A method for separating weathered graphite ore
By combining grinding and multiple fine-tuning with a composite collector, the problem of mineralization failure in the flotation process of weathered graphite ore was solved, achieving efficient recovery and production of high-purity graphite concentrate.
Patent Information
- Application Number
- CN202611516538.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Weathered graphite is prone to mineralization failure during flotation, resulting in low graphite recovery. Existing grinding processes easily damage the large flake structure, affecting process efficiency.
A method combining grinding, multiple beneficiation, and grinding with a composite collector, including a combination of kerosene, aniline, n-octylbenzene, sodium alkyl sulfonate, and 80 Tween, was adopted to optimize the compatibility and point-by-point addition of the reagents, thereby improving the hydrophobicity and collecting ability of graphite.
It improved the recovery rate of weathered graphite ore and the fixed carbon content of concentrate, reduced the amount of reagents used, enhanced the beneficiation effect, and improved resource utilization efficiency.
Smart Images

Figure CN123102497A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of mineral flotation, and more particularly to a method for separating weathered graphite ore. Background Technology
[0002] Weathered graphite deposits are formed on the surface of graphite mines. They are a type of graphite resource formed by the weathering and oxidation of primary graphite ore over many years.
[0003] After primary graphite ore is weathered, the original reducing minerals and hydrous minerals in the ore undergo chemical transformation, the structure of the weathered graphite resource itself is destroyed, the degree of graphitization is reduced, and the shear strength is significantly reduced. In addition, the weathering process leads to the mixing of clay minerals and fine-grained gangue minerals (such as quartz and pyrite) into the graphite ore, forming a large amount of sludge.
[0004] Although weathered graphite ore is easy to crush and has low grinding difficulty, its poor crystallinity, high degree of graphite oxidation, fine gangue minerals, and large specific surface area make it prone to "mineralization failure" during flotation. A large amount of graphite will gradually return to the previous flotation / regrinding process, affecting the process efficiency. Furthermore, the existing grinding technology is prone to excessive flake crushing, which destroys the large flake structure.
[0005] Therefore, there is an urgent need to provide a separation method suitable for weathered graphite ore to solve the above problems. Summary of the Invention
[0006] The purpose of this application is to provide a method for separating weathered graphite ore to solve the above-mentioned problems.
[0007] To achieve the above objectives, this application provides a method for separating weathered graphite ore, comprising: The weathered graphite ore is mixed with water and then ground to obtain a graphite slurry; The graphite slurry, collector aid, composite collector, and frother are mixed and roughed to obtain rough concentrate and rough concentrate. The roughing concentrate undergoes a first classification to obtain a first underflow and a first overflow. The first underflow is then ground to obtain a ground first underflow. The ground first underflow is then mixed with the first overflow to obtain a liberated roughing concentrate. The dissociated crude concentrate and the composite collector are mixed and subjected to multiple fine selections and grinding processes to obtain graphite concentrate; The raw materials of the composite collector, based on a total mass of 100%, include: kerosene 80%-90%, aniline 1%-3%, n-octylbenzene 1%-3%, sodium alkyl sulfonate 2%-7%, and 80 Tween 2%-7%.
[0008] Optionally, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The mass ratio of the weathered graphite ore to the water is 0.25-0.35:1; B. The graphite slurry contains 40%-70% material with a fineness of -100 mesh.
[0009] Optionally, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The catalytic agent includes 2-octanol and / or methyl isobutyl methanol; B. The foaming agent comprises 2-octanol and methyl isobutyl methanol, wherein the mass ratio of 2-octanol to methyl isobutyl methanol is 1:1-5; C. In the roughing process, the mass of the collector aid is 0.1 kg / t raw ore to 1 kg / t raw ore, the mass of the composite collector is 0.1 kg / t raw ore to 1 kg / t raw ore, and the mass of the frother is 0.1 kg / t raw ore to 0.5 kg / t raw ore.
