A photocatalyst for degrading microplastic pollutants and its preparation method
By designing a tetraazabenzoporphyrin photocatalyst, the problems of limited light response range and low physical contact efficiency were solved, and efficient photocatalytic degradation and separation recycling of microplastics were achieved.
Patent Information
- Application Number
- CN202611098180.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photocatalysts have limited light response range when degrading microplastic pollutants, and the physical contact efficiency between hydrophobic microplastics and inorganic catalysts with good water dispersibility is low, which affects the efficiency of active species transfer and attack, making it difficult to achieve efficient degradation.
Design a photocatalyst whose molecular structure includes a tetraazabenzoporphyrin as the photoactive core, with long-chain alkyl groups linked by phosphorus hydroxyl and quaternary ammonium groups to form a hydrophobic and oleophilic amphiphilic structure, adsorbing microplastics and uniformly dispersing them in the aqueous phase, and using singlet oxygen to achieve oxidative degradation.
It achieves efficient photocatalytic degradation of microplastics, with high singlet oxygen quantum yield, uniform molecular dispersion in aqueous phase, easy separation and recovery, and a degradation rate of up to 55%.
Smart Images

Figure CN123102421A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photocatalyst technology, specifically to a photocatalyst for degrading microplastic pollutants and its preparation method. Background Technology
[0002] Microplastics (plastic particles with a diameter of less than 5 mm) are an emerging persistent pollutant widely distributed in the global aquatic environment, posing a serious threat to ecosystems and human health. Traditional physical filtration and biological treatment methods are not satisfactory in removing microplastic particles from water, especially for nanoscale microplastics. Therefore, developing efficient and green microplastic degradation technologies has become an urgent need in the field of environmental governance.
[0003] Photocatalysis, which uses light energy to drive chemical reactions, can mineralize or convert organic pollutants into harmless substances at room temperature and pressure, and is considered one of the most promising methods for treating microplastic pollution. Currently, published patents for the photocatalytic degradation of microplastics mainly focus on inorganic semiconductor materials. For example, constructing heterojunctions (such as C3N4-based, Co3O4 / CeO2, CuO / TiO2, bismuth-based composites, etc.) can improve the separation efficiency of photogenerated carriers, thereby enhancing the degradation capacity of microplastics such as polyethylene terephthalate (PET). In addition, some studies have converted microplastics themselves into carbon quantum dots for constructing composite photocatalysts.
[0004] However, existing technologies still have some limitations: First, most semiconductor catalysts have limited photoresponse ranges, and the utilization rate of visible light needs to be improved. Second, microplastic surfaces are usually hydrophobic, and the physical contact efficiency between many water-dispersible inorganic catalysts and microplastics is low, affecting the transfer and attack efficiency of active species (such as hydroxyl radicals) to the microplastic surface. Although some studies have attempted to develop amphiphilic materials (such as amphiphilic CoP / g-C3N4) to improve interfacial contact, designing molecular photocatalysts that combine efficient light harvesting, strong interfacial adsorption, and high reactive oxygen generation capabilities remains a challenge.
[0005] Unlike semiconductor catalysis based on electron-hole pairs, the photosensitization pathway uses a photocatalyst to absorb light energy, exciting ground-state oxygen (³O₂) into highly reactive singlet oxygen (¹O₂), thereby achieving the oxidative degradation of microplastics such as polyethylene. Phthalocyanines, porphyrins, and other macrocyclic conjugated organic molecules are commonly used photocatalysts, exhibiting high singlet oxygen quantum yields and good photostability. However, traditional water-soluble organic photocatalysts have weak affinity for hydrophobic microplastics; while lipophilic photocatalysts are difficult to disperse uniformly in an aqueous phase. Summary of the Invention
[0006] The purpose of this invention is to overcome the shortcomings of the existing technology and provide a photocatalyst for degrading microplastic pollutants and its preparation method.
[0007] To achieve the above objectives, the technical solution of the present invention is: a photocatalyst for degrading microplastic pollutants, the general molecular structure of which is shown in formula (Ⅰ):
[0008] Equation (I) In formula (Ⅰ), R1 is selected from C1~C3 straight-chain alkyl groups; R2 is selected from tert-butyl, phenyl, or p-tert-butylphenyl; R3 is selected from a straight-chain alkyl group of C12, C16 or C18.
