature to obtain an M-precursor solution. Then add 13g of NaOH and stir for 10 minutes until the NaOH is completely dissolved and then cool to room temperature. Place the PTFE beaker in a high-temperature oven that has been heated to 300°C and react for 48 hours. After that, remove the beaker and pour the activated sample into a pulverizer to pulverize for 2-5 minutes to obtain a metal-containing activated precursor powder.

[0048] 2) Zeolite preparation: The above-mentioned metal-containing activated precursor was pulverized in a pulverizer for 4 min to obtain activated precursor powder. 19.8 g of activated precursor powder was weighed and dissolved in 46.11 g of deionized water. 0.72 g of solid silica gel was added under stirring. After stirring evenly, 1.97 g of NaOH was added, and finally 0.17 g of seed crystals (NaX molecular sieve) was added. The mixture was vigorously stirred and aged at room temperature for 12 h. After the reactants were mixed evenly, they were transferred to a crystallization vessel and crystallized at 100 °C for 34 h. The product was taken out, cooled, centrifuged, washed until neutral, dried at 100 °C for 12 h, and then calcined at 550 °C for 4 h to obtain La-FAU zeolite.

[0049] XRD characterization of La-FAU zeolite revealed characteristic peaks typical of FAU zeolite. Commercial NaX was selected as the standard sample, with a relative crystallinity of 63%.

[0050] The BSD-MAB multi-component adsorption breakthrough curve analyzer (e.g.) was used. Figure 13 As shown, the molecular sieve prepared in Example 1 was applied to a CO2 / N2 breakthrough experiment. Specifically, 0.3 g of La-FAU sample was loaded into the breakthrough column, and the sample was pretreated by purging with helium at 300°C for 1 hour. After the pretreatment was completed and cooled to room temperature, a mixture of CO2 and N2 (15% CO2 and 85% N2) was introduced into the separation column at a total flow rate of 4 mL / min, 25°C, and 1 bar. A mass spectrometer was connected to the gas outlet of the separation column to monitor the composition of the outlet gas in real time. The test results are shown below. Figure 9 As shown, the efflux time for CO2 was 93 minutes. The dynamic adsorption capacity of La-FAU for CO2 was 2.640 mmol / g, and the adsorption capacity for N2 was 0.185 mmol / g. The dynamic adsorption capacity of La-FAU for CO2 was comparable to that of Comparative Example 1, while the adsorption capacity for N2 was lower. The dynamic adsorption capacity ratio of CO2 / N2 was 14.3 (2.640 / 0.185), which was significantly higher than that of Comparative Example 1 (13.7 (2.690 / 0.197), indicating that La-FAU has better CO2 / N2 adsorption selectivity.

[0051] Example 2

[0052] A method for preparing a zeolite-based adsorbent material (Ce-FAU zeolite) for CO2 / N2 separation includes the following steps:

[0053] 1) Synthesis of activated precursors containing rare earth metals:

[0054] Add 32g of deionized water, 8.5g of sodium aluminate, and 4.2g of silica sol to a polytetrafluoroethylene (PTFE) beaker and stir for 10 min. Then add 1.5g of Ce(NO3)3·6H2O and stir at room temperature for 60 min to obtain an M-precursor solution. Next, add 10g of NaOH and stir for 10 min until the NaOH is completely dissolved and then cool to room temperature. Place the PTFE beaker in a high-temperature oven preheated to 300℃ and react for 48 h. After that, remove the beaker to obtain a metal-containing activated precursor. Pour the metal-containing activated precursor into a pulverizer and pulverize for 2-5 min to obtain a metal-containing activated precursor powder.

[0055] 2) Zeolite preparation: The metal-containing activated precursor was pulverized in a pulverizer for 4 min to obtain metal-containing activated precursor powder. 15.3 g of the activated precursor powder was weighed and dissolved in 34.58 g of deionized water. 0.54 g of solid silica gel was added under stirring, and after stirring evenly, 1.48 g of NaOH was added, and finally 0.12 g of seed crystals (NaX molecular sieve) was added. The mixture was vigorously stirred and aged at room temperature for 10 h. After the reactants were mixed evenly, they were transferred to a crystallization vessel and crystallized at 90 °C for 26 h. The product was taken out, cooled, centrifuged, washed until neutral, dried at 100 °C for 12 h, and then calcined at 550 °C for 4 h to obtain Ce-FAU zeolite.