[0010] Optionally, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The material with a fineness of -100 mesh accounts for 60%-80% of the first overflow; B. The material with a fineness of -100 mesh accounts for 60%-80% of the dissociated crude concentrate.
[0011] Optionally, the number of times the selection is repeated is 7 to 11. The grinding process is repeated 6 to 10 times.
[0012] Optionally, the multiple cleaning and grinding processes include 8-stage cleaning and 7-stage grinding performed sequentially and alternately; the middlings from the first 4 stages of cleaning are mixed, dehydrated, and ground to obtain mixed middlings; the mixed middlings, the composite collector, and the frother are mixed and scavenged to obtain middlings concentrate; the middlings concentrate is returned to the second stage of cleaning for further processing; and the middlings from the last 4 stages of cleaning are returned to the previous stage in sequence.
[0013] Optionally, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. In the multi-stage beneficiation process, the mass of the composite collector added to each stage of beneficiation is independently 0.01 kg / t raw ore to 0.05 kg / t raw ore; B. During the fifth-stage beneficiation, the frother is also added, and the dosage of the frother is 0.01 kg / t raw ore to 0.05 kg / t raw ore; C. In the process of selecting and scavenging the middlings ore, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore; the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore.
[0014] Optionally, the roughing concentrate is subjected to a second classification to obtain a second underflow and a second overflow. The second underflow is ground to obtain a post-grinding second underflow. The post-grinding second underflow is mixed with the second overflow and subjected to scavenging to obtain scavenging concentrate and scavenging tailings. The scavenging concentrate is returned to the roughing process.
[0015] Optionally, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. During the scavenging process, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore, and the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore; B. In the second underflow, materials with a fineness of -200 mesh account for 50%-60%.
[0016] Optionally, the graphite concentrate has a fixed carbon content of ≥93% and a particle size of +100 mesh of ≥10%.
[0017] Compared with the prior art, the beneficial effects of this application include: The separation method for weathered graphite ore provided in this application, through process optimization, reagent compatibility and point-by-point addition of reagents, achieves the reduction of flotation concentrate concentration, enhances reagent selectivity and action, ensures the hydrophobicity of weakly crystalline weathered graphite minerals in long-process beneficiation, realizes efficient separation of weathered graphite ore, and effectively improves the utilization efficiency of weathered graphite resources. Attached Figure Description
[0018] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of this application and should not be regarded as a limitation on the scope of this application.
[0019] Figure 1 This is a schematic flowchart of the separation method for weathered graphite ore provided in Example 1. Detailed Implementation
[0020] As used in this article: "Prepared from" is synonymous with "comprising". The terms "comprising", "including", "having", "containing", or any other variations thereof as used herein are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.
[0021] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1–5” is disclosed, the described range should be interpreted as including ranges “1–4”, “1–3”, “1–2”, “1–2 and 4–5”, “1–3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.
[0022] In these embodiments, unless otherwise specified, the portions and percentages are all by weight.
[0023] "Parts by mass" refers to the basic unit of measurement that expresses the mass ratio of multiple components. One part can represent any unit mass, such as 1g or 2.689g. If we say that component A has "a" parts by mass and component B has "b" parts by mass, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it can mean that the mass of component A is aK and the mass of component B is bK (where K is any number representing a multiplier). It is important to understand that, unlike parts by mass, the sum of the mass parts of all components is not limited to 100 parts.
[0024] "And / or" is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0025] It is important to note that after primary graphite ore is weathered, the original reducing and hydrous minerals in the ore undergo chemical transformations (specifically, oxidation reactions of reducing minerals). For example, sulfides such as pyrite / pyrrhotite transform into limonite, muscovite transforms into biotite, and the clay mineral content increases. Therefore, the first characteristic of weathered graphite ore is its large specific surface area, high oxygen-containing functional groups on the surface, and small mineral particle size. In addition, primary graphite ore also undergoes a certain degree of oxidation under weathering conditions, with oxygen-containing functional groups replacing the clean carbon-containing surface of the graphite, which can enhance the hydrophilicity of weathered graphite ore. At the same time, the structure of weathered graphite ore itself is damaged, the degree of graphitization decreases, and the shear strength is significantly reduced, which manifests as reduced difficulty in crushing and grinding, and reduced difficulty in the dissociation of large flakes.