[0009] Another technical solution of the present invention is: a method for preparing the aforementioned photocatalyst for degrading microplastic pollutants, comprising the following steps: (1) 4,5-Dimethylphthalonitrile undergoes a free radical substitution reaction with a brominating reagent in toluene solution under the initiator to generate 4,5-dibromomethylphthalonitrile, named Pn1; (2) Compound Pn1 was subjected to a cyclization reaction with di(N-alkyl)ethylenediamine under alkaline conditions and in an aprotic solvent to generate a dinitrile compound with a tetrahydropyrazine structure, which was named Pn2; (3) Compound Pn2 was subjected to an amination reaction with an amination reagent in n-butanol solution under the catalysis of a strong base catalyst to obtain an intermediate with an iminoisoindoline structure, named IntA; (4) The compound with the butenedionitrile structure was subjected to an amination reaction with an amination reagent in an ethanol solution to obtain an intermediate with a diimine pyrrole structure, named IntB; (5) Intermediate IntA and intermediate IntB are mixed in n-butanol solution, and lithium metal is added to carry out cyclization condensation reaction to generate porphyrin dilithium with tetraazamonobenzoporphyrin structure. Then, acid is added to carry out hydrolysis reaction to remove lithium ions, and tetraazamonobenzoporphyrin compound is obtained and named tambp. (6) The compound tambp was reacted with phosphorus tribromooxyphosphorus POBr3 in pyridine solution to obtain a phosporphyrin compound, named ptambp; (7) The compound ptambp was reacted with 1-chloro-straight-chain alkanes in acetonitrile solution under the catalysis of an alkaline catalyst to obtain the target product photocatalyst, named ptambp+.
[0010] The synthesis route diagram is as follows:
[0011] Further; the brominating reagent in step (1) is selected from N-bromosuccinimide (NBS), 1,3-dibromo-5,5-dimethylhydantoin (DBH) or liquid bromine; the initiator is selected from azobisisobutyronitrile (AIBN), dimethyl azobisisobutyrate (AIBME) or benzoyl peroxide (BPO); the molar ratio between 4,5-dimethylphthalonitrile, the brominating reagent and the initiator is 1:(1~1.5):(0.04~0.1), the mass-volume ratio of 4,5-dimethylphthalonitrile to toluene is (1~2) g:20 mL, the reaction temperature is 75~85℃, and the reaction time is 2~4 h.
[0012] Further; in step (2), the molar ratio of compound Pn1 to di(N-alkyl)ethylenediamine is 5:(5.5~6), and the mass-to-volume ratio of compound Pn1 to the aprotic solvent is (1~2) g:10 mL; the aprotic solvent is selected from N,N-dimethylformamide (DMF) or dimethyl sulfoxide (DMSO); the alkyl group in the di(N-alkyl)ethylenediamine is selected from methyl, ethyl or n-propyl; the alkaline conditions are adjusted to pH=9.5~10.5 using K2CO3 or Na2CO3; the cyclization reaction temperature is the reflux temperature, and the reaction time is 1~5 h.
[0013] Further; in step (3), the molar ratio of compound Pn2 to strong base catalyst and amination reagent is 3:(0.1~0.3):(6-9), the mass-volume ratio of compound Pn2 to n-butanol is (6~7) g:100mL, the strong base catalyst is selected from sodium methoxide, sodium ethoxide or lithium isopropoxide, the amination reagent is selected from ammonia, ammonium acetate or urea, the amination reaction temperature is reflux temperature, and the reaction time is 4~6h.
[0014] Further; in step (4), the molar ratio of the compound with the butenedionitrile structure to the amination reagent is 1:(1~2), the mass-volume ratio of the compound with the butenedionitrile structure to ethanol is (2~3) g:30 mL, the compound with the butenedionitrile structure is selected from cis-2-tert-butyl,2-butenedionitrile, cis-2-phenyl,2-butenedionitrile or cis-2-p-tert-butyl-phenyl,2-butenedionitrile, the amination reagent is ammonium acetate, the amination reaction temperature is the reflux temperature, and the reaction time is 7~10 h.
[0015] Further; in step (5), the molar ratio of intermediate IntA, intermediate IntB and lithium metal is 1:3:(1~3), the mass-volume ratio of intermediate IntA to n-butanol is (4~5) g:150 mL, the mass-volume ratio of intermediate IntA to acid is (4~5) g:250 mL, the acid is 0.1 M HCl, the cyclization condensation reaction temperature is the reflux temperature, the reaction time is 10~12 h, the hydrolysis reaction temperature is 60~80 °C, and the reaction time is 0.5~2 h.
