A method for synergistic treatment of valuable metal enrichment and heavy metal stabilization and solidification in tungsten slag
By synergistic activation of sodium carbonate-calcium iron components and weak alkali selective leaching, combined with gravity-magnetic levitation enrichment and iron-phosphorus-slag cement composite solidification, the problems of low tungsten and molybdenum leaching rates and heavy metal migration in tungsten slag treatment are solved, achieving efficient recovery of valuable metals and stable solidification of heavy metals. It is suitable for applications such as mine backfilling and road base materials.
Patent Information
- Application Number
- CN202611605964.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing tungsten slag treatment processes suffer from problems such as low tungsten and molybdenum leaching rates, difficulty in segmented enrichment of tin, copper, zinc, and lead, easy migration of heavy metals during acid and alkali leaching, high consumption of solidification agents in tailings, and large amounts of wastewater. These processes cannot achieve the synergistic treatment of valuable metal recovery and stable solidification of heavy metals.
By employing a method of synergistic activation of sodium carbonate-calcium iron components, weak alkali selective leaching, combined gravity and magnetic levitation enrichment, and iron-phosphorus-slag cement composite solidification, valuable metals are efficiently recovered and heavy metals are stably solidified through mineral phase activation roasting, selective alkali leaching, and multi-metal stepwise separation.
It significantly improves the leaching rate of tungsten and molybdenum, realizes multi-metal cascade recovery, reduces the consumption of solidification agents, reduces wastewater generation, and the prepared solidified body has good mechanical properties, making it suitable for mine filling, road base materials, and non-fired building materials.
Smart Images

Figure CN123102709A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization and harmless treatment technology, and more specifically, relates to a method for the synergistic treatment of valuable metal enrichment and heavy metal stabilization and solidification in tungsten slag. Background Technology
[0002] Tungsten, as a key strategic metal, is widely used in cemented carbide, special steel, electronics, military, and high-temperature wear-resistant materials. my country ranks among the world's top countries in tungsten resource reserves and smelting and processing capacity. Tungsten smelting processes, including alkaline leaching, acid leaching, purification and crystallization, and secondary resource recovery, generate a large amount of alkaline leaching residue, purification residue, and filter press residue, collectively known as tungsten slag.
[0003] Tungsten slag is characterized by large output, diverse sources, and significant fluctuations in composition. The slag not only contains valuable metal components such as tungsten, molybdenum, tin, copper, zinc, lead, iron, and manganese that have not been fully recovered, which have extremely high secondary resource utilization value, but also contains toxic environmental factors such as arsenic, cadmium, chromium, nickel, and fluorine, posing significant environmental risks.
[0004] Currently, the industry primarily treats tungsten slag by either recovering only valuable metals or by solidifying and landfilling, resulting in significant technological shortcomings. Traditional acid and alkali leaching processes suffer from poor selectivity, leading to secondary leaching of heavy metals, high reagent consumption, severe equipment corrosion, and significant secondary pollution. Conventional roasting processes focus solely on increasing tungsten and molybdenum leaching rates without simultaneously managing the risk of heavy metal migration. Traditional solidification technologies often treat tungsten slag as an inert filler, neglecting changes in the activity of smelting tailings, resulting in insufficient compressive strength of the solidified body, susceptibility to cracking and efflorescence, and poor stability of heavy metals. Furthermore, existing processes operate in isolation, lacking integrated design for material and water circulation, leading to low water resource utilization, high disposal costs, and an inability to achieve a synergistic balance between the resource utilization of tungsten slag and the harmless and stable treatment of heavy metals.
[0005] Therefore, there is an urgent need to develop a method for the synergistic treatment of valuable metal enrichment and heavy metal stabilization and solidification in tungsten slag. Summary of the Invention
[0006] The purpose of this invention is to provide a method for the synergistic treatment of valuable metal enrichment and heavy metal stabilization and solidification in tungsten slag. This addresses the problems of low tungsten and molybdenum leaching rates, difficulty in segmented enrichment of tin, copper, zinc, and lead, easy migration of heavy metals during acid and alkali leaching, high consumption of solidification agents in tailings, and excessive wastewater in existing tungsten slag treatment processes. This invention utilizes synergistic activation of sodium carbonate and calcium-iron components, weak alkali selective leaching, combined gravity and magnetic levitation enrichment, and iron-phosphorus-slag cement composite solidification to continuously complete valuable metal recovery and pollutant passivation in the same process, while also achieving water recycling.
[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for the synergistic treatment of valuable metal enrichment and heavy metal stabilization and solidification in tungsten slag includes the following steps: S1. Pretreatment of tungsten slag: The tungsten slag is aged for 12-72 hours, crushed to a particle size of <10mm, and the dry basis moisture content is adjusted to 6%-12% to obtain pretreated tungsten slag. The purpose of aging is to stabilize the free alkali, sulfite and some reducing substances. If necessary, the moisture content is controlled by spraying with circulating washing liquid to facilitate uniform coating and granulation of subsequent additives.
[0008] S2. Mineral Phase Activation Roasting: Sodium carbonate, calcium components, and iron components are added to the pretreated tungsten slag, mixed and granulated, and then roasted in air at 650–800℃ for 40–100 min to prepare activated roasted sand. Sodium carbonate is used to convert calcium tungstate, iron manganese tungstate, and some glass-encapsulated tungsten into soluble sodium tungstate, while promoting the formation of molybdate from molybdate; the calcium components are used to regulate the silicate mineral phase and capture fluorine, arsenic, and some lead and cadmium; the iron components are used to form iron arsenate, iron chromium spinel, or iron oxide hydroxylate precursor phases.
[0009] S3. Selective Alkaline Leaching: Activated roasted sand is ground to a particle size of -0.074 mm (55%–85%), and then leached with water or circulating leachate using alkaline leaching. During leaching, the SiO2 concentration in the leachate is controlled to be <2.5 g / L and the Al2O3 concentration to be <1.8 g / L. Solid-liquid separation yields a tungsten- and molybdenum-containing leachate and leaching residue. This pH range allows tungstates and molybdates to fully enter the liquid phase while preventing the large-scale dissolution of heavy metals such as Pb, Cd, Cr, and Ni. Controlling the silica and aluminum concentration reduces the filtration resistance caused by colloidal silica and molybdenum.