[0026] Based on the aforementioned characteristics of weathered graphite ore, this application proposes a method for separating weathered graphite ore, comprising: The weathered graphite ore is mixed with water and then ground to obtain a graphite slurry; The graphite slurry, collector aid, composite collector, and frother are mixed and roughed to obtain rough concentrate and rough concentrate. The roughing concentrate undergoes a first classification to obtain a first underflow and a first overflow. The first underflow is then ground to obtain a ground first underflow. The ground first underflow is then mixed with the first overflow to obtain a liberated roughing concentrate. It is important to note that the first grading is the most efficient grading process for the raw ore, and the resulting first-grade concentrate forms the basis for subsequent concentrate grading.
[0027] The dissociated crude concentrate and the composite collector are mixed and subjected to multiple cleaning and grinding processes to obtain graphite concentrate. It should be noted that multiple rounds of selection and grinding will increase the carbon content and particle size, resulting in graphite concentrate with a higher carbon content, which lays the foundation for subsequent purification work. The raw materials of the composite collector, based on a total mass of 100%, include: kerosene 80%-90%, aniline 1%-3%, n-octylbenzene 1%-3%, sodium alkyl sulfonate 2%-7%, and 80 Tween 2%-7%.
[0028] Optionally, the raw materials of the composite collector, based on a total mass of 100%, may include kerosene at any value between 80%, 85%, 90%, or 80%-90%, aniline at any value between 1%, 2%, 3%, or 1%-3%, n-octylbenzene at any value between 1%, 2%, 3%, or 1%-3%, sodium alkyl sulfonate at any value between 2%, 3%, 4%, 5%, 6%, 7%, or 2%-7%, and 80 Tween at any value between 2%, 3%, 4%, 5%, 6%, 7%, or 2%-7%.
[0029] It is important to note that weathered graphite ore itself contains a large number of oxygen-containing functional groups, resulting in poor hydrophobicity. Optimizing the composition of the composite collector enhances its dispersion ability in the slurry. Simultaneously, based on the SP2 hybridization characteristics of the six-membered rings in graphite interlayers, the composite collector promotes the formation of interlayer π bonds with the six-membered rings. These two aspects improve the collector's ability to collect graphite and enhance the hydrophobicity of weathered graphite minerals. Addressing the characteristics of weathered graphite ore—high weathering degree, large proportion of fine particles, and severe slime covering—the surfactant component in the composite collector promotes the emulsification and dispersion of hydrocarbon oils in the slurry, forming micro-oil droplets to improve the collision and adhesion efficiency with fine-grained graphite. Simultaneously, the aromatic ring-containing organic molecules undergo π-π stacking interactions with the delocalized π electron clouds on the graphite six-membered rings, forming stable interlayer π bonds and enhancing the adsorption strength of the composite collector on the graphite surface. Compared with single kerosene collectors, composite collectors can achieve a fixed carbon content of over 90% in the concentrate and a recovery rate of 5-10 percentage points with a 20% to 30% reduction in reagent dosage, effectively overcoming the interference of weathered slime on the flotation process.
[0030] In some embodiments, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The mass ratio of the weathered graphite ore to the water is 0.25-0.35:1; Optionally, the mass ratio of weathered graphite ore to water can be 0.25:1, 0.3:1, 0.35:1, or any value between 0.25 and 0.35:1; B. The graphite slurry contains 40%-70% material with a fineness of -100 mesh.
[0031] Optionally, the material with a fineness of -100 mesh in the graphite slurry can account for any value between 40%, 50%, 60%, 70%, or 40%-70%.