[0016] Further; in step (6), the molar ratio of compound tambp to phosphorus tribromooxyphosphorus (POBr3) is 1:(1~1.2), the mass-volume ratio of compound tambp to pyridine solution is (6~7) g:125 mL, the reaction temperature is 60~80℃, and the reaction time is 4~6 h.
[0017] Further; in step (7), the molar ratio of compound ptambp to 1-chloro linear alkane and basic catalyst is 1:(4~6):(1~2), the 1-chloro linear alkane is selected from 1-chlorododecane, 1-chlorohexadecane, and 1-chlorooctadecane, the basic catalyst is selected from K2CO3 or Na2CO3, the reaction temperature is 60~80℃, and the reaction time is 8~12h.
[0018] Another technical solution of the present invention is: the application of the aforementioned photocatalyst in the photocatalytic oxidation degradation of microplastics, wherein the photocatalyst adsorbs microplastics in an aqueous phase with hydrophobic straight-chain alkyl groups and maintains the aqueous phase dispersion with hydrophilic quaternary ammonium salt groups to form micelles, thereby achieving photocatalytic degradation of microplastics; wherein the microplastics are selected from one or more of polyethylene, polyvinyl chloride, and polystyrene.
[0019] The beneficial effects of this invention: The photocatalyst molecule of this invention uses tetraaza-monobenzophosporphyrin as the photoactive core, ensuring a high singlet oxygen quantum yield and strong absorption in the visible light region (Q band approximately 685 nm). The four long-chain alkyl groups attached to the phosphorus hydroxyl and quaternary ammonium groups provide strong hydrophobicity. The two quaternary ammonium salt groups (-N) introduced on the benzo[a] ring through a quaternization reaction... + (R 2 )3X -This modification provides strong hydrophilicity. The optimized molecular configuration exhibits a three-dimensional amphiphilic structure with one hydrophilic end and one lipophilic end. This allows the molecule to adsorb and encapsulate equally hydrophobic microplastics in aqueous solutions via long alkyl chains, significantly shortening the transport distance of reactive oxygen species (singlet oxygen). Simultaneously, the hydrophilic quaternary ammonium salt groups can be effectively dispersed in the aqueous reaction system, ensuring uniform dispersion of the photocatalyst and light energy capture. The resulting micelle solution is easily decomposed by strong electrolytes or thermal heating, facilitating the separation and recovery of the photocatalyst from the reaction system. Attached Figure Description
[0020] Figure 1 This is the spatial configuration of the photocatalyst ptambp+ prepared in Example 1; Figure 2 The image shows the MALDI-TOF MS spectrum of the intermediate product ptambp from Example 1; the inset (A) is a magnified view of the mass spectrometry peaks to show the isotope peaks and their relative abundances, and the small image (B) embedded in the inset (A) is the isotope peaks and their relative abundances simulated by the software theory. Figure 3 It is the photocatalyst ptambp+ prepared in Example 1. 1 H-NMR spectrum; Figure 4 The image shows the MALDI-TOF MS spectrum of the photocatalyst ptambp+ prepared in Example 1; the inset (A) is a magnified view of the mass spectrum peaks to show the isotope peaks and their relative abundances, and the small image (B) embedded in the inset (A) is the isotope peaks and their relative abundances simulated by the software theory. Figure 5 This is the UV-Vis spectrum of the photocatalyst ptambp+ prepared in Example 1 in water and DMSO; Figure 6 This is a diagram showing the critical micelle concentration of the photocatalyst ptambp+ prepared in Example 1 in water; Figure 7 This is an ABDA absorbance decay curve of the singlet oxygen quantum yield of the photocatalyst ptambp+ prepared in Example 1; the inset is a kinetic curve of ABDA concentration change during the test of singlet oxygen quantum yield; Figure 8 This is a graph showing the degradation curve of the photocatalyst ptambp+ prepared in Example 1 on microplastics, where the inset graph is a graph showing the change of carbonyl index on the surface of the microplastics; Figure 9 These are infrared spectra of microplastics before and after photocatalytic degradation. Detailed Implementation