[0010] S4. Tungsten-Molybdenum Precipitation and Enrichment: Calcium and / or magnesium salts are added to the tungsten-molybdenum-containing leachate to precipitate and recover tungsten and molybdenum. The mother liquor after alkali replenishment and periodic salt removal purification is returned to step S3 as circulating leachate. The periodic salt removal purification is: when the Na+ content in the circulating leachate decreases... + Concentration exceeding 80g / L or When the cumulative concentration exceeds 15 g / L, 10% to 20% of the circulating liquid is drawn out for cooling, crystallization, and salt removal. After salt removal, the clear liquid is replenished with alkali and then returned to the leaching process.
[0011] S5. Tin-copper-lead-zinc stepwise separation: The leaching residue is slurryed to a mass concentration of 25% to 40%, and then subjected to gravity separation, magnetic separation and sulfide flotation in sequence to produce tin-iron mixed concentrate, copper-zinc-lead polymetallic concentrate and tailings, respectively.
[0012] S6. Co-solidification of terminal tailings: Iron salts, phosphates, slag powder, cement, lime and water glass are compounded into the terminal tailings, mixed with water, molded and cured to obtain a heavy metal stable solidified body.
[0013] Preferably, the tungsten slag is a residue generated during tungsten smelting, tungsten ore alkali decomposition, tungstate production, or secondary tungsten resource treatment. The tungsten slag contains 0.20%–3.50% WO3, 0.02%–0.80% Mo, 0.10%–2.00% Sn, 0.03%–1.00% Cu, and 0.05%–1.50% Zn, and contains one or more heavy metals selected from Pb, Cd, As, Cr, and Ni.
[0014] Preferably, in step S2, based on the dry weight of the pretreated tungsten slag, the amount of sodium carbonate added is 1.5%–6.0%, the amount of calcium component (calculated as CaO) is 1.0%–5.0%, and the amount of iron component (calculated as Fe2O3) is 0.5%–3.0%. The calcium component is one or more of calcium oxide, calcium hydroxide, limestone powder, and carbide slag; the iron component is one or more of iron oxide, ferrous sulfate, red mud, and iron tailings powder.
[0015] Preferably, in step S3, the liquid-to-solid ratio of the alkaline leaching is 2.5:1 to 5.5:1, the pH is adjusted by sodium hydroxide, sodium carbonate, or a mixture of the two, the leaching pH is 10.2 to 12.0, the leaching temperature is 60 to 90°C, and the leaching time is 45 to 105 min.
[0016] Preferably, in step S4, the reaction temperature for precipitation is 50–85°C, the pH is 8.5–10.5, and the reaction time is 20–60 min; the total molar ratio of calcium and magnesium to tungsten and molybdenum is 1.05–1.40:1; the calcium salt is selected from calcium chloride, calcium nitrate, or lime milk, and the magnesium salt is selected from magnesium chloride or magnesium oxide slurry; the tungsten precipitation rate is ≥95%, and the molybdenum precipitation rate is ≥88%. After the reaction, insoluble tungstate, molybdate, or their composite precipitate are generated. After filtration and washing, a tungsten-molybdenum enrichment is obtained. The total mass fraction of WO3 and MoO3 in this enrichment is not less than 25%, which can be returned to the main tungsten smelting process or used as a raw material for wet tungsten extraction.
[0017] Preferably, in step S5, the gravity separation equipment is a spiral sluice, a shaking table, or a centrifugal concentrator, and the magnetic induction intensity of the magnetic separation is 0.6 to 1.4 T; the sulfide flotation specifically involves adding 600 to 1500 g / t of sodium sulfide, 60 to 180 g / t of butyl xanthate, and 10 to 45 g / t of No. 2 oil, and controlling the flotation pH to 9.0 to 10.0.
[0018] Preferably, the leaching residue is washed until the conductivity of the filtrate is less than 8 mS / cm before slurry preparation. The leaching residue washing water is used for slurry preparation or to prepare solidification mixing water, and the flotation return water is reused for grinding and flotation after settling.
[0019] Preferably, in step S6, based on the dry weight of the final tailings: 0.5%–2.5% iron salt, 0.8%–4.0% phosphate, 8%–30% slag powder, 6%–18% cement, 2%–8% lime, and 0.5%–3.0% water glass; water-cement ratio 0.35–0.65; curing conditions: temperature 15–35℃, relative humidity ≥85%, curing cycle 7–28 days; the iron salt is selected from ferrous sulfate, ferric sulfate, or ferric chloride; the phosphate is selected from calcium dihydrogen phosphate, sodium dihydrogen phosphate, or diammonium hydrogen phosphate. The iron salt provides Fe. 2+ or Fe 3+ It forms stable iron salts with arsenate, chromate and some sulfide oxidation products; phosphates cause Pb, Cd, Zn and other metals to form low-solubility phosphates; slag powder, cement, lime and water glass together form hydrated calcium silicate (CSH), ettringite (AFt) and aluminosilicate gel, which encapsulate, adsorb and fix heavy metals in the crystal lattice.
[0020] The prepared heavy metal stabilized solidified body internally generates a complex mineral phase of calcium silicate hydrate (CSH), ettringite (AFt), ferric phosphate, lead apatite and carbonate. Through multiple mechanisms such as lattice solidification, chemical precipitation and gel encapsulation, the heavy metal is effectively trapped and stabilized for a long time. The 28-day compressive strength is ≥8MPa, and it can be used for mine filling, road base materials, non-fired block aggregate or cement admixture.
[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: (1) Achieving synergistic coupling between mineral phase activation and in-situ controlled release of heavy metals. This invention employs a sodium carbonate composite calcium-iron component synergistic roasting system, which can effectively break down encapsulated and bound insoluble tungsten and molybdenum minerals, significantly improving tungsten and molybdenum leaching efficiency. Tungsten recovery rate can reach 70.4%–91.4%, and molybdenum recovery rate can reach 63.8%–86.2%. At the same time, through the in-situ confinement effect of calcium-iron mineral phases, heavy metals such as arsenic, lead, cadmium, and chromium are effectively fixed, inhibiting the migration of heavy metals in the liquid phase from the source.
[0022] (2) Excellent leaching selectivity and green, low-consumption process. This invention adopts a mild, weakly alkaline selective leaching system, abandoning the traditional strong acid leaching mode, which can effectively avoid the problem of simultaneous leaching of multiple heavy metals; the whole process adopts a closed-loop circulation of mother liquor and a periodic salt discharge and purification process, which significantly reduces the generation and discharge of high-salt wastewater.