[0032] In some embodiments, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The catalytic agent includes 2-octanol and / or methyl isobutyl methanol; It should be noted that trapping aids are agents that improve the efficiency of compound trapping agents, and can significantly reduce the amount of compound trapping agents used while increasing the harvesting efficiency. B. The foaming agent comprises 2-octanol and methyl isobutyl methanol, wherein the mass ratio of 2-octanol to methyl isobutyl methanol is 1:1-5; Optionally, the mass ratio of 2-octanol to methyl isobutyl methanol can be any value between 1:1, 1:2, 1:3, 1:4, 1:5, or 1:1-5; C. In the roughing process, the mass of the collector is 0.1 kg / t raw ore to 1 kg / t raw ore, the mass of the composite collector is 0.1 kg / t raw ore to 1 kg / t raw ore, and the mass of the frother is 0.1 kg / t raw ore to 0.5 kg / t raw ore.
[0033] Optionally, the mass of the collector aid can be any value between 0.1 kg / t raw ore, 0.5 kg / t raw ore, 1 kg / t raw ore, or 0.1 kg / t raw ore and 1 kg / t raw ore; the mass of the compound collector can be any value between 0.1 kg / t raw ore, 0.3 kg / t raw ore, 0.5 kg / t raw ore, 1 kg / t raw ore, or 0.1 kg / t raw ore and 1 kg / t raw ore; and the mass of the frother can be any value between 0.15 kg / t raw ore, 0.3 kg / t raw ore, 0.5 kg / t raw ore, or 0.1 kg / t raw ore and 0.5 kg / t raw ore.
[0034] In some embodiments, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. The material with a fineness of -100 mesh accounts for 60%-80% of the first overflow; Optionally, the material with a fineness of -100 mesh in the first overflow can account for any value between 60%, 70%, 80%, or 60%-80%; B. The material with a fineness of -100 mesh accounts for 60%-80% of the dissociated crude concentrate.
[0035] Optionally, the material with a fineness of -100 mesh in the liberated concentrate can account for any value between 60%, 70%, 80%, or 60%-80%.
[0036] In some embodiments, the number of times the multi-level selection is performed is 7 to 11. Optionally, the number of selection levels can be 7, 8, 9, 10, or 11. The grinding process is repeated 6 to 10 times.
[0037] Optionally, the number of grinding stages can be 6, 7, 8, 9, or 10.
[0038] In some embodiments, the multiple cleaning and multiple grinding processes include sequentially alternating 8-stage cleaning and 7-stage grinding; the middlings from the first 4 stages of cleaning are mixed, dehydrated, and ground to obtain mixed middlings; the mixed middlings, the composite collector, and the frother are mixed and scavenged to obtain middlings concentrate; the middlings concentrate is returned to the second stage of cleaning for further processing; and the middlings from the last 4 stages of cleaning are returned sequentially to the previous stage.
[0039] It should be noted that due to the poor hydrophobicity of weathered graphite ore, the middlings recycling volume is large during the beneficiation process. For the high and medium concentration of middlings, the middlings from the first four stages of beneficiation are concentrated. Since the middlings in beneficiation are mostly graphite intergrowths, water is pre-classified to improve beneficiation and regrinding efficiency. After the middlings are scavenged, the fixed carbon content in the tailings is significantly reduced, meeting the requirements for direct tailings disposal. A small amount of concentrate is directly returned, greatly improving beneficiation efficiency. In some embodiments, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. In the multi-stage beneficiation process, the mass of the composite collector added to each stage of beneficiation is independently 0.01 kg / t raw ore to 0.05 kg / t raw ore; Optionally, the mass of the compound collector added in each stage of refining can be independently 0.01 kg / t raw ore, 0.02 kg / t raw ore, 0.05 kg / t raw ore, or any value between 0.01 kg / t raw ore and 0.05 kg / t raw ore; B. During the fifth-stage beneficiation, the frother is also added at a dosage of 0.01 kg / t raw ore to 0.05 kg / t raw ore. Optionally, during the fifth-stage beneficiation, the amount of frother can be 0.01 kg / t, 0.02 kg / t, 0.05 kg / t of raw ore, or any value between 0.01 kg / t of raw ore and 0.05 kg / t of raw ore; C. In the process of selecting and scavenging the middlings ore, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore; the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore.