[0056] Ce-FAU zeolite was characterized by XRD, and its characteristic peaks were those of FAU zeolite. Commercial NaX was selected as the standard sample with a relative crystallinity of 67%.

[0057] The BSD-MAB multi-component adsorption breakthrough curve analyzer (e.g.) was used. Figure 13 As shown, the molecular sieve prepared in Example 2 was applied to a CO2 / N2 breakthrough experiment. Specifically, 0.26 g of Ce-FAU sample was loaded into the breakthrough column, and the sample was pretreated by purging with helium at 300°C for 1 hour. After the pretreatment was completed and cooled to room temperature, a mixture of CO2 and N2 (15% CO2 and 85% N2) was introduced into the separation column at a total flow rate of 4 mL / min, 25°C, and 1 bar. A mass spectrometer was connected to the gas outlet of the separation column to monitor the composition of the outlet gas in real time. The test results are shown below. Figure 10 As shown, the efflux time for CO2 was 103 minutes, and the dynamic adsorption capacity of Ce-FAU for CO2 was 2.903 mmol / g, while the adsorption capacity for N2 was 0.184 mmol / g. The dynamic adsorption ratio of CO2 / N2 for Ce-FAU was 15.8 (2.903 / 0.184), which was significantly higher than the 13.7 of Comparative Example 1.

[0058] Example 3

[0059] A method for preparing a zeolite-based adsorbent material (Y-FAU zeolite) for CO2 / N2 separation includes the following steps:

[0060] 1) Synthesis of metal-containing activated precursors:

[0061] Add 30g of deionized water, 6.6g of sodium aluminate and 3.3g of water glass to a polytetrafluoroethylene beaker, stir for 10 min, then add 1g of Y(NO3)3·6H2O, stir at room temperature for 60 min to obtain the M-precursor solution, then add 7g of NaOH, stir for 10 min until the NaOH is completely dissolved and then cool to room temperature. Place the polytetrafluoroethylene beaker in a high-temperature oven that has been heated to 300℃, react for 48 h, then remove the beaker to obtain the metal-containing activated precursor.

[0062] 2) Zeolite preparation: The metal-containing activated precursor was pulverized in a pulverizer for 4 min to obtain metal-containing activated precursor powder. 10.9 g of the activated precursor powder was weighed and dissolved in 40.35 g of deionized water. 0.63 g of solid silica gel was added under stirring, and after stirring evenly, 1.73 g of NaOH was added, and finally 0.15 g of seed crystals (NaX molecular sieve) was added. The mixture was vigorously stirred and aged at room temperature for 10 h. After the reactants were mixed evenly, they were transferred to a crystallization vessel and crystallized at 90 °C for 22 h. The reaction vessel was removed, cooled, centrifuged, washed until neutral, dried at 100 °C for 12 h, and then calcined at 550 °C for 4 h to obtain γ-FAU zeolite.

[0063] XRD characterization of γ-FAU zeolite revealed characteristic peaks typical of FAU zeolite. Commercial NaX was selected as the standard sample, with a relative crystallinity of 76%.

[0064] The BSD-MAB multi-component adsorption breakthrough curve analyzer (e.g.) was used. Figure 13 As shown, the molecular sieve prepared in Example 3 was applied to a CO2 / N2 breakthrough experiment. Specifically, 0.29 g of γ-FAU sample was loaded into the breakthrough column, and the sample was pretreated by purging with helium at 300 °C for 1 hour. After the pretreatment was completed and cooled to room temperature, a mixture of CO2 and N2 (15% CO2 and 85% N2) was introduced into the separation column at a total gas flow rate of 4 mL / min, 25 °C, and 1 bar. A mass spectrometer was connected to the gas outlet of the separation column to monitor the composition of the outlet gas in real time. The test results are shown below. Figure 11 As shown, the efflux time for CO2 was 101 minutes, and the dynamic adsorption capacity of Y-FAU for CO2 was 2.813 mmol / g, while the adsorption capacity for N2 was 0.191 mmol / g. The dynamic adsorption ratio of CO2 / N2 for Y-FAU was 14.7 (2.813 / 0.191), which was higher than the 13.7 of Comparative Example 1.

[0065] Comparative Example 1

[0066] Using the same preparation method as in Example 1, but without adding rare earth metal salts in step 1), unmodified FAU molecular sieve adsorbent FAU was prepared.