[0023] (3) Multi-metal cascade recovery with high resource utilization rate. This invention adopts a combination of gravity separation, magnetic separation and sulfide flotation cascade separation process to efficiently recover tin-iron mixed concentrate and copper-zinc-lead polymetallic concentrate, based on the mineral characteristics of leaching slag, thereby realizing the comprehensive resource utilization of multi-component valuable resources in tungsten slag.
[0024] (4) Low curing cost and good long-term stability of heavy metals. This invention changes the activity of the silicon, aluminum and calcium phases of the final slag through calcination activation. Compared with the direct curing of the original slag, the amount of cementitious material can be reduced by 15% to 30%. XRD phase analysis confirms that a large number of characteristic phases of CSH, ettringite and lead apatite are generated inside the solidified body, realizing multiple stabilization mechanisms of chemical precipitation, lattice doping and gel encapsulation.
[0025] (5) The cured body has excellent mechanical properties and a wide range of applications. The 28-day compressive strength of the cured body prepared by this invention can reach more than 8.6 MPa, and the heavy metal leaching index meets the national standards. It can be widely used in mine filling, road base construction, preparation of non-fired building materials, cement admixtures and other fields.
[0026] (6) The process is highly continuous and adaptable to industrialization. The process flow of this invention is compact and the parameters are controllable. It can be upgraded based on the mature equipment of existing tungsten smelting enterprises. Water resources are recycled in stages throughout the process, making it suitable for large-scale continuous industrial production. Attached Figure Description
[0027] Figure 1 The image shows the XRD pattern of the solidified tailings from Example 16. Detailed Implementation
[0028] Numerous specific details are set forth in the following description to provide a full understanding of the invention. However, the invention can be practiced in many other ways than those described herein, and similar modifications can be made by those skilled in the art without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. It should be noted that the reagents and other materials used in these embodiments are all commercially available products.
[0030] In the following examples, all percentages of additives are based on the dry weight of tungsten slag or tailings. The tungsten slag used in the examples was obtained from the alkaline decomposition and pressure cooking process of a typical tungsten smelting enterprise in central China. This enterprise uses standard wolframite or scheelite concentrate as raw material and extracts tungsten using a high-pressure alkaline cooking process with sodium hydroxide (NaOH), resulting in tungsten slag. After mixing and fractionation, the main chemical composition (dry basis) of the tungsten slag was determined to be: WO3 1.12%, Mo 0.16%, Sn 0.48%, Cu 0.21%, Zn 0.36%, Pb 860 mg / kg, Cd 18 mg / kg, and As 420 mg / kg. This slag sample exhibits typical characteristics of high arsenic, high lead, and low tungsten and molybdenum, demonstrating good representativeness for process verification.
[0031] The heavy metal leaching concentration of the solidified body was determined according to the "Leaching Toxicity of Solid Waste - Sulfuric Acid and Nitric Acid Method" (HJ / T299-2007); the compressive strength was determined according to the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T 17671-2021).
[0032] It should be noted that the following embodiments are simplified descriptions, using a single experiment to verify the effects of each step; in actual continuous industrial production, the precipitate mother liquor obtained in each embodiment is returned to step S3 for leaching after alkali replenishment according to the method of the present invention, and the Na+ is monitored periodically. + and Concentration, when Na in the circulating leachate + Concentration exceeding 80g / L or When the cumulative concentration exceeds 15 g / L, 10%–20% of the circulating liquid is drawn off for cooling, crystallization, and salt removal. After salt removal, the clarified liquid is replenished with alkali and returned to the leaching process to maintain stable system operation. Meanwhile, to ensure full disclosure of process conditions, in each embodiment, the leaching residue is washed until the filtrate conductivity is less than 8 mS / cm before subsequent sorting (see descriptions of each step).
[0033] The 16 examples were set with parameters increasing in increments, such as sodium carbonate addition of 1.5%-6.0%, calcination temperature of 650-800℃, calcination time of 40-100 min, and leaching temperature of 60-90℃. Each example was performed according to steps S1 to S6.
[0034] Example 1
[0035] Take 1000g of tungsten slag (dry basis), age for 24h, crush to less than 10mm, add 1.5% Na2CO3, 1.00% CaO, and 0.50% Fe2O3, granulate, and calcine at 650℃ for 40min in air atmosphere. Grind the calcined sand to 55% of the particles being -0.074mm, leach at 60℃ for 45min with a liquid-to-solid ratio of 2.5:1, pH=10.2, and separate the solid and liquid to obtain filtrate and leaching residue. Add CaCl2 to the filtrate to precipitate, obtaining approximately 27g of tungsten-molybdenum enriched material (dry weight) (WO3 + MoO3 total approximately 35%). The leaching residue was washed with clean water until the conductivity of the filtrate was less than 8 mS / cm. The residue slurry was adjusted to a mass concentration of 25%, and first subjected to gravity separation in a spiral chute, then magnetic separation at 0.60T, and finally sulfide flotation (with the addition of 600 g / t sodium sulfide, 60 g / t butyl xanthate, and 30 g / t No. 2 oil, flotation pH=9.5), producing 18.5 g of tin-iron mixed concentrate, 15.2 g of copper-zinc-lead polymetallic concentrate, and 924.3 g of tailings. The tailings were then mixed with 0.5% FeSO4, 0.8% calcium dihydrogen phosphate, 8% slag powder, 6% cement, 2% lime, and 0.5% water glass (by dry weight) to a water-cement ratio of 0.45. The mixture was cured for 28 days at 20±2℃ and relative humidity ≥90% to obtain a stable solidified heavy metal body. The tungsten and molybdenum recovery rates were 70.4% and 63.8%, respectively. The compressive strength of the solidified body was 8.6 MPa, and the Pb / Cd / As leaching values were 0.18 / 0.018 / 0.28 mg / L.
[0036] Example 2
[0037] Take 1000g of tungsten slag (dry basis), crush it to less than 10mm, adjust the moisture content to 6%, add 1.8% Na2CO3, 1.27% CaO, and 0.67% Fe2O3, granulate, and calcine at 660℃ for 44min in air atmosphere. Grind the calcined sand to 57% -0.074mm, leach at 62℃ for 49min with a liquid-to-solid ratio of 2.7:1, pH=10.3, and precipitate with calcium salts to obtain approximately 28g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed with water until the conductivity was <8 mS / cm, then the slurry was adjusted to a mass concentration of 26%. It was first subjected to gravity separation in a spiral chute, then magnetic separation at 0.65T, and finally sulfide flotation (660 g / t sodium sulfide, 68 g / t butyl xanthate, 30 g / t No. 2 oil, pH=9.5), yielding 18.8 g of tin-iron mixed concentrate, 15.5 g of copper-zinc-lead polymetallic concentrate, and 923.7 g of tailings. The tailings (dry basis) were mixed with 0.63% FeSO4, 1.0% calcium dihydrogen phosphate, 9.4% slag powder, 6.8% cement, 2.4% lime, and 0.66% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 72.0% and 65.1%, respectively. The 28-day strength of the solidified body was 9.8 MPa, and the Pb / Cd / As leaching values were 0.16 / 0.016 / 0.25 mg / L.