[0021] Example 1:
[0022] A method for preparing the photocatalyst for degrading microplastic pollutants includes the following steps: (1) 15.8 g (0.1 mol) of 4,5-dimethylphthalonitrile and 0.82 g (0.005 mol) of AIBN were dissolved in 200 mL of anhydrous toluene and heated to 80 °C under argon protection. 18.7 g (0.105 mol) of NBS was added (in batches of 1 g at 2-minute intervals). After the addition was complete, the reaction was continued for 2 h. The organic phase was separated by washing with water. After the solvent was removed by vacuum evaporation, the crude product was purified by recrystallization with acetonitrile as solvent to obtain 26.7 g of compound Pn1, with a yield of about 85% based on 4,5-dimethylphthalonitrile. (2) Take 15.7 g (0.05 mol) of compound Pn1 obtained in step (1) and 8.6 g (0.053 mol) of di(N-methyl)ethylenediamine and dissolve it in 100 mL of DMF. Add 3.5 g (0.025 mol) of K2CO3 and reflux the reaction under argon protection for 2 hours. After the reaction is complete, filter out the K2CO3 particles, add 200 mL of water to dilute and extract with ethyl acetate. Wash the organic phase with water and dry it. Then, recover the solvent under reduced pressure to obtain about 10 g of crude product Pn2. (3) Take 6.36g (0.03mol) of compound Pn2 prepared in step (2) and mix it with 1.08g (0.002mol) sodium methoxide and dissolve it in 100 mL of n-butanol. Heat it to reflux under the protection of argon and reflux bubble reaction for 4 hours. During the reaction, dry ammonia gas is slowly introduced at a flow rate of 0.1 L per minute. After the reaction is completed, the n-butanol is recovered under reduced pressure. After washing with 0.1M dilute hydrochloric acid, the precipitate is collected, dried and separated and purified by alumina column chromatography with ethyl acetate and n-hexane (volume ratio 3:7) as eluent to obtain intermediate IntA; (4) 13.4 g (0.1 mol) of cis-2-tert-butyl,2-butenedionitrile (FumaN) and 11.5 g (0.15 mol) of ammonium acetate were mixed in 150 mL of ethanol and refluxed for 8 hours. After the reaction was completed, the solvent was recovered by vacuum evaporation, and the unreacted ammonium acetate was washed away with water. The product was then purified by recrystallization in 0.1 M hydrochloric acid to obtain 10.5 g of intermediate IntB, with a yield of approximately 75% based on FumaN. (5) Take 9g (0.06mol) of IntB prepared in step (4) and 4.58g (0.02mol) of IntA prepared in step (3), and 0.24g (0.034mol) of lithium scrap, mix them in 150 mL of n-butanol, reflux for 12 hours under argon protection, and after the solvent is recovered under reduced pressure, add 250 mL of 0.1M hydrochloric acid to the remaining reactants, stir at 60°C for 2 hours, filter out the solid product, wash and neutralize with water, and purify on a silica gel column using dichloromethane and methanol (volume ratio 8:2) as the developing solvent to obtain 7.4 g of dark purple solid product tambp, with a yield of about 65% based on IntA; (6) Dissolve 6.16 g (9 mmol) tambp in 100 mL of pyridine, heat to 80 °C under argon protection, add 2.87 g (10 mmol) POBr3 (POBr3 was pre-dissolved in 25 mL of pyridine), continue heating for 4 hours after the addition is complete, destroy the remaining POBr3 with 1 M sodium carbonate solution until no more bubbles are produced, evaporate the solvent under reduced pressure to recover the solvent, and purify the crude product on a silica gel column using pyridine and toluene (volume ratio 8:2) as the developing solvent to obtain 5.00 g ptambp, with a yield of approximately 80% based on tambp; Characterization of ptambp: MALDI-TOF-MS (ethanol solvent, DHB matrix, see...) Figure 2 ): cal.: 679.34 (100%), 680.35(44.3%), 681.35(12.7%), 682.34(2.9%); found: 679.35 (M+, 100%), 680.34 (45%), 681.35 (12.9%); 662.35 (M loses one OH group, 100%), 663.35 (45%), 664.35 (12.1%). The spectrum shows an M+ molecular ion peak at 679.3 and an M-17 peak at 662.3, which is the peak of ptambp dissociating one OH group. The isotopic abundance is consistent with the theoretical simulation value.