[0067] The BSD-MAB multi-component adsorption breakthrough curve analyzer (e.g.) was used. Figure 13 (As shown) The molecular sieve prepared in Comparative Example 1 was applied to a CO2 / N2 breakthrough experiment. Specifically, 0.29 g of FAU sample was loaded into the breakthrough column, and the sample was pretreated with helium at 300℃ for 1 hour. After the pretreatment was completed and cooled to room temperature, a mixture of CO2 and N2 (15% CO2, 85% N2) was introduced into the separation column at a total gas flow rate of 4 mL / min, 25℃, and 1 bar. A mass spectrometer was connected to the gas outlet of the separation column to monitor the composition of the outlet gas in real time. The test results are shown below. Figure 12 As shown. The CO2 effluent time was 95 minutes, and the dynamic adsorption capacity of FAU for CO2 was 2.690 mmol / g, while the adsorption capacity for N2 was 0.197 mmol / g. The CO2 / N2 dynamic adsorption ratio of unmodified FAU was 13.7 (2.690 / 0.197), which was lower than that of Examples 1-3.

[0068] The above embodiments are merely illustrative of the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein, without departing from the spirit and substance defined by the claims of the present invention; and such modifications or substitutions are still within the scope defined by the claims of the present invention.

Claims

1. A process for the preparation of a rare earth metal modified FAU type molecular sieve adsorbent, characterized in that, Includes the following steps: 1) Mix aluminum source, silicon source, sodium hydroxide, rare earth metal salt and water, stir evenly to obtain a mixture, place the mixture in an oven, and react at 100~350℃ for 48~60 hours to obtain an activated precursor containing rare earth metal; 2) The rare earth metal-containing activated precursor is crushed to obtain activated precursor powder. Then the activated precursor powder is mixed with alkali source, seed crystal, supplementary silicon source and water, and aged at room temperature for 10-16 hours to obtain initial gel. 3) The initial gel was transferred into a stainless steel reactor with a polytetrafluoroethylene liner and hydrothermally crystallized at 80~160℃ for 22~48 hours to obtain a solid product; 4) The above solid product is centrifuged, washed, dried and calcined to obtain M-FAU molecular sieve adsorbent, wherein M is a rare earth metal.

2. The method of claim 1, wherein the rare earth metal modified FAU type molecular sieve adsorbent is prepared by the steps of: In step 1), the mass ratio of the aluminum source, silicon source, sodium hydroxide, rare earth metal salt and water is 1:(0.4-0.6):(0.8-1.4):(0.1-0.3):(3-5).

3. The method of claim 1, wherein the rare earth metal modified FAU type molecular sieve adsorbent is prepared by the steps of: In step 1), the rare earth metal salt is a nitrate, chloride, or acetate of at least one of the following metals: lanthanum, cerium, praseodymium, neodymium, samarium, and yttrium.

4. The method of claim 1, wherein the rare earth metal modified FAU type molecular sieve adsorbent is prepared by the steps of: In step 2), the mass ratio of the activated precursor powder, alkali source, seed crystal, supplementary silicon source and water is (5-15):1:(0.05-0.12):(0.3-0.5):(20-30).

5. The method of claim 1, wherein the rare earth metal modified FAU type molecular sieve adsorbent is prepared by the steps of: In step 1), the silicon source is at least one of solid silica gel, silica sol, water glass, and tetraethyl orthosilicate, and the aluminum source is at least one of sodium aluminate, aluminum sol, and boehmite.

6. The method of claim 1, wherein the rare earth metal-modified FAU-type molecular sieve adsorbent is prepared by the steps of: In step 2), the alkali source is sodium hydroxide, the seed crystal is NaX molecular sieve, and the supplementary silicon source is at least one of silica sol, water glass, and tetraethyl orthosilicate.

7. The method of claim 1, wherein the rare earth metal modified FAU type molecular sieve adsorbent is prepared by the steps of: In step 4), the calcination temperature is 250~650℃ and the calcination time is 2~8 h.

8. The rare earth metal modified FAU type molecular sieve adsorbent obtained by the preparation method according to any one of claims 1 to 7.

9. The application of the rare earth metal modified FAU molecular sieve adsorbent obtained by the preparation method according to any one of claims 1 to 7 in the selective separation of CO2 / N2 mixed gas.

Citation Information

Patent Citations

  • Zeolite-based adsorption material for separation of acetylene and ethylene as well as preparation method and application of zeolite-based adsorption material

    CN117861613A