[0038] Example 3
[0039] Take 1000g of tungsten slag (dry basis), crush, age, and adjust the moisture content to 8%. Add 2.1% Na2CO3, 1.53% CaO, and 0.83% Fe2O3, mix and granulate, then calcine at 670℃ for 48min in air atmosphere. Grind the calcined sand to a density of -0.074mm (59%), leach at a liquid-to-solid ratio of 2.9:1, pH=10.4, and 64℃ for 53min. Precipitate the leachate with calcium chloride to obtain approximately 28g of tungsten-molybdenum enriched material (dry weight). After washing the leaching residue with clean water until the conductivity met the standard, the slurry was adjusted to a mass concentration of 27%, and subjected to gravity separation on a shaking table, followed by magnetic separation at 0.70T, and finally sulfide flotation (720g / t sodium sulfide, 76g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5), yielding 19.2g of tin-iron mixed concentrate, 15.9g of copper-zinc-lead polymetallic concentrate, and 922.9g of tailings. The tailings were treated with 0.76% FeSO4, 1.2% phosphate, 10.8% slag powder, 7.6% cement, 2.8% lime, and 0.82% water glass, with a water-to-binder ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 74.1% and 66.5%, respectively, the compressive strength of the solidified body was 11.0MPa, and the leaching concentrations were 0.14 / 0.014 / 0.22mg / L.
[0040] Example 4
[0041] 1000g of tungsten slag (dry basis) was crushed to less than 10mm and aged. 2.4% Na₂CO₃, 1.80% CaO, and 1.00% Fe₂O₃ were added, and the mixture was granulated and calcined at 680℃ for 52min in air. The calcined slag was ground to a density of -0.074mm (61%), and leached at 66℃ for 57min with a liquid-to-solid ratio of 3.1:1 and pH=10.5. Calcium salts precipitated from the filtrate yielded approximately 29g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurryed to a concentration of 28%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 0.75T, and finally sulfide flotation (780g / t sodium sulfide, 84g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 19.6g of tin-iron mixed concentrate, 16.3g of copper-zinc-lead polymetallic concentrate, and 922.1g of tailings. The tailings were treated with 0.89% FeSO4, 1.4% dicalcium dihydrogen phosphate, 12.2% slag powder, 8.4% cement, 3.2% lime, and 0.98% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 76.0% and 68.0%, respectively. The compressive strength of the solidified body was 12.3 MPa, and the leaching concentrations were 0.12 / 0.012 / 0.20 mg / L.
[0042] Example 5
[0043] 1000g of tungsten slag (dry basis) was aged, crushed and sieved, and then mixed with 2.7% Na2CO3, 2.07% CaO, and 1.17% Fe2O3. The mixture was then calcined at 690℃ for 56 min in air. The calcined slag was ground to a density of -0.074mm (63%) and leached at 68℃ for 61 min with a liquid-to-solid ratio of 3.3:1, pH=10.6. The filtrate was precipitated with CaCl2 to obtain approximately 30g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed and the slurry was adjusted to a mass concentration of 29%. It was first subjected to gravity separation in a spiral chute, then magnetic separation at 0.80T, and finally sulfide flotation (840g / t sodium sulfide, 92g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5), yielding 20.0g of tin-iron mixed concentrate, 16.7g of copper-zinc-lead polymetallic concentrate, and 921.3g of tailings. The tailings were treated with 1.02% FeSO4, 1.6% phosphate, 13.6% slag powder, 9.2% cement, 3.6% lime, and 1.14% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 78.2% and 69.4%, respectively. The compressive strength of the solidified body was 13.5 MPa, and the leaching concentrations were 0.105 / 0.010 / 0.18 mg / L.
[0044] Example 6
[0045] Take 1000g of tungsten slag (dry basis), crush it to less than 10mm, add 3.0% Na2CO3, 2.33% CaO, and 1.33% Fe2O3, granulate, and calcine at 700℃ for 60min in air atmosphere. Grind the calcined sand to -0.074mm (65%), leach at 70℃ for 65min with a liquid-to-solid ratio of 3.5:1, pH=10.7, and the leachate. After calcium salt precipitation, approximately 31g of tungsten-molybdenum enriched material (dry weight) (WO3 + MoO3 total 36.8%) was obtained. After washing the leaching residue to a conductivity <8 mS / cm, the slurry was adjusted to a mass concentration of 30%, subjected to gravity separation on a shaking table, followed by magnetic separation at 0.85T, and finally sulfide flotation (900 g / t sodium sulfide, 100 g / t butyl xanthate, 30 g / t No. 2 oil, pH=9.5), yielding 20.5 g of tin-iron mixed concentrate, 17.2 g of copper-zinc-lead polymetallic concentrate, and 920.3 g of tailings. The tailings were treated with 1.15% FeSO4, 1.8% calcium dihydrogen phosphate, 15.0% slag powder, 10.0% cement, 4.0% lime, and 1.30% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 80.1% and 71.0%, respectively. The compressive strength of the solidified body was 14.8 MPa, and the leaching concentrations were 0.092 / 0.009 / 0.16 mg / L.
[0046] Example 7
[0047] 1000g of tungsten slag (dry basis) was homogenized and aged for 24h, then crushed and calcined at 710℃ for 64min with 3.3% Na2CO3, 2.60% CaO, and 1.50% Fe2O3 in air. The calcined slag was ground to a density of -0.074mm (67%) and leached at 72℃ for 69min with a liquid-to-solid ratio of 3.7:1 and pH=10.8. Calcium chloride precipitate was collected from the filtrate to obtain approximately 31g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry was adjusted to a mass concentration of 31%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 0.90T, and finally sulfide flotation (960g / t sodium sulfide, 108g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 20.9g of tin-iron mixed concentrate, 17.6g of copper-zinc-lead polymetallic concentrate, and 919.5g of tailings. The tailings were treated with 1.28% FeSO4, 2.0% phosphate, 16.4% slag powder, 10.8% cement, 4.4% lime, and 1.46% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 82.0% and 72.8%, respectively. The compressive strength of the solidified body was 16.1 MPa, and the leaching concentrations were 0.080 / 0.008 / 0.14 mg / L.