[0023] (7) Dissolve 5g ptambp (7.3mmol) and 7.5g (36.5mmol) 1-chlorododecane in 100ml acetonitrile, add 2g (14mmol) K2CO3, heat to 80℃ under argon protection, react for 10 hours. After the reaction is complete, filter to remove K2CO3, recover acetonitrile under reduced pressure, and purify the crude product by recrystallization with ethanol and water (volume ratio 1:1) to obtain 8.5g of the final product ptambp+, whose molecular structure is as follows, and the yield is approximately 75% based on ptambp.
[0024]
[0025] Characterization of ptambp+: 1 H-NMR (see) Figure 3 d 6 -DMSO, 300MHz): 0.88-0.89 (t, 12H, CH3), 1.26-1.31 (m, 64H, long-chain alkyl), 1.35 (s, 27H, tert-butyl); 1.51 (m, 4H, OC-CH2), 1.73 (m, 4H, NC-CH2), 3.22 (t, 4H, N-CH2), 3.51-3.52 (m, 4H, O-CH2), 3.68 (t, 4H, cyclic N-CH2-CH2-N), 3.75 (s, 6H, N-CH3), 5.22 (m, 2H, benzo[a] ortho-five-membered ring H), 6.10 (s, 1H, benzo[b] para-five-membered ring outer end H), 7.81-7.90 (d, 2H, benzene ring H).
[0026] MALDI-TOF-MS (see) Figure 4 (Ethanol solvent, DHB matrix): cal.: M / 3+ 451.37 (92.6%), 451.70 (100%), 452.02 (44.6%), 452.37 (12.8%), 452.70 (2.7%), 453.02 (1.9%); found: 451.37 (92%), 451.71 (100%), 452.02 (45.1%), 452.35 (12.5%), 452.71 (2.9%); 677.05 (M / 2+, 100%), 676.71 (90%), 677.38 (45%), 677.71 (12%); 1354.1 (M / 1+, 100%), 1353.72 (92%), 1354.5 (40%).
[0027] Measurements were taken in positive ion mode using DHB as the matrix. Since ptambp+ carries three positive charges, the figure shows that the molecular ion peak of M / 3+ is dominant (around 451.70), while the molecular ion peak of M / 2+ with two positive charges (around 677.05) is weaker. The molecular ion peak of M / 1+ with one positive charge (around 1354.1) can also be observed. The intensity and position of the isotope peaks are consistent with the theoretical simulation.
[0028] UV-vis: (see) Figure 5DMSO solvent): 685 nm (Q band), 560 nm, 380 nm, 350 nm (B band); Water solvent (micelle dispersion system): 695 nm (Q band), 600 nm, 360 nm (B band).
[0029] Example 2: Determination of surface activity behavior and photocatalytic ability In aqueous solution, the critical micelle concentration of ptambp+ synthesized in Example 1 was determined to be 0.53 × 10⁻⁶ at 20°C using conductivity. -6 mol / L (see Figure 6 However, due to the large steric hindrance of its molecules, the micelle solution has poor stability. High-speed centrifugation (12,000 rpm, 10 minutes), raising the temperature to 50°C, or adding 1% by mass of the strong electrolyte Al2(SO4)3 can destroy the micelles and cause the solution to aggregate and separate, which is beneficial for the separation and recovery of ptambp+.
[0030] Using 9,10-anthrayl-bis(methylene)dimalonic acid (ABDA) as a singlet oxygen scavenger and tetrasulfonic acid zinc phthalocyanine (singlet oxygen quantum yield 0.45) as a standard reference, the singlet oxygen quantum yield was measured to be 0.52 in micellar solution (see [reference needed]). Figure 7 This indicates that ptambp+ molecules have good photocatalytic ability in the micelle state.