[0040] Optionally, in the middlings ore scavenging process, the mass of the compound collector can be any value between 0.05 kg / t raw ore, 0.1 kg / t raw ore, 0.2 kg / t raw ore, 0.3 kg / t raw ore, 0.4 kg / t raw ore, 0.5 kg / t raw ore, or 0.05 kg / t raw ore - 0.5 kg / t raw ore, and the frother can be any value between 0.05 kg / t raw ore, 0.1 kg / t raw ore, 0.2 kg / t raw ore, 0.25 kg / t raw ore, or 0.05 kg / t raw ore - 0.25 kg / t raw ore.
[0041] In some embodiments, the roughing concentrate is subjected to a second classification to obtain a second underflow and a second overflow. The second underflow is ground to obtain a post-grinding second underflow. The post-grinding second underflow is mixed with the second overflow and subjected to scavenging to obtain scavenging concentrate and scavenging tailings. The scavenging concentrate is returned to the roughing process.
[0042] In some embodiments, the method for separating weathered graphite ore satisfies at least one of the following conditions: A. During the scavenging process, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore, and the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore; Optionally, during the scavenging process, the mass of the compound collector can be any value between 0.05 kg / t raw ore, 0.3 kg / t raw ore, 0.5 kg / t raw ore, or 0.05 kg / t raw ore and 0.5 kg / t raw ore, and the mass of the frother can be any value between 0.05 kg / t raw ore, 0.2 kg / t raw ore, 0.25 kg / t raw ore, or 0.05 kg / t raw ore and 0.25 kg / t raw ore. B. In the second underflow, materials with a fineness of -200 mesh account for 50%-60%.
[0043] Optionally, the material with a fineness of -200 mesh in the second underflow can account for any value between 50%, 55%, 60%, or 50%-60%.
[0044] In some embodiments, the graphite concentrate has a fixed carbon content of ≥93% and a particle size of +100 mesh of ≥10%.
[0045] In some embodiments, the graphite concentrate has a fixed carbon content of 93.15% and a particle size of +100 mesh accounting for ≥10%.
[0046] It should be noted that this application optimizes the reagent ratio, changing the traditional coarse scavenging reagent addition to a co-addition mode of coarse, multi-stage fine, and scavenging. This ensures excellent graphite floatability, prevents over-grinding of middlings, and avoids a reduction in the content of large flakes, resulting in good economic efficiency and environmental benefits.
[0047] The implementation schemes of this application will be described in detail below with reference to specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating this application and should not be regarded as limiting the scope of this application. Unless otherwise specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments used without specified manufacturers are all conventional products that can be purchased commercially.