[0048] Example 8
[0049] 1000g of tungsten slag (dry basis) was crushed, sieved, and moistened to 9%. Na₂CO₃ 3.6%, CaO 2.87%, and Fe₂O₃ 1.67% were added, granulated, and calcined at 720℃ for 68 min in air. The calcined slag was ground to a density of -0.074mm (69%), leached at a liquid-to-solid ratio of 3.9:1, pH=10.9, and 74℃ for 73 min. Calcium salts precipitated from the filtrate yielded approximately 32g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 32%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 0.95T, and finally sulfide flotation (sodium sulfide 1020g / t, butyl xanthate 116g / t, No. 2 oil 30g / t, pH=9.5), producing 21.3g of tin-iron mixed concentrate, 18.0g of copper-zinc-lead polymetallic concentrate, and 918.7g of tailings. The tailings were treated with 1.41% FeSO4, 2.2% calcium dihydrogen phosphate, 17.8% slag powder, 11.6% cement, 4.8% lime, and 1.62% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 83.5% and 74.3%, respectively. The compressive strength of the solidified body was 17.4 MPa, and the leaching concentrations were 0.069 / 0.007 / 0.12 mg / L.
[0050] Example 9
[0051] 1000g of tungsten slag (dry basis) was aged and then crushed to less than 10mm. 3.9% Na₂CO₃, 3.13% CaO, and 1.83% Fe₂O₃ were added, mixed thoroughly, granulated, and calcined at 730℃ for 72min in air. The calcined slag was ground to a density of -0.074mm (71%) and leached at 76℃ for 77min with a liquid-to-solid ratio of 4.1:1, pH=11.0. CaCl₂ precipitate was obtained from the leaching solution, yielding approximately 32g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 33%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 1.00T, and finally sulfide flotation (1080g / t sodium sulfide, 124g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 21.7g of tin-iron mixed concentrate, 18.4g of copper-zinc-lead polymetallic concentrate, and 917.9g of tailings. The tailings were treated with FeSO4 1.54%, phosphate 2.4%, slag powder 19.2%, cement 12.4%, lime 5.2%, and water glass 1.78%, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 84.7% and 75.8%, respectively. The compressive strength of the solidified body was 18.7 MPa, and the leaching concentrations were 0.058 / 0.006 / 0.105 mg / L.
[0052] Example 10
[0053] 1000g of tungsten slag (dry basis) was crushed, homogenized, and moistened. 4.2% Na₂CO₃, 3.40% CaO, and 2.00% Fe₂O₃ were added, and the mixture was granulated and calcined at 740℃ for 76 min in air. The calcined slag was ground to a density of -0.074mm (73%) and leached at 78℃ for 81 min with a liquid-to-solid ratio of 4.3:1 and pH=11.1. The filtrate yielded approximately 33g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 34%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 1.05T, and finally sulfide flotation (1140g / t sodium sulfide, 132g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 22.1g of tin-iron mixed concentrate, 18.8g of copper-zinc-lead polymetallic concentrate, and 917.1g of tailings. The tailings were treated with 1.67% FeSO4, 2.6% calcium dihydrogen phosphate, 20.6% slag powder, 13.2% cement, 5.6% lime, and 1.94% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 86.0% and 77.4%, respectively. The compressive strength of the solidified body was 20.0 MPa, and the leaching concentrations were 0.050 / 0.0055 / 0.092 mg / L.
[0054] Example 11
[0055] 1000g of tungsten slag (dry basis) was aged for 24 hours and then crushed to less than 10mm. 4.5% Na₂CO₃, 3.67% CaO, and 2.17% Fe₂O₃ were added, and the slag was calcined at 750℃ for 80 minutes in air. The calcined slag was ground to a density of -0.074mm (75%) and leached at 80℃ for 85 minutes with a liquid-to-solid ratio of 4.5:1, pH=11.2. Calcium salts were added to the tungsten-molybdenum-containing solution to precipitate approximately 33g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 35%, and subjected to gravity separation on a shaking table, followed by magnetic separation at 1.10T, and finally sulfide flotation (1200g / t sodium sulfide, 140g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 22.6g of tin-iron mixed concentrate, 19.3g of copper-zinc-lead polymetallic concentrate, and 916.1g of tailings. The tailings were treated with 1.80% FeSO4, 2.8% phosphate, 22.0% slag powder, 14.0% cement, 6.0% lime, and 2.10% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 87.1% and 79.0%, respectively. The compressive strength of the solidified body was 21.3 MPa, and the leaching concentrations were 0.043 / 0.0050 / 0.080 mg / L.
[0056] Example 12
[0057] 1000g of tungsten slag (dry basis) was crushed and sieved. 4.8% Na₂CO₃, 3.93% CaO, and 2.33% Fe₂O₃ were added, mixed, granulated, and calcined at 760℃ for 84 min in air. The calcined slag was ground to a density of -0.074mm (77%), leached at 82℃ for 89 min with a liquid-to-solid ratio of 4.7:1 and pH=11.3. Calcium salts precipitated from the filtrate yielded approximately 34g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed and slurry adjusted to a mass concentration of 36%. It was then subjected to gravity separation via a spiral chute, followed by magnetic separation at 1.15T, and finally sulfide flotation (1260g / t sodium sulfide, 148g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5), yielding 23.0g of tin-iron mixed concentrate, 19.7g of copper-zinc-lead polymetallic concentrate, and 915.3g of tailings. The tailings were treated with 1.93% FeSO4, 3.0% calcium dihydrogen phosphate, 23.4% slag powder, 14.8% cement, 6.4% lime, and 2.26% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 88.0% and 80.5%, respectively. The compressive strength of the solidified body was 22.5 MPa, and the leaching concentrations were 0.036 / 0.0045 / 0.069 mg / L.