[0031] Example 3: Microplastic Adsorption and Degradation Capacity Test 1. Microplastic treatment: Commercial polyethylene microplastic balls (Zhongke Keyou, average particle size 400-600um) are pre-irradiated with a 250nm wavelength ultraviolet lamp for 1 hour, then etched in 1M NaOH at 40℃ for 1 hour, washed with water until neutral, and dried. 2. Microplastic adsorption capacity test of micelle solution: Add 0.135 g of ptambp+ (2×10) to 500 ml of pure water. -5 M) and 2g of the pretreated microplastics were ultrasonically agitated at 600W for 15 minutes, followed by high-speed shearing and stirring at 1500 rpm for 15 minutes to prepare a micelle solution adsorbed with microplastics. After this step, the mass of microplastic fragments smaller than 0.25µm accounted for approximately 1% of the original mass. Subsequently, the micelle solution was centrifuged at 12000 rpm to break up the micelle solution, separating the aqueous phase and the emulsion suspension. Both phases were filtered through a 0.25µm filter membrane and weighed. The distribution ratio of microplastic particles in the aqueous phase and the emulsion suspension was 1:10, demonstrating that micelles formed by ptambp+ molecules have a better adsorption effect on microplastic particles.
[0032] 3. Determination of photocatalytic degradation ability of microplastics: The micelle solution with microplastics adsorbed as prepared above was subjected to photocatalytic degradation experiments. A 120W xenon lamp with a cooling jacket (Guangzhou Xingchuang Electronics, wavelength 400-700nm) was used for illumination. A blank (2g of the pretreated microplastics added to 500ml of pure water) and a control experiment under dark conditions (0.135g of ptambp+ and 2g of the pretreated microplastics added to 500ml of pure water) were set up. Pure oxygen was introduced, and the photocatalytic degradation experiment was carried out under stirring. During and after the reaction, 25ml samples were taken at certain time intervals, 15mg of Al2(SO4)3 was added, and the temperature was raised to 50℃ to destroy the micelle system. The microplastics were filtered out through a 0.25µm filter membrane, and the degradation weight loss of the microplastics was calculated. The carbonyl index on the surface was also measured (see...). Figure 8 ).
[0033] Experimental results show that under 24 hours of continuous light irradiation, the degradation rate of microplastics, measured by weight loss, can reach 55%, indicating that the singlet oxygen generated by ptambp+ photocatalysis can effectively oxidize and degrade polyethylene microplastics. In the blank experiment, without a photocatalyst, light irradiation only caused a weight loss of less than 5% in the microplastics. The control experiment shows that without light irradiation, the photocatalyst cannot exert its catalytic degradation ability, and the microplastics show almost no weight loss. After 24 hours of photocatalytic degradation, compared with before degradation, the carbonyl index on the surface of the microplastics can reach up to 0.8, and the infrared spectrum (see [reference needed]) shows... Figure 9 An absorption peak representing the carbonyl group (1750 cm⁻¹) also appeared in the sample. -1 These findings indicate the presence of carbonyl groups formed by oxidation within the polyethylene molecule. Studies have shown that the presence of these carbonyl groups facilitates further oxidative degradation of microplastics.
[0034] Comparative Example 1 Synthesis of photocatalyst ptap+: 3 g (20 mmol) of IntB prepared in step (4) of Example 1 and 0.6 g (10 mmol) of lithium scrap were mixed in 50 mL of n-butanol and refluxed for 10 hours under argon protection. After solvent recovery under reduced pressure, the remaining reactants were added to 100 mL of 0.1 M hydrochloric acid and stirred at 60 °C for 2 hours. The solid product was filtered out, washed with water, neutralized and dried to obtain 2.0 g (about 3.5 mmol) of crude tetratert-butyltetraazaporphyrin (tap). 2.0 g of tap was dissolved in 50 mL of pyridine and heated to 80 °C under argon protection. 0.73 g (2.5 mmol) was added dropwise. POBr3 (pre-dissolved in 5 mL of pyridine) was added dropwise and heated for 4 hours. After the reaction was complete, the remaining POBr3 was destroyed with 1 M sodium carbonate solution until no more bubbles were produced. The solvent was recovered by evaporation under reduced pressure. The crude product was purified on a silica gel column using pyridine and toluene (volume ratio 6:4) as the developing solvent to obtain 1.20 g (approximately 2 mmol) of tetratert-butyltetraazaphosphorphyrin (ptap). The obtained ptap was then dissolved in 5 mL of acetonitrile with 0.9 g (5 mmol) of 1-chlorododecane. 0.5 g (3.5 mmol) of K2CO3 was added and heated to 80 °C under argon protection for 4 hours. After the reaction was complete, K2CO3 was removed by filtration, and acetonitrile was recovered under reduced pressure. The crude product was purified by recrystallization from ethanol and toluene (volume ratio 1:1) to obtain 1.0 g of photocatalyst ptap+, whose molecular structure is shown in formula (II). Compared with ptambp+ of the present invention, it lacks two quaternary ammonium salt groups and two long-chain alkyl groups.