[0048] Example 1 This embodiment provides a method for separating weathered graphite ore, the specific steps of which are as follows: S1: Weathered graphite ore and water are mixed and ground to obtain graphite slurry, wherein the mass ratio of weathered graphite ore to water is 3:10; S2: Graphite slurry, 0.1 kg / t raw ore of collector aid (2-octanol), 0.2 kg / t raw ore of composite collector, and 0.1 kg / t raw ore of composite frother are mixed and roughed to obtain graphite rough concentrate and rough concentrate. S3: The graphite roughing concentrate is pre-classified to obtain underflow and overflow. The overflow contains 65% material with a fineness of -100 mesh. The underflow is regrinded and mixed with the overflow to obtain a liberated rough concentrate with 70% material of -100 mesh. S4: The liberated rough concentrate and the composite collector are mixed and subjected to 8 cleaning cycles and 7 regrinding cycles respectively. In addition, 0.02 kg / t of composite frother is added during the fifth cleaning cycle. The final graphite concentrate and flotation ore 1-8 are obtained. The amount of composite collector added in each of the 8 cleaning cycles is 0.02 kg / t of raw ore. The end point of each of the 7 regrinding cycles is: with the proportion of +100 mesh (+0.150 mm) as a reference, the fineness after grinding is ≤95% of the fineness before grinding, and the next regrinding cycle can be started or the process can be ended. S5: Mix the middlings from flotation stages 1-4, dewater them using a hydrocyclone, regrind them, add a composite collector and a composite frother for middlings scavenging, and obtain middlings scavenging concentrate and middlings scavenging tailings. The middlings scavenging concentrate is returned for the second stage of cleaning. S6: Return the ore from the 5th to 8th stages of flotation to the previous stage of operation; S7: The roughing tailings are classified to obtain underflow and overflow. 55% of the material in the underflow has a fineness of -200 mesh. After grinding, the underflow and overflow are mixed and then scavenged. 0.1 kg / t of composite collector and 0.05 kg / t of composite frother from the raw ore are added to the overflow for scavenging to obtain scavenged concentrate and scavenged tailings. The scavenged concentrate is returned to the roughing stage. The flow chart of this separation method for weathered graphite ore is as follows: Figure 1 As shown.
[0049] The raw materials of the composite collector, based on a total mass of 100%, include: kerosene 87%, aniline 1%, n-octylbenzene 3%, sodium alkyl sulfonate 7%, and 80 Tween 2%. The composite foaming agent is octanol and methyl isobutyl methanol in a mass ratio of 1:1.5.
[0050] Example 2 The difference from Example 1 is that the raw materials of the composite collector, based on a total mass of 100%, include: kerosene 85%, aniline 3%, n-octylbenzene 3%, sodium alkyl sulfonate 7%, and 80 Tween 2%.
[0051] Example 3 The difference from Example 1 is that the composite foaming agent is octanol and methyl isobutyl methanol in a mass ratio of 1:2.
[0052] Comparative Example 1 The difference from Example 1 is that the pre-grading step S3 is not performed.
[0053] Comparative Example 2 The difference from Example 1 is that aniline is not added to the composite collector.
[0054] Comparative Example 3 The difference from Example 1 is that 80 Tween is not added to the composite collector.
[0055] Comparative Example 4 The difference from Example 1 is that no trapping agent is added in step S2.
[0056] Comparative Example 5 The difference from Example 1 is that in the S4 step of fine selection, only 8 fine selections are performed, and no regrinding is performed.
[0057] Comparative Example 6 The difference from Example 1 is that in the S4 step of fine selection, only 4 fine selections and 3 re-grindings are performed.
[0058] Comparative Example 7 The difference from Example 1 is that in step S5, the ore from flotation of stages 1-4 is directly returned to the previous stage of operation.
[0059] The results of the eight selections in Example 1 are shown in Table 1.
[0060] Table 1. Results of 8 selections in Example 1
[0061] The recovery rate, fixed carbon content, and particle size of the final products of the separation methods for weathered graphite ore provided in the above embodiments and comparative examples were tested, and the specific results are shown in Table 2.
[0062] Table 2. Test results for the examples and comparative examples.
[0063] analyze: The data above shows that after multiple grinding and beneficiation processes, the fixed carbon content of the concentrate is significantly increased, and the particle size also changes accordingly. The purity of graphite is significantly improved after multiple grinding and beneficiation processes.
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and are not intended to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application.
[0065] Furthermore, those skilled in the art will understand that although some embodiments herein include certain features included in other embodiments but not others, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the foregoing claims, any of the claimed embodiments can be used in any combination. The information disclosed in this background section is intended only to enhance the understanding of the general background of this application and should not be construed as an admission or in any way implying that such information constitutes prior art known to those skilled in the art.