[0058] Example 13
[0059] 1000g of tungsten slag (dry basis) was aged, crushed, and homogenized. Na₂CO₃ (5.1%), CaO (4.20%), and Fe₂O₃ (2.50%) were added, and the mixture was granulated and calcined at 770℃ for 88 min in air. The calcined slag was ground to a density of -0.074mm (79%) and leached at 84℃ for 93 min with a liquid-to-solid ratio of 4.9:1, pH 11.4. CaCl₂ precipitate from the leachate yielded approximately 34g of tungsten-molybdenum enrichment (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 37%, and subjected to gravity separation via a spiral chute, followed by magnetic separation at 1.20T, and finally sulfide flotation (sodium sulfide 1320g / t, butyl xanthate 156g / t, No. 2 oil 30g / t, pH 9.5). This yielded 23.4g of tin-iron mixed concentrate, 20.1g of copper-zinc-lead polymetallic concentrate, and 914.5g of tailings. The tailings were treated with FeSO4 2.06%, phosphate 3.2%, slag powder 24.8%, cement 15.6%, lime 6.8%, and water glass 2.42%, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 89.2% and 82.0%, respectively. The compressive strength of the solidified body was 23.7 MPa, and the leaching concentrations were 0.030 / 0.0040 / 0.058 mg / L.
[0060] Example 14
[0061] Take 1000g of tungsten slag (dry basis), crush it to less than 10mm, add 5.4% Na2CO3, 4.47% CaO, and 2.67% Fe2O3, mix well, and calcine at 780℃ for 92min in air atmosphere. Grind the calcined sand to -0.074mm (81%), leach at 86℃ for 97min with a liquid-to-solid ratio of 5.1:1, pH=11.5, and add calcium salt to the filtrate to obtain approximately 35g of tungsten-molybdenum enrichment (dry weight). After washing the leaching residue, adjust the slurry to a mass concentration of 38%, perform gravity separation in a spiral chute, then magnetic separation at 1.25T, and finally sulfide flotation (sodium sulfide 1380g / t, butyl xanthate 164g / t, No. 2 oil 30g / t, pH=9.5), producing 23.8g of tin-iron mixed concentrate, 20.5g of copper-zinc-lead polymetallic concentrate, and 913.7g of tailings. The tailings were treated with 2.19% FeSO4, 3.4% dicalcium dihydrogen phosphate, 26.2% slag powder, 16.4% cement, 7.2% lime, and 2.58% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 90.0% and 83.5%, respectively. The compressive strength of the solidified body was 25.0 MPa, and the leaching concentrations were 0.025 / 0.0035 / 0.049 mg / L.
[0062] Example 15
[0063] 1000g of tungsten slag (dry basis) was aged and sieved, then 5.7% Na2CO3, 4.73% CaO, and 2.83% Fe2O3 were added. The slag was granulated and calcined at 790℃ for 96 min in air. The calcined slag was ground to a density of -0.074mm (83%) and leached at 88℃ for 101 min with a liquid-to-solid ratio of 5.3:1, pH=11.6. Calcium salts precipitated from the tungsten-molybdenum leaching solution yielded approximately 35g of tungsten-molybdenum enriched concentrate (dry weight). The leaching residue was washed, slurry adjusted to a mass concentration of 39%, and subjected to gravity separation in a spiral chute, followed by magnetic separation at 1.30T, and finally sulfide flotation (1440g / t sodium sulfide, 172g / t butyl xanthate, 30g / t No. 2 oil, pH=9.5). This yielded 24.2g of tin-iron mixed concentrate, 20.9g of copper-zinc-lead polymetallic concentrate, and 912.9g of tailings. The tailings were treated with FeSO4 2.32%, phosphate 3.6%, slag powder 27.6%, cement 17.2%, lime 7.6%, and water glass 2.74%, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 90.8% and 85.0%, respectively. The compressive strength of the solidified body was 26.4 MPa, and the leaching concentrations were 0.020 / 0.0030 / 0.040 mg / L.
[0064] Example 16
[0065] Take 1000g of tungsten slag (dry basis), crush it to less than 10mm and adjust the moisture content. Add 6.0% Na2CO3, 5.00% CaO, and 3.00% Fe2O3, granulate, and calcine at 800℃ for 100min in air atmosphere. Grind the calcined sand to 85% of the particles being -0.074mm, leach at 90℃ for 105min with a liquid-to-solid ratio of 5.5:1 and pH=11.7. Add CaCl2 to the filtrate, react at 80℃, and filter to obtain approximately 35g of tungsten-molybdenum enrichment (dry weight). After washing the leaching residue to a conductivity of <8 mS / cm, the slurry was adjusted to a mass concentration of 40%, followed by gravity separation in a spiral chute, magnetic separation at 1.35T, and finally sulfide flotation (sodium sulfide 1500 g / t, butyl xanthate 180 g / t, No. 2 oil 30 g / t, pH=9.5), yielding 24.7 g of tin-iron mixed concentrate, 21.3 g of copper-zinc-lead polymetallic concentrate, and 912.0 g of tailings. The tailings were treated with 2.45% FeSO4, 3.8% calcium dihydrogen phosphate, 29.0% slag powder, 18.0% cement, 8.0% lime, and 2.90% water glass, with a water-cement ratio of 0.45, and cured under the same conditions for 28 days. The tungsten and molybdenum recoveries were 91.4% and 86.2%, respectively. The compressive strength of the solidified body was 27.8 MPa, and the leaching concentrations were 0.015 / 0.0025 / 0.032 mg / L.
[0066] The solidified tailings from Example 16 were subjected to XRD phase analysis. The XRD pattern clearly showed the following characteristic diffraction peaks: 2θ = 29.4°, 32.1°, and 49.8° were characteristic of CSH gel dispersion diffraction; 2θ = 9.1°, 15.8°, and 23.0° were characteristic peaks of ettringite (AFt); and 2θ = 26.6°, 30.1°, and 44.3° were characteristic peaks of lead apatite (Pb). 10 The characteristic peaks of (PO4)6(OH)2; the characteristic peaks of iron arsenate (FeAsO4) at 2θ=31.7° and 45.5°. The coexistence of the above phases confirms the synergistic effect of the triple stabilization mechanism of chemical precipitation, lattice doping and gel encapsulation in the solidified body of the present invention.