[0035]
[0036] Formula (II)
[0037] Characterization of ptap+: MALDI-TOF-MS: cal. m / z: 937.69 (100.0%), 938.70 (61.7%), 939.70 (19.1%), found 937.70 (100%), 938.70 (62%), 939.71 (19.5%), singlet oxygen quantum yield 0.51 (aqueous dispersion).
[0038] The ptambp prepared in step (6) of Example 1 and the ptap+ prepared in Comparative Example 1 were subjected to photocatalytic degradation experiments according to the test method of Example 3. Water-soluble zinc tetrasulfonate phthalocyanine (ZnPcS4) was used as a control. The results are shown in Table 1: Table 1
[0039] The comparison shows that the degradation efficiency of ptambp for microplastics (15%) is only 1 / 4 that of ptambp+ after quaternization (55%). This indicates the importance of the four dodecyl long chains added in step (7) of Example 1 for the photocatalytic degradation efficiency of microplastics, given the consistent tetraazabenzylphosphorphyrin structure. The molecular configuration of ptambp+ (see...) Figure 1 It exhibits a conical structure, with four dodecyl chains forming a spatial configuration resembling four interlaced hooks. The positively charged quaternary ammonium salt is located at the edge, exposed to the opposite direction of the alkyl chains, thus forming two centers: a hydrophilic center and a lipophilic center. The alkyl chains can effectively interact with the microplastics, while the hydrophilic quaternary ammonium groups ensure that the molecules can be uniformly dispersed in aqueous solution to form micelles. These micelles transfer dissolved oxygen molecules from the water to generate singlet oxygen through photocatalysis, thereby achieving the oxidative degradation of the adsorbed microplastics.
[0040] The water-soluble zinc sulfonate phthalocyanine, lacking effective contact with microplastics, exhibits limited degradation efficiency (4%) despite a good singlet oxygen quantum yield in aqueous solution. While unsubstituted quaternary ammonium groups (ptap+) exhibit stronger lipophilicity, their degradation efficiency for microplastics is only 9%. This may be because the positive ions formed by the substitution of two quaternary ammonium salts enhance the hydrophilicity of the ptambp+ molecule, playing a crucial role in the formation of stable micelles in aqueous solution. Furthermore, the interaction between ptambp+ with four long-chain alkyl groups and microplastics is significantly stronger than that with two long-chain alkyl groups (ptap+).
[0041] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the present invention in any way. Other variations and modifications may be made without departing from the technical solutions described in the claims.
Claims
1. A photocatalyst for degrading microplastic pollutants, characterized in that: Its general molecular structure is shown in formula (Ⅰ): Equation (I) In formula (Ⅰ), R1 is selected from C1~C3 straight-chain alkyl groups; R2 is selected from tert-butyl, phenyl, or p-tert-butylphenyl; R3 is selected from a straight-chain alkyl group of C12, C16 or C18.
2. A method for preparing a photocatalyst for degrading microplastic pollutants as described in claim 1, characterized in that, Includes the following steps: (1) 4,5-Dimethylphthalonitrile undergoes a free radical substitution reaction with a brominating reagent in toluene solution under the initiator to generate 4,5-dibromomethylphthalonitrile, named Pn1; (2) Compound Pn1 was subjected to a cyclization reaction with di(N-alkyl)ethylenediamine under alkaline conditions and in an aprotic solvent to generate a dinitrile compound with a tetrahydropyrazine structure, which was named Pn2; (3) Compound Pn2 was subjected to an amination reaction with an amination reagent in n-butanol solution under the catalysis of a strong base catalyst to obtain an intermediate with an iminoisoindoline structure, named IntA; (4) The compound with the butenedionitrile structure was subjected to an amination reaction with an amination reagent in an ethanol solution to obtain an intermediate with a diimine pyrrole structure, named IntB; (5) Intermediate IntA and intermediate IntB are mixed in n-butanol solution, and lithium metal is added to carry out cyclization condensation reaction to generate porphyrin dilithium with tetraazamonobenzoporphyrin structure. Then, acid is added to carry out hydrolysis reaction to remove lithium ions, and tetraazamonobenzoporphyrin compound is obtained and named tambp. (6) The compound tambp was reacted with phosphorus tribromooxy in pyridine solution to obtain a phosporphyrin compound, named ptambp; (7) The compound ptambp was reacted with 1-chloro-straight-chain alkanes in acetonitrile solution under the catalysis of an alkaline catalyst to obtain the target product photocatalyst.
3. The preparation method according to claim 2, characterized in that: The brominating reagent in step (1) is selected from NBS, DBH or liquid bromine; the initiator is selected from AIBN, AIBME or BPO; the molar ratio between 4,5-dimethylphthalonitrile, brominating reagent and initiator is 1:(1~1.5):(0.04~0.1); the mass-volume ratio of 4,5-dimethylphthalonitrile to toluene is (1~2) g:20 mL; the reaction temperature is 75~85℃; and the reaction time is 2~4 h.
4. The preparation method according to claim 2, characterized in that: In step (2), the molar ratio of compound Pn1 to di(N-alkyl)ethylenediamine is 5:(5.5~6), and the mass-to-volume ratio of compound Pn1 to the aprotic solvent is (1~2) g:10 mL; the aprotic solvent is selected from DMF or DMSO; the alkyl group in the di(N-alkyl)ethylenediamine is selected from methyl, ethyl or n-propyl; the alkaline conditions are adjusted to pH=9.5~10.5 using K2CO3 or Na2CO3; the cyclization reaction temperature is the reflux temperature, and the reaction time is 1~5 h.
5. The preparation method according to claim 2, characterized in that: In step (3), the molar ratio of compound Pn2 to strong base catalyst and amination reagent is 3:(0.1~0.3):(6-9), the mass-volume ratio of compound Pn2 to n-butanol is (6~7) g:100mL, the strong base catalyst is selected from sodium methoxide, sodium ethoxide or lithium isopropoxide, the amination reagent is selected from ammonia, ammonium acetate or urea, the amination reaction temperature is reflux temperature, and the reaction time is 4~6h.
6. The preparation method according to claim 2, characterized in that: In step (4), the molar ratio of the compound with the butenedionitrile structure to the amination reagent is 1:(1~2), the mass-volume ratio of the compound with the butenedionitrile structure to ethanol is (2~3) g:30 mL, the compound with the butenedionitrile structure is selected from cis-2-tert-butyl,2-butenedionitrile, cis-2-phenyl,2-butenedionitrile or cis-2-p-tert-butyl-phenyl,2-butenedionitrile, the amination reagent is ammonium acetate, the amination reaction temperature is the reflux temperature, and the reaction time is 7~10 h.
7. The preparation method according to claim 2, characterized in that: In step (5), the molar ratio of intermediate IntA, intermediate IntB and lithium metal is 1:3:(1~3), the mass-volume ratio of intermediate IntA to n-butanol is (4~5) g:150 mL, the mass-volume ratio of intermediate IntA to acid is (4~5) g:250 mL, the acid is 0.1 M HCl, the cyclization condensation reaction temperature is reflux temperature, the reaction time is 10~12 h, the hydrolysis reaction temperature is 60~80 °C, and the reaction time is 0.5~2 h.
8. The preparation method according to claim 2, characterized in that: In step (6), the molar ratio of compound tambp to phosphorus tribromooxy is 1:(1~1.2), the mass-volume ratio of compound tambp to pyridine solution is (6~7) g:125 mL, the reaction temperature is 60~80℃, and the reaction time is 4~6 h.
9. The preparation method according to claim 2, characterized in that: In step (7), the molar ratio of compound ptambp to 1-chloro linear alkane and basic catalyst is 1:(4~6):(1~2). The 1-chloro linear alkane is selected from 1-chlorododecane, 1-chlorohexadecane or 1-chlorooctadecane. The basic catalyst is selected from K2CO3 or Na2CO3. The reaction temperature is 60~80℃ and the reaction time is 8~12h.
10. The application of the photocatalyst according to claim 1 in the photocatalytic oxidative degradation of microplastics, characterized in that: The photocatalyst adsorbs microplastics in an aqueous phase using hydrophobic straight-chain alkyl groups and maintains the aqueous phase dispersion with hydrophilic quaternary ammonium salt groups to form micelles, thereby achieving photocatalytic degradation of microplastics; the microplastics are selected from one or more of polyethylene, polyvinyl chloride, and polystyrene.