Claims
1. A method for separating weathered graphite ore, characterized in that, include: The weathered graphite ore is mixed with water and then ground to obtain a graphite slurry; The graphite slurry, collector aid, composite collector, and frother are mixed and roughed to obtain rough concentrate and rough concentrate. The roughing concentrate undergoes a first classification to obtain a first underflow and a first overflow. The first underflow is then ground to obtain a ground first underflow. The ground first underflow is then mixed with the first overflow to obtain a liberated roughing concentrate. The dissociated crude concentrate and the composite collector are mixed and subjected to multiple cleaning and grinding processes to obtain graphite concentrate. The raw materials of the composite collector, based on a total mass of 100%, include: kerosene 80%-90%, aniline 1%-3%, n-octylbenzene 1%-3%, sodium alkyl sulfonate 2%-7%, and 80 Tween 2%-7%.
2. The method for separating weathered graphite ore according to claim 1, characterized in that, At least one of the following conditions must be met: A. The mass ratio of the weathered graphite ore to the water is 0.25-0.35:1; B. The graphite slurry contains 40%-70% material with a fineness of -100 mesh.
3. The method for separating weathered graphite ore according to claim 1, characterized in that, At least one of the following conditions must be met: A. The catalytic agent includes 2-octanol and / or methyl isobutyl alcohol; B. The foaming agent comprises 2-octanol and methyl isobutyl alcohol, wherein the mass ratio of 2-octanol to methyl isobutyl alcohol is 1:1-5; C. In the roughing process, the mass of the collector is 0.1 kg / t raw ore to 1 kg / t raw ore, the mass of the composite collector is 0.1 kg / t raw ore to 1 kg / t raw ore, and the mass of the frother is 0.1 kg / t raw ore to 0.5 kg / t raw ore.
4. The method for separating weathered graphite ore according to claim 1, characterized in that, At least one of the following conditions must be met: A. The material with a fineness of -100 mesh accounts for 60%-80% of the first overflow; B. The material with a fineness of -100 mesh accounts for 60%-80% of the dissociated crude concentrate.
5. The method for separating weathered graphite ore according to claim 1, characterized in that, The number of times the selection is made is 7-11. The grinding process is repeated 6 to 10 times.
6. The method for separating weathered graphite ore according to claim 5, characterized in that, The multiple refining and grinding processes include 8-stage refining and 7-stage grinding performed sequentially and alternately. The middlings from the first 4 stages of refining are mixed, dehydrated, and ground to obtain mixed middlings. The mixed middlings, the composite collector, and the frother are mixed and scavenged to obtain middlings concentrate. The middlings concentrate is returned to the second stage of refining for further processing. The middlings from the last 4 stages of refining are returned to the previous stage in sequence.
7. The method for separating weathered graphite ore according to claim 6, characterized in that, At least one of the following conditions must be met: A. In the multi-stage beneficiation process, the mass of the composite collector added to each stage of beneficiation is independently 0.01 kg / t raw ore to 0.05 kg / t raw ore; B. During the fifth-stage beneficiation, the frother is also added, and the amount of the frother is 0.01 kg / t raw ore to 0.05 kg / t raw ore; C. In the process of selecting and scavenging the middlings ore, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore; the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore.
8. The method for separating weathered graphite ore according to claim 1, characterized in that, The roughing concentrate is subjected to a second classification to obtain a second underflow and a second overflow. The second underflow is ground to obtain a post-grinding second underflow. The post-grinding second underflow is mixed with the second overflow and subjected to scavenging to obtain scavenging concentrate and scavenging tailings. The scavenging concentrate is returned to the roughing process.
9. The method for separating weathered graphite ore according to claim 8, characterized in that, At least one of the following conditions must be met: A. During the scavenging process, the mass of the composite collector is 0.05 kg / t raw ore to 0.5 kg / t raw ore, and the mass of the frother is 0.05 kg / t raw ore to 0.25 kg / t raw ore; B. In the second underflow, materials with a fineness of -200 mesh account for 50%-60%.
10. The method for separating weathered graphite ore according to any one of claims 1-9, characterized in that, The graphite concentrate has a fixed carbon content of ≥93% and a particle size of +100 mesh of ≥10%.