[0067] To assess the impact of salt accumulation during cyclic leaching, a cyclic leaching experiment was conducted using the mother liquor from Example 16, focusing on the Na+ content. + and The cumulative effect of concentration changes on the leaching rate of tungsten and molybdenum recovery indicators. Experimental results show that when the Na concentration in the circulating solution increases... + As the concentration gradually increased from an initial 12.5 g / L to 78 g / L, the tungsten leaching rate slowly decreased from 91.4% to 88.2%; when Na... + When the concentration exceeded 82 g / L, the tungsten leaching rate dropped sharply to 79.6%, while the viscosity of the leachate increased significantly, and the filtration rate decreased by approximately 40%. When the cumulative concentration exceeds 18 g / L, the calcium-molybdenum precipitation reaction is significantly interfered with, and the molybdenum precipitation rate decreases from 86.2% to 74.5%. Therefore, this invention sets that when Na... + >80g / L or When the concentration is >15g / L, 15% of the circulating liquid is drawn off for cooling, crystallization, and salt removal. After salt removal, the Na content in the clear liquid is [missing information]. + Reduced to 52g / L The concentration dropped to 8.6 g / L, and after alkali replenishment, the leaching rate of tungsten and molybdenum could be restored to over 91.0%, proving the effectiveness of the salt removal and purification measures.
[0068] Analysis of the concentrate products obtained in Example 16: The tin-iron mixed concentrate (yield 24.7 g) contained 18.6% Sn and 42.3% Fe, with Sn recovery rates of 72.4% and Fe recovery rates of 15.2% relative to the original slag. It can be sold as a tin-iron rich material or used as an auxiliary material in ironmaking. The copper-zinc-lead polymetallic concentrate (yield 21.3 g) contained 6.8% Cu, 11.2% Zn, and 9.5% Pb, with a total grade of 27.5%, making it suitable for sale for comprehensive recovery.
[0069] To verify the necessity and superiority of the synergistic calcination of sodium carbonate, calcium, and iron in step S2 of this invention, comparative examples 1 to 3 were set up as follows. Each comparative example was based on Example 5 (Na2CO3 2.7%, CaO 2.07%, Fe2O3 1.17%, calcined at 690°C for 56 min in air atmosphere, with the remaining conditions of S3 to S6 being exactly the same, and the leaching residues were all subjected to the same washing treatment).
[0070] Comparative Example 1 (without sodium carbonate) Except for the absence of sodium carbonate, the conditions were exactly the same as in Example 5. Results: The tungsten recovery rate was only 18.6%, and the molybdenum recovery rate was only 12.3%, indicating that sodium carbonate is the core driving force for the activation and transformation of tungsten and molybdenum phases, and tungsten and molybdenum can hardly be effectively leached without the addition of sodium carbonate.
[0071] Comparative Example 2 (without calcium and iron components) Except for the absence of CaO and Fe2O3, the conditions were identical to those in Example 5. Results: Tungsten recovery was 76.8%, and molybdenum recovery was 67.5% (slightly lower than in Example 5). However, the As concentration in the leachate was as high as 8.6 mg / L, and the Pb concentration was 3.2 mg / L. The 28-day compressive strength of the solidified tailings was only 9.8 MPa, with Pb / Cd / As leaching concentrations of 0.42 / 0.035 / 0.56 mg / L, respectively. This indicates that while the absence of calcium and iron components has a limited impact on tungsten and molybdenum leaching, it leads to the large-scale dissolution of arsenic and lead during leaching, severely deteriorating the heavy metal stability and mechanical properties of the subsequent solidified body. This fully demonstrates the crucial role of calcium and iron components in the in-situ confinement of heavy metals.
[0072] Comparative Example 3 (no roasting, raw residue directly alkali leaching) Tungsten slag was directly subjected to S3 alkaline leaching and subsequent S4-S6 steps without S2 roasting treatment. Results: Tungsten recovery rate was only 35.2%, and molybdenum recovery rate was only 28.6%. This indicates that without roasting and activation, tungsten and molybdenum are encapsulated by the glassy phase and iron-manganese oxides, making it difficult to fully react with the leaching agent. Roasting and activation are necessary prerequisites for ensuring efficient recovery of tungsten and molybdenum.
[0073] To verify the superiority of the final residue after pretreatment in S1 to S5 in the S6 curing step of the present invention in terms of cementitious material usage compared with the original residue after direct curing, comparative examples 4 to 6 were set up. Comparative examples 4 to 6 are all based on Example 6.
[0074] Comparative Example 4 (Direct solidification of raw slag) 1000g of untreated raw tungsten slag (dry basis) was directly mixed, molded, and cured using the same curing formula as in Example 6. Results: The 28-day compressive strength of the cured body was only 4.2 MPa, with Pb / Cd / As leaching concentrations of 0.85 / 0.072 / 1.25 mg / L, respectively. Although the leaching concentrations did not exceed the limits specified in GB 5085.3-2007, the strength of the cured body was far below the minimum requirements for cementitious materials in applications such as mine backfilling and road base courses (typically ≥8 MPa). Compared to Example 6, the strength decreased by 71.6% with the same amount of cementitious material, indicating that without the activation pretreatment of this invention, even if the leaching meets the standards, it is impossible to obtain a cured body with engineering value from the raw slag.
[0075] Comparative Example 5 (High-content solidification of raw slag) 1000g of raw tungsten slag (dry basis) was taken, and the total content of cementitious material (slag powder + cement + lime) was increased from 29% (15% + 10% + 4%) in Example 6 to 45% (slag powder 25%, cement 15%, lime 5%), while the amount of iron salt and phosphate added remained unchanged. Results: The 28-day compressive strength of the solidified body reached 6.8 MPa, and the Pb / Cd / As leaching values were 0.32 / 0.031 / 0.48 mg / L, respectively. Although these met the limits of GB5085.3-2007, the strength was still below 8 MPa, and the total amount of cementitious material increased by 55%, resulting in a significant increase in cost. This demonstrates that directly solidifying the raw slag requires a substantial increase in the amount of cementitious material, yet it is still difficult to achieve optimal performance. This fully proves that the present invention effectively stimulates the cementitious activity of the tailings slag through pre-roasting-leaching-sorting treatment, significantly reducing the consumption of cementitious material.
[0076] Comparative Example 6 (Final tailings without iron salts / phosphate solidification) Take 920.3g of the final residue obtained in Example 6, and add 15% slag powder, 10% cement, 4% lime, and 1.3% water glass to the solidification batch without adding ferrous sulfate and calcium dihydrogen phosphate, with a water-cement ratio of 0.45, and cure under the same conditions for 28 days. Results: The 28-day compressive strength of the solidified body was 13.5 MPa. While the strength decreased slightly due to the reduced dilution effect of iron salts / phosphates, the leaching concentrations of Pb, Cd, and As reached 0.58, 0.051, and 0.82 mg / L, respectively. Although these leaching concentrations met the limits of GB 5085.3-2007, compared to Example 6 (0.092, 0.009, and 0.16 mg / L), the leaching concentrations of lead, cadmium, and arsenic increased by 5.3 times, 4.7 times, and 4.1 times, respectively. This indicates that without iron salts / phosphates, heavy metals rely solely on the physical encapsulation of hydration products, lacking chemical precipitation and lattice solidification. Under long-term environmental conditions such as acidic rainfall and carbonization, there is a high risk of secondary leaching exceeding the limits. Therefore, the synergistic chemical fixation of iron salts and phosphates is indispensable for ensuring the long-term confinement of heavy metals and the environmental safety of the solidified body.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A synergistic treatment method for tungsten residue valuable metal enrichment and heavy metal stable solidification, characterized in that, Includes the following steps: S1. Pretreatment of tungsten slag: The tungsten slag is aged, crushed to a particle size of <10mm, and the dry basis moisture content is adjusted to 6% to 12% to obtain pretreated tungsten slag. S2. Mineral phase activation roasting: Sodium carbonate, calcium components and iron components are added to the pretreated tungsten slag, mixed and granulated, and then roasted at 650-800℃ for 40-100 min in air atmosphere to prepare activated roasted sand. S3. Selective alkaline leaching: Activated roasted sand is ground to a particle size of -0.074mm, accounting for 55% to 85%, and then water or circulating leachate is added for alkaline leaching. Solid-liquid separation is performed to obtain tungsten-molybdenum-containing leachate and leaching residue. S4. Tungsten and molybdenum precipitation enrichment: Calcium salt and / or magnesium salt are added to the tungsten and molybdenum-containing leachate to precipitate and recover tungsten and molybdenum. The mother liquor of the precipitate is purified by adding alkali and periodically removing salt and then returned to step S3 as a circulating leachate. S5. Tin-copper-lead-zinc stepwise separation: The leaching residue is slurryed to a mass concentration of 25% to 40%, and then subjected to gravity separation, magnetic separation and sulfide flotation in sequence to produce tin-iron mixed concentrate, copper-zinc-lead polymetallic concentrate and tailings, respectively. S6. Co-solidification of terminal tailings: Iron salts, phosphates, slag powder, cement, lime and water glass are compounded into the terminal tailings, mixed with water, molded and cured to obtain a heavy metal stable solidified body.
2. The method according to claim 1, characterized in that, In step S2, based on the dry basis of the pretreated tungsten slag, the tungsten slag is the residue generated during tungsten smelting, tungsten ore alkaline decomposition, tungstate production, or secondary tungsten resource treatment. The tungsten slag contains WO3 content of 0.20% to 3.50%, Mo content of 0.02% to 0.80%, Sn content of 0.10% to 2.00%, Cu content of 0.03% to 1.00%, Zn content of 0.05% to 1.50%, and contains one or more heavy metals selected from Pb, Cd, As, Cr, and Ni.
3. The method according to claim 1 or 2, characterized in that, Based on the dry weight of tungsten slag, the amount of sodium carbonate added is 1.5% to 6.0%, the amount of calcium component (calculated as CaO) added is 1.0% to 5.0%, and the amount of iron component (calculated as Fe2O3) added is 0.5% to 3.0%.
4. The method according to claim 3, characterized in that, The calcium component is one or more of calcium oxide, calcium hydroxide, limestone powder, and carbide slag; the iron component is one or more of iron oxide, ferrous sulfate, red mud, and iron tailings powder; the amount of calcium and iron components added is calculated as CaO and Fe2O3.
5. The method according to claim 1, characterized in that, In step S3, the liquid-to-solid ratio of the alkaline leaching is 2.5:1 to 5.5:1, the pH is adjusted by sodium hydroxide, sodium carbonate or a mixture of the two, the leaching pH is 10.2 to 12.0, the leaching temperature is 60 to 90°C, and the leaching time is 45 to 105 min.
6. The method according to claim 1, characterized in that, In step S4, the reaction temperature for precipitation is 50–85°C, the pH is 8.5–10.5, and the reaction time is 20–60 min; the total molar ratio of calcium and magnesium to tungsten and molybdenum is 1.05–1.40:1; the calcium salt is selected from calcium chloride, calcium nitrate, or lime milk, and the magnesium salt is selected from magnesium chloride or magnesium oxide slurry; the tungsten precipitation rate is ≥95%, and the molybdenum precipitation rate is ≥88%.
7. The method according to claim 1, characterized in that, In step S5, the gravity separation equipment is selected from spiral sluices, shaking tables, or centrifugal concentrators, and the magnetic induction intensity of the magnetic separation is 0.6 to 1.4 T; the sulfide flotation specifically involves adding 600 to 1500 g / t of sodium sulfide, 60 to 180 g / t of butyl xanthate, and 10 to 45 g / t of No. 2 oil, and controlling the flotation pH to 9.0 to 10.
0.
8. The method according to claim 1, characterized in that, In step S6, based on the dry weight of the final tailings: 0.5%–2.5% iron salt, 0.8%–4.0% phosphate, 8%–30% slag powder, 6%–18% cement, 2%–8% lime, and 0.5%–3.0% water glass; water-cement ratio 0.35–0.65; curing conditions: temperature 15–35℃, relative humidity ≥85%, curing cycle 7–28 days; the iron salt is selected from ferrous sulfate, ferric sulfate, or ferric chloride; the phosphate is selected from calcium dihydrogen phosphate, sodium dihydrogen phosphate, or diammonium hydrogen phosphate.
9. The method according to claim 1, characterized in that, The periodic salt removal and purification mentioned in step S4 refers to: when the Na in the circulating leachate... + Concentration exceeding 80g / L or When the cumulative concentration exceeds 15 g / L, 10% to 20% of the circulating liquid is drawn out for cooling, crystallization, and salt removal. After salt removal, the clear liquid is replenished with alkali and then returned to the leaching process.
10. The method according to claim 1, characterized in that, The prepared heavy metal stabilized solidified body internally generates a complex mineral phase consisting of hydrated calcium silicate (CSH), ettringite (AFt), ferric phosphate, lead apatite, and carbonate. Through multiple mechanisms such as lattice solidification, chemical precipitation, and gel encapsulation, the heavy metals are effectively imprisoned and stabilized. The 28-day compressive strength is ≥8MPa, and the heavy metal leaching concentration of the solidified body meets the limit requirements of GB 5085.3-2007 